Thallium solidifying agent, preparation method, application and resourceful treatment method of lithium slag

By using solid thallium agent and cement granulation technology in the lithium mica lithium extraction process, the problem of removing thallium elements in lithium slag is solved, the operating costs of lithium smelters are reduced and the environment is protected.

CN119016477APending Publication Date: 2024-11-26YICHUN JIANGLI LITHIUM BATTERY NEW ENERGY IND RES INST
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411129284.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The lithium slag produced in the lithium mica extraction process contains highly toxic thallium elements, which leads to environmental and human health threats. The problems of its treatment and resource utilization have not been effectively solved, resulting in lithium smelters facing high rental costs and environmental risks.

Method used

Using a preparation method of thallium solidifying agent, by reacting sodium hydroxide and sulfur in hot water, a red-brown product liquid is generated to cure thallium in lithium slag, and mixed with cement to granulate cement aggregate spheres. , used in concrete to realize the resource treatment of lithium slag.

Benefits of technology

Effectively reduce the thallium content in the lithium slag leaching liquid, making it less than 5ppb, avoiding the risk of thallium leakage, and realizing the resource utilization of lithium slag. The cement aggregate balls produced can be used as gravels in concrete, avoiding thallium Damage to the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016477A_ABST
    Figure CN119016477A_ABST
Patent Text Reader

Abstract

The invention relates to a thallium solidifying agent, a preparation method, application and a resourceful treatment method of lithium slag. The preparation method of the thallium solidifying agent comprises the following steps: adding sodium hydroxide into hot water to obtain a sodium hydroxide solution; adding sulfur into hot water to obtain sulfur slurry; adding the sulfur slurry into a sodium hydroxide solution, and then adding hot water to obtain mixed slurry; and reacting the mixed slurry under a second temperature condition to obtain the reserved thallium solidifying agent. The invention also provides the thallium solidifying agent prepared by the preparation method. The invention further provides application of the thallium solidifying agent in lithium slag. The invention also provides a resourceful treatment method of the lithium slag, which comprises the following steps: mixing the stored thallium-fixing agent with water to obtain a thallium-fixing agent; carrying out dry mixing on the lithium slag, cement and a quick-drying agent to obtain a mixture; and the mixture and the thallium solidifying agent are mixed and granulated, cement aggregate balls are obtained, and resourceful treatment of the lithium slag is achieved. According to the method, the problem that the thallium content in the existing lithium slag leachate exceeds the standard is solved, and resource reutilization of the lithium slag is also realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resource utilization of lithium slag, and in particular to a thallium-fixing agent, a preparation method, an application and a resource processing method of lithium slag. Background Art

[0002] With the rapid advancement of new energy vehicle technology, the global demand for lithium-ion batteries has increased dramatically, directly driving up the price of lithium resources. In this context, extracting lithium from low-grade lepidolite has become a technical direction with great economic potential. Yichun City, Jiangxi Province, as an important production area of ​​lepidolite resources in China, has rich lepidolite deposits that provide a solid foundation for the development of lithium extraction technology.

[0003] In the lithium extraction process of lepidolite, sulfate roasting method is widely used due to its high efficiency and applicability. This method mixes lepidolite with sulfate (such as potassium sulfate, sodium sulfate, etc.), roasts it at high temperature, and uses the principle of high-temperature ion replacement to replace the lithium in the lepidolite to form soluble lithium sulfate, and then extracts the lithium element through wet leaching and other processes. This method occupies a dominant position in the lepidolite lithium extraction industry, significantly improves the efficiency of lithium extraction, and promotes the production of battery-grade lithium carbonate and other products.

[0004] However, while the sulfate roasting lithium extraction process brings economic benefits, it also produces a large amount of lithium slag. As a by-product of this process, the treatment and disposal of lithium slag has become an urgent problem to be solved. In particular, the highly toxic thallium element contained in lithium slag poses a serious threat to the environment and human health. According to the detection of the toxic leaching method, the thallium content in the lithium slag leachate generally exceeds the prescribed standard of less than 5ppb, reaching more than 20ppb, which makes it impossible for the lithium slag to be directly discharged into the environment or recycled.

[0005] At present, lithium smelters generally use the method of temporarily storing lithium slag in special warehouses to store these hazardous wastes. However, with the continuous expansion of the lithium extraction industry from lepidolite, the amount of lithium slag produced is also increasing year by year, resulting in rising warehouse rental costs, which has brought great pressure to the operation of lithium smelters. In addition, long-term storage of lithium slag also poses environmental risks. Once a leak or accident occurs, it will cause immeasurable damage to the surrounding environment.

[0006] Therefore, developing an efficient and environmentally friendly lithium slag treatment technology to achieve the effective removal of thallium from lithium slag and the resource utilization of lithium slag is of great significance for promoting the sustainable development of the lithium extraction industry from lithium mica, reducing corporate operating costs, and protecting the ecological environment. Summary of the invention

[0007] In view of this, the purpose of the present invention is to provide a thallium-fixing agent, a preparation method, an application and a resource treatment method for lithium slag, so as to solve the problem of excessive thallium content in the existing lithium slag leaching solution, and to achieve resource recycling of lithium slag, in order to solve the current problem of lithium slag treatment.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a thallium-fixing agent comprises the following steps:

[0010] S1. Add sodium hydroxide to hot water at a first temperature and stir for 10 to 30 minutes to obtain a sodium hydroxide solution; add sulfur to hot water at a first temperature and stir for 10 to 30 minutes to obtain a sulfur slurry;

[0011] S2, adding the sulfur slurry into the sodium hydroxide solution, and then adding hot water at the first temperature to obtain a mixed slurry, and stirring for 10 minutes to 30 minutes; reacting the mixed slurry under the second temperature condition to obtain a reserve thallium solid agent;

[0012] The second temperature is greater than the first temperature.

[0013] According to the above technical means, by further heating the heated sodium hydroxide solution and sulfur slurry to react, the obtained reddish brown product liquid can solidify the thallium in the lithium slag, so that the thallium content in the leaching solution of the lithium slag after solidification is less than 5ppb, which is within the prescribed standard of less than 5ppb, thereby avoiding the risk of thallium leakage from the long-term stored lithium slag and causing damage to the surrounding environment. The problem of excessive thallium content in the existing lithium slag leaching solution is effectively solved.

[0014] Preferably, the first temperature is greater than or equal to 80°C.

[0015] Preferably, the second temperature is greater than or equal to 95°C.

[0016] By using hot water to beat the slurry, the beating speed is effectively guaranteed; further increasing the temperature to react effectively ensures the progress of the chemical reaction, so as to successfully prepare the thallium solid agent.

[0017] Preferably, the mixed slurry reacts at the second temperature for 1 h to 1.5 h.

[0018] Preferably, in the sodium hydroxide solution, the mass ratio of sodium hydroxide to hot water is 1:2 to 2.2.

[0019] Preferably, in the sulfur slurry, the mass ratio of sulfur to hot water is 1:2 to 2.2.

[0020] Preferably, in the mixed slurry, the mass ratio of sodium hydroxide, sulfur and hot water is 1:2-2.2:10-12.

[0021] Preferably, S1 specifically includes: adding sodium hydroxide into hot water at a first temperature, stirring and melting, and maintaining the heating state to obtain a sodium hydroxide solution.

[0022] Preferably, S2 specifically includes: adding sulfur slurry into sodium hydroxide solution, and then adding hot water at a first temperature to obtain a mixed slurry; reacting the mixed slurry under a second temperature condition, and when the mixed slurry appears reddish brown, stopping heating and filtering to obtain a reddish brown liquid reserve thallium solid agent.

[0023] The present invention also provides a thallium-fixing agent prepared by the preparation method of the present invention.

[0024] The present invention also provides application of the thallium-fixing agent prepared by the preparation method of the present invention in lithium slag.

[0025] The present invention also provides a method for recycling lithium slag, comprising the following steps:

[0026] The reserve thallium-fixing agent prepared by the preparation method of the present invention is mixed with water to obtain the thallium-fixing agent;

[0027] dry-mixing lithium slag, cement and a quick-drying agent to obtain a mixture;

[0028] The mixture is mixed with a thallium-fixing agent and granulated to obtain cement aggregate balls;

[0029] The cement aggregate balls are used in concrete to realize resource processing of lithium slag.

[0030] According to the above technical means, by using the thallium-fixing agent of the present invention to infiltrate and granulate lithium slag, the thallium content in the leaching liquid of the prepared cement aggregate balls can be lower than 5ppb, thereby effectively achieving the fixation of thallium in the lithium slag, and the prepared cement aggregate balls can be used as gravel in concrete, effectively realizing the resource utilization of lithium slag, solving the current problem of lithium slag treatment, and the thallium contained in the prepared concrete will not leak into the environment, effectively avoiding the damage of thallium to the environment.

[0031] The thallium-fixing agent and cement are used to block the internal channels of the particles, so that the thallium-containing substances are solidified inside the particles.

[0032] Preferably, the cement aggregate balls are mixed with water at a ratio of 1:10 in terms of g:mL, and then allowed to stand after being shaken to obtain a toxic leachate; the thallium content in the toxic leachate is less than 5 ppb.

[0033] Preferably, the cement aggregate balls are mixed with water at a ratio of 1:10 in terms of g:mL, horizontally shaken for 8 hours at room temperature, and allowed to stand for 16 hours to obtain a toxic leachate; the thallium content in the toxic leachate is less than 5 ppb.

[0034] Preferably, the water content of the lithium slag is less than or equal to 10%.

[0035] Preferably, the cement is 325 cement or 425 cement.

[0036] Preferably, the lithium slag is lithium slag obtained by extracting lithium from lepidolite by sulfate roasting.

[0037] Preferably, the quick-drying agent is selected from a mixture of calcium aluminate, sodium aluminate and sodium carbonate.

[0038] Preferably, the quick-drying agent is a mixture of 20% by mass of calcium aluminate, 75% by mass of sodium aluminate and 5% by mass of sodium carbonate.

[0039] Preferably, the particle size of the cement aggregate balls is 4 mm to 24 mm.

[0040] Preferably, the cement aggregate balls are used as gravel in concrete.

[0041] Preferably, the mass ratio of the thallium-fixing agent to water is 1:20-22.

[0042] Preferably, the mass ratio of the lithium slag (based on a moisture content of 0), cement, quick-drying agent and total water (the total water includes the added water, the water contained in the lithium slag and the water contained in the thallium-fixing agent) is 100:20-22:2-2.2:35-40.

[0043] Beneficial effects of the present invention:

[0044] The preparation method of the thallium-fixing agent of the invention further heats the heated sodium hydroxide solution and sulfur slurry to react, and the obtained reddish-brown product liquid can solidify the thallium in the lithium slag, so that the thallium content in the leaching solution of the lithium slag after the thallium is fixed is lower than 5 ppb, which is within the prescribed standard of less than 5 ppb, thereby avoiding the risk of thallium leakage from the lithium slag stored for a long time and causing damage to the surrounding environment. The preparation method has the advantages of simple preparation method, easy to obtain raw materials, mild process conditions and environmental friendliness, and is particularly suitable for industrial production and application.

[0045] The resource treatment method of lithium slag of the present invention uses the thallium fixing agent of the present invention to infiltrate and granulate the lithium slag, so that the thallium content in the leaching solution of the prepared cement aggregate balls leached again can be lower than 5ppb, thereby effectively realizing the fixation of thallium in the lithium slag, and the prepared cement aggregate balls can be used as stones in concrete, effectively realizing the resource utilization of lithium slag, solving the current treatment problem of lithium slag, and the thallium contained in the prepared concrete will not leak into the environment, effectively avoiding the damage of thallium to the environment, and having promotion and application value in the technical field of lithium slag resource utilization. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The invention is used to prepare cement aggregate balls with a diameter of 4mm to 24mm. DETAILED DESCRIPTION

[0047] The following will describe the embodiments of the present invention with reference to the preferred embodiments, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.

[0048] The present invention aims to disclose a thallium-fixing agent, a preparation method, an application and a resource treatment method for lithium slag, so as to solve the problem of excessive thallium content in the existing lithium slag leaching solution, and realize the resource recycling of lithium slag, so as to solve the current problem of lithium slag treatment.

[0049] The preparation method of the thallium-fixing agent comprises the following steps:

[0050] S1. Adding sodium hydroxide to hot water at a first temperature and stirring for 10 to 30 minutes to obtain a sodium hydroxide solution; adding sulfur to the hot water at the first temperature to obtain a sulfur slurry;

[0051] S2, adding the sulfur slurry into the sodium hydroxide solution, and then adding hot water at the first temperature, stirring for 10 minutes to 30 minutes to obtain a mixed slurry; reacting the mixed slurry under the second temperature condition to obtain a reserve thallium solid agent;

[0052] The second temperature is greater than and lower than the first temperature.

[0053] By further heating the heated sodium hydroxide solution and sulfur slurry to react, the obtained product can solidify the thallium in the lithium slag, so that the thallium content in the leaching solution of the lithium slag after solidification is less than 5ppb, which is within the prescribed standard of less than 5ppb, thereby avoiding the risk of thallium leakage from long-term stored lithium slag and causing damage to the surrounding environment. The problem of excessive thallium content in the existing lithium slag leaching solution is solved.

[0054] In some embodiments, the first temperature is greater than or equal to 80°C.

[0055] In some embodiments, the second temperature is greater than or equal to 95°C.

[0056] In some embodiments, the mixed slurry is reacted at the second temperature for 1 hour to 1.5 hours.

[0057] Exemplarily, the mixed slurry is reacted under the second temperature condition for 1 hour.

[0058] In some embodiments, in the sodium hydroxide solution, the mass ratio of sodium hydroxide to hot water is 1:2 to 2.2.

[0059] Exemplarily, in the sodium hydroxide solution, the mass ratio of sodium hydroxide to hot water is 1:2.

[0060] In some embodiments, in the sulfur slurry, the mass ratio of sulfur to hot water is 1:2 to 2.2.

[0061] Exemplarily, in the sulfur slurry, the mass ratio of sulfur to hot water is 1:2.

[0062] In some embodiments, in the mixed slurry, the mass ratio of sodium hydroxide, sulfur and hot water is 1:2-2.2:10-12.

[0063] Exemplarily, in the mixed slurry, the mass ratio of sodium hydroxide, sulfur and hot water is 1:2:10.

[0064] In some embodiments, S1 specifically includes: adding sodium hydroxide into hot water at a first temperature, stirring and melting, and maintaining the heating state to obtain a sodium hydroxide solution;

[0065] In some embodiments, S2 specifically includes: adding sulfur slurry to sodium hydroxide solution, and then adding hot water at a first temperature to obtain a mixed slurry; reacting the mixed slurry under a second temperature condition, and when the mixed slurry appears reddish brown, stopping heating and filtering to obtain a reddish brown liquid reserve thallium solid agent.

[0066] In some embodiments, a thallium-fixing agent prepared by the preparation method in any of the above embodiments is also provided.

[0067] In some embodiments, a use of a thallium-fixing agent prepared by the preparation method in any of the above embodiments in lithium slag is also provided.

[0068] In some embodiments, a method for recycling lithium slag is also provided, comprising the following steps:

[0069] Mixing the reserve thallium-fixing agent obtained by the preparation method in any of the above embodiments with water to obtain the thallium-fixing agent;

[0070] dry-mixing lithium slag, cement and a quick-drying agent to obtain a mixture;

[0071] The mixture is mixed with a thallium-fixing agent and granulated to obtain cement aggregate balls;

[0072] Cement aggregate balls are used in concrete to realize the resource processing of lithium slag.

[0073] By using the thallium-fixing agent in any of the above embodiments to infiltrate and granulate lithium slag, the thallium content in the leaching liquid of the prepared cement aggregate balls can be lower than 5ppb, thereby effectively fixing the thallium in the lithium slag, and the prepared cement aggregate balls can be used as gravel in concrete, effectively realizing the resource utilization of lithium slag, solving the current problem of lithium slag treatment, and the thallium contained in the prepared concrete will not leak into the environment, effectively avoiding the damage of thallium to the environment.

[0074] In some embodiments, cement aggregate balls are mixed with water at a ratio of 1:10 in terms of g:mL, and then allowed to stand after being shaken to obtain a toxic leachate; the thallium content in the toxic leachate is less than 5 ppb.

[0075] Exemplarily, the cement aggregate balls are mixed with water at a ratio of 1:10 in terms of g:mL, horizontally shaken for 8 hours at room temperature, and allowed to stand for 16 hours to obtain a toxic leachate; the thallium content in the toxic leachate is less than 5 ppb.

[0076] In some embodiments, the water content of the lithium slag is less than or equal to 10%.

[0077] In some embodiments, the cement is 325 cement or 425 cement.

[0078] In some embodiments, the lithium slag is lithium slag obtained by extracting lithium from lepidolite by sulfate roasting.

[0079] In some embodiments, the fast-drying agent is a mixture of calcium aluminate, sodium aluminate, and sodium carbonate.

[0080] Exemplarily, the quick-drying agent is a mixture of 20% by weight calcium aluminate, 75% by weight sodium aluminate and 5% by weight sodium carbonate.

[0081] In some embodiments, the particle size of the cement aggregate balls is 4 mm to 24 mm.

[0082] In some embodiments, cement aggregate balls are used as stones in concrete.

[0083] In some embodiments, the mass ratio of the thallium-fixing agent to water is 1:20-22.

[0084] Exemplarily, the mass ratio of the reserve thallium solid agent to water is 1:22.

[0085] In some embodiments, the mass ratio of lithium slag (with a moisture content of 0), cement, quick-drying agent and total water (the total water includes added water, water contained in the lithium slag and water contained in the thallium-fixing agent) is 100:20-22:2-2.2:35-40.

[0086] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the preparation method of the thallium solid agent and the resource treatment method of lithium slag of the present invention will be further described in detail below in combination with specific embodiments and drawings. Obviously, the specific embodiments described are only part of the embodiments of the present application, not all of them. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation to the present application and its application. Based on the specific embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work belong to the scope of protection of the present application.

[0087] If no specific techniques or conditions are specified in the specific embodiments, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0088] Example 1

[0089] A method for recycling lithium slag comprises the following steps:

[0090] S1. Preparation of reserve thallium solid agent:

[0091] S11, adding 10g of sodium hydroxide to 20g of hot water at a temperature of 85°C, stirring for 30min to obtain a sodium hydroxide solution, and keeping the sodium hydroxide solution heated at a constant temperature; adding 20g of sulfur to 40g of hot water at a temperature of 85°C, stirring for 10min to obtain a sulfur slurry;

[0092] S12, adding sulfur slurry to sodium hydroxide solution, and then adding hot water at 85°C, so that the mass ratio of sodium hydroxide, sulfur and water in the mixed slurry is 1:2:11; then raising the temperature of the mixed slurry to 99°C, reacting at high temperature until the solution turns reddish brown, stopping heating, filtering to obtain a reddish brown liquid, which is the reserve thallium solid agent;

[0093] S2. Preparation of cement aggregate balls from lithium slag:

[0094] S21, taking 10 g of the reserve thallium-fixing agent obtained in S1, adding it to 220 g of water, mixing evenly, to obtain a thallium-fixing agent;

[0095] S22, in a disc granulator, 1000g of lithium slag after lithium extraction from lithium mica ore with a water content of 10% by sulfate roasting, 198g of 325 cement and 19.8g of quick-drying agent are dry-mixed, and mixed evenly to obtain a mixture; in the mixture, the mass ratio of lithium slag (water content is 0): cement and quick-drying agent is 100:22:2.2;

[0096] S23, transport the mixture in S22 to a disc granulator by a belt, and then spray 260g of the thallium-fixing agent in S21 into the mixture in the disc granulator. The lithium slag, cement and quick-drying agent are balled under the rotation of the disc granulator and the wetting of the thallium-fixing agent. The lithium slag (with a moisture content of 0): cement: quick-drying agent: total water (the total water includes the added water, the water contained in the lithium slag and the water contained in the thallium-fixing agent) = 100:22:2.2:40. After the balls are made, they can be condensed into harder cement aggregate balls within 20 minutes, and then sieved to obtain cement aggregate balls with a particle size of 4mm to 24mm. After the toxicity leaching test, the thallium content in the toxic leaching solution is 4.3ppb; the actual picture of the prepared cement aggregate balls is as follows Figure 1 As shown, the cement aggregate balls can replace gravel in road concrete, thereby realizing the resource utilization of lithium slag.

[0097] Example 2

[0098] A method for recycling lithium slag comprises the following steps:

[0099] S1. Preparation of reserve thallium solid agent:

[0100] S11, adding 10 g of sodium hydroxide to 22 g of hot water at a temperature of 80° C., stirring for 10 min to obtain a sodium hydroxide solution, and keeping the sodium hydroxide solution heated at a constant temperature; adding 22 g of sulfur to 48.4 g of hot water at a temperature of 80° C., stirring for 30 min to obtain a sulfur slurry;

[0101] S12, adding sulfur slurry to sodium hydroxide solution, and then adding hot water at 80°C, so that the mass ratio of sodium hydroxide, sulfur and water in the mixed slurry is 1:2.2:12; then raising the temperature of the mixed slurry to 95°C, reacting at high temperature until the solution turns reddish brown, stopping heating, filtering to obtain a reddish brown liquid, which is the reserve thallium solid agent;

[0102] S2. Preparation of cement aggregate balls from lithium slag:

[0103] S21, taking 10 g of the reserve thallium-fixing agent obtained in S1, adding it to 200 g of water, mixing evenly, to obtain a thallium-fixing agent;

[0104] S22, in a disc granulator, 1000g of lithium slag obtained by calcining lithium from lithium mica ore with a water content of 5%, 190g of 425 cement and 19g of quick-drying agent are dry-mixed, and mixed evenly to obtain a mixture. In the mixture, the mass ratio of lithium slag (water content is 0): cement and quick-drying agent is 100:20:2;

[0105] S23, transport the mixture in S22 to a disc granulator by a belt, and then spray 282.5g of thallium-fixing agent in S21 into the mixture in the disc granulator, and make balls of lithium slag, cement and quick-drying agent under the rotation of the disc granulator and the wetting of the thallium-fixing agent, lithium slag (with a moisture content of 0): cement: quick-drying agent: total water (the total water includes the added water, the water contained in the lithium slag and the water contained in the thallium-fixing agent) = 100:20:2:35, and the balls can be condensed into harder cement aggregate balls within 20 minutes after being made, and then sieved to obtain cement aggregate balls with a particle size of 4mm to 24mm. After toxic leaching experiments, the thallium content in the toxic leaching solution is 3.9ppb; the actual picture of the prepared cement aggregate balls is as follows Figure 1 As shown, the cement aggregate balls can replace gravel in road concrete, thereby realizing the resource utilization of lithium slag.

[0106] Example 3

[0107] A method for recycling lithium slag comprises the following steps:

[0108] S1. Preparation of reserve thallium solid agent:

[0109] S11, adding 10g of sodium hydroxide to 21g of hot water at a temperature of 83°C, stirring for 20min to obtain a sodium hydroxide solution, and keeping the sodium hydroxide solution heated at a constant temperature; adding 21g of sulfur to 44.1g of hot water at a temperature of 83°C, stirring for 20min to obtain a sulfur slurry;

[0110] S12, adding sulfur slurry to sodium hydroxide solution, and then adding hot water at 83°C, so that the mass ratio of sodium hydroxide, sulfur and water in the mixed slurry is 1:2.2:12; then raising the temperature of the mixed slurry to 97°C, reacting at high temperature until the solution turns reddish brown, stopping heating, filtering to obtain a reddish brown liquid, which is the reserve thallium solid agent;

[0111] S2. Preparation of cement aggregate balls from lithium slag:

[0112] S21, taking 10 g of the reserve thallium-fixing agent obtained in S1, adding it to 210 g of water, mixing evenly, to obtain a thallium-fixing agent;

[0113] S22, in a disc granulator, 1000g of lithium slag after lithium extraction from lithium mica ore with a water content of 0% by sulfate roasting, 210g of 425 cement and 21g of quick-drying agent are dry-mixed, and mixed evenly to obtain a mixture. In the mixture, the mass ratio of lithium slag (water content is 0): cement and quick-drying agent is 100:21:2.1;

[0114] S23, transport the mixture in S22 to a disc granulator by a belt, and then spray 370g of the thallium-fixing agent in S21 into the mixture in the disc granulator. The lithium slag, cement and quick-drying agent are balled under the rotation of the disc granulator and the wetting of the thallium-fixing agent. The lithium slag (with a moisture content of 0): cement: quick-drying agent: total water (the total water content includes the added water, the water contained in the lithium slag and the water contained in the thallium-fixing agent) = 100:21:2.1:37. After the balls are made, they can be condensed into harder cement aggregate balls within 20 minutes, and then sieved to obtain cement aggregate balls with a particle size of 4mm to 24mm. After the toxicity leaching test, the thallium content in the toxic leaching solution is 4.2ppb; the actual picture of the prepared cement aggregate balls is as follows Figure 1 As shown, the cement aggregate balls can replace gravel in road concrete, thereby realizing the resource utilization of lithium slag.

[0115] Comparative Example 1 (without reinforcing thallium agent)

[0116] A method for recycling lithium slag comprises the following steps:

[0117] S1. Preparation of cement aggregate balls from lithium slag:

[0118] S11, in a disc granulator, 1000g of lithium slag after lithium extraction from lithium mica ore with a water content of 10% by sulfate roasting, 198g of 325 cement and 19.8g of quick-drying agent are dry-mixed, and mixed evenly to obtain a mixture. In the mixture, the mass ratio of lithium slag (water content is 0): cement and quick-drying agent is 100:22:2.2;

[0119] S12, transporting the mixture in S22 to a disc granulator by a belt, spraying 260g of tap water into the mixture in the disc granulator, and making balls of lithium slag, cement and quick-drying agent under the rotation of the disc granulator and the wetting of the thallium-fixing agent, lithium slag (with a moisture content of 0): cement: quick-drying agent: total water (the total water content includes the added water, the water contained in the lithium slag and the water contained in the thallium-fixing agent) = 100:22:2.2:40, and the balls can be condensed into harder cement aggregate balls within 20 minutes after being made, and then sieved to obtain cement aggregate balls with a particle size of 4mm to 24mm. After toxic leaching experiments, the thallium content in the toxic leaching solution is 8.6ppb; since the thallium content in the leaching solution exceeds the specified 5ppb, the cement aggregate balls cannot replace gravel in road concrete, and the resource utilization of lithium slag cannot be achieved.

[0120] Comparative Example 2 (without cement)

[0121] A method for recycling lithium slag comprises the following steps:

[0122] S1. Preparation of reserve thallium solid agent:

[0123] S11, adding 10g of sodium hydroxide to 22g of hot water at a temperature of 80°C, stirring for 20min to obtain a sodium hydroxide solution, and keeping the sodium hydroxide solution heated at a constant temperature; adding 22g of sulfur to 48.4g of hot water at a temperature of 80°C, stirring for 20min to obtain a sulfur slurry;

[0124] S12, adding sulfur slurry to sodium hydroxide solution, and then adding hot water at 80°C, so that the mass ratio of sodium hydroxide, sulfur and water in the mixed slurry is 1:2.2:12; then raising the temperature of the mixed slurry to 95°C, reacting at high temperature until the solution turns reddish brown, stopping heating, filtering to obtain a reddish brown liquid, which is the reserve thallium solid agent;

[0125] S2. Preparation of cement aggregate balls from lithium slag:

[0126] S21, taking 10 g of the reserve thallium-fixing agent obtained in S1, adding it to 200 g of water, mixing evenly, to obtain a thallium-fixing agent;

[0127] S22, in a disc granulator, dry-mix 1000g of lithium slag obtained by calcining lithium from lithium mica ore with a water content of 5% with sulfate and 19g of a quick-drying agent, and mix them evenly to obtain a mixture. In the mixture, the mass ratio of lithium slag (water content of 0) to quick-drying agent is 100:2;

[0128] S23. The mixture in S22 is transported to a disc granulator by a belt, and 282.5 g of the thallium-fixing agent in S21 is sprayed into the mixture in the disc granulator. The lithium slag and the quick-drying agent are balled under the rotation of the disc granulator and the wetting of the thallium-fixing agent. The lithium slag (water content is 0): quick-drying agent: total water content = 100:2:35. This method forms agglomerates, but does not form balls after drying, but becomes powder. After toxic leaching experiments, the thallium content in the toxic leaching solution is 9.4 ppb. Since the thallium content in the leaching solution exceeds the specified 5 ppb, the cement aggregate balls cannot replace gravel in road concrete, and the resource utilization of lithium slag cannot be achieved.

[0129] Detection and analysis

[0130] 1) Determination of thallium content in cement aggregate ball leachate

[0131] The specific operation steps are as follows: 100 g of the cement aggregate balls prepared in Example 1 and Control Example 1, and lithium slag obtained by calcining lithium mica ore without any treatment with sulfate are added into 1000 mL of water, horizontally shaken at room temperature for 8 hours, and allowed to stand for 16 hours to obtain a toxic leachate, and the toxic leachate is taken to analyze the thallium content.

[0132] The results show that the thallium content in the toxic leachate of the cement aggregate balls prepared in Example 1, Example 2 and Example 3 is less than 5 ppb. The thallium content in the toxic leachate of the cement aggregate balls prepared in Control Example 1 and Control Example 2 is higher than 5 ppb. The thallium content in the toxic leachate of the lithium slag after lithium extraction from lithium mica ore without any treatment by sulfate roasting is 26 ppb.

[0133] In summary, the preparation method of the thallium-fixing agent of the present invention is to further heat the heated sodium hydroxide solution and sulfur slurry to react, and the obtained reddish-brown product liquid can solidify the thallium in the lithium slag. When used in combination with cement, the cement and the thallium-fixing agent have a synergistic thallium-fixing effect, so that the thallium content in the leaching solution of the lithium slag after thallium fixing is lower than 5ppb, which is within the prescribed standard of less than 5ppb, thereby avoiding the risk of thallium leakage from the long-term stored lithium slag and causing damage to the surrounding environment.

[0134] The resource treatment method of lithium slag of the present invention uses the thallium fixing agent of the present invention to infiltrate and granulate the lithium slag, so that the thallium content in the leaching solution of the prepared cement aggregate balls leached again can be lower than 5ppb, thereby effectively realizing the fixation of thallium in the lithium slag, and the prepared cement aggregate balls can be used as stones in concrete, effectively realizing the resource utilization of lithium slag, solving the current treatment problem of lithium slag, and the thallium contained in the prepared concrete will not leak into the environment, effectively avoiding the damage of thallium to the environment, and having promotion and application value in the technical field of lithium slag resource utilization.

[0135] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.

Claims

1. A method for preparing a thallium-fixing agent, characterized in that: The following steps are involved: S1, adding sodium hydroxide into hot water at a first temperature, stirring for 10 min to 30 min, to obtain a sodium hydroxide solution; Adding sulfur into hot water at the first temperature and stirring for 10 to 30 minutes to obtain sulfur slurry; S2, adding sulfur slurry to sodium hydroxide solution, and then adding hot water at a first temperature to obtain a mixed slurry; reacting the mixed slurry under a second temperature condition to obtain a reserve thallium solid agent; The second temperature is greater than the first temperature.

2. The method for preparing the thallium-fixing agent according to claim 1, characterized in that: The first temperature is greater than or equal to 80°C; and / or, the second temperature is greater than or equal to 95° C.; And / or, the mixed slurry is reacted under the second temperature condition for 1 hour to 1.5 hours.

3. The method for preparing the thallium-fixing agent according to claim 1, characterized in that: In the sodium hydroxide solution, the mass ratio of sodium hydroxide to hot water is 1:2 to 2.2; and / or, in the sulfur slurry, the mass ratio of sulfur to hot water is 1:2 to 2.2; And / or, in the mixed slurry, the mass ratio of sodium hydroxide, sulfur and hot water is 1:2-2.2:10-12.

4. The method for preparing the thallium-fixing agent according to claim 1, characterized in that: The step S1 specifically includes: adding sodium hydroxide into hot water at a first temperature, stirring and melting, and maintaining the heating state to obtain a sodium hydroxide solution; And / or, S2 specifically includes: adding sulfur slurry to sodium hydroxide solution, and then adding hot water at a first temperature to obtain a mixed slurry; reacting the mixed slurry under a second temperature condition, and when the mixed slurry appears reddish brown, stopping heating and filtering to obtain a reddish brown liquid reserve thallium solid agent.

5. A thallium-fixing agent obtained by the preparation method according to any one of claims 1 to 4.

6. An application of a thallium-fixing agent obtained by the preparation method according to any one of claims 1 to 4, characterized in that: Application of the thallium-fixing agent in lithium slag.

7. A method for recycling lithium slag, characterized in that: The following steps are involved: Mixing the reserve thallium-fixing agent obtained by the preparation method according to any one of claims 1 to 4 with water to obtain the thallium-fixing agent; dry-mixing lithium slag, cement and a quick-drying agent to obtain a mixture; The mixture is mixed with a thallium-fixing agent and granulated to obtain cement aggregate balls; The cement aggregate balls are used in concrete to realize resource processing of lithium slag.

8. The method for recycling lithium slag according to claim 7, characterized in that: The cement aggregate balls and water are mixed at a ratio of 1:10 in terms of g:mL, shaken and then allowed to stand to obtain a toxic leachate; the thallium content in the toxic leachate is less than 5 ppb.

9. The method for recycling lithium slag according to claim 7, characterized in that: The water content of the lithium slag is less than or equal to 10%; And / or, the lithium slag is lithium slag obtained by extracting lithium from lepidolite by sulfate roasting; And / or, the quick-drying agent is a mixture of calcium aluminate, sodium aluminate and sodium carbonate; And / or, the particle size of the cement aggregate balls is 4 mm to 24 mm; And / or, the cement aggregate balls are used as stones in concrete.

10. The method for recycling lithium slag according to claim 7, characterized in that: The mass ratio of the reserve thallium-fixing agent to water is 1:20-22; And / or, the mass ratio of the lithium slag, cement, quick-drying agent and total water is 100:20-22:2-2.2:35-40.

Citation Information

Patent Citations

  • Method for synthesizing sulfur-containing silane coupling agent from sodium polysulfide

    CN102875587A

  • Method for recovering thallium and rhenium from smelting acidic wastewater

    CN109626414A

  • Method for preparing thallium chloride using thallium-containing acidic wastewater of smelting plant as raw material

    CN109850935A

  • Preparation method of lithium slag concrete

    CN111646773A

  • Thallium-containing desulfurization wastewater advanced treatment device and treatment method

    CN112537860A