Method for repairing giant bearing seat through laser
Through laser repair methods, the wear-resistant and corrosion-resistant cobalt-based alloy cladding layer is welded after cleaning and turning, which solves the wear problem of giant bearing seats, extends service life and reduces costs, and achieves efficient repair of giant bearing seats.
Patent Information
- Application Number
- CN202411174984.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-26
AI Technical Summary
The giant bearing seat cannot cooperate with the giant bearing due to wear during use, and the existing repair methods cannot be completely repaired, resulting in a short service life and high cost, and requires frequent replacement.
Using laser repair method, the impurities are removed through cleaning tools, the inner wall is turned, the welding route is designed and the wear-resistant and corrosion-resistant cobalt-based alloy cladding layer is welded with a thickness of 1+0.5mm and the surface hardness is HRC40-45 , the mechanical properties reach Rm≥900N/mm2, Rel≥700N/mm2, Z≥50%, A5≥12%, AKDVM≥50J.
It significantly extends the service life of the giant bearing seat, avoids the problems of frequent replacement and customization, reduces the cost of use, and the welded cladding can be reused.
Smart Images

Figure CN119017004A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of laser repair of giant bearing seats and relates to a method for laser repair of giant bearing seats. Background Art
[0002] The giant bearing seat is a component of the giant steel rolling mill. Although lubricating oil is added to the connection between the giant bearing seat and the giant bearing, the inner wall of the giant bearing seat will also be worn and consumed during daily use. The wear will cause the giant bearing seat and the giant bearing to be unable to cooperate. Even if a new giant bearing is replaced, it cannot be used due to the large gap. Therefore, the worn giant bearing seat needs to be replaced, but the giant bearing seat weighs more than 20 tons and is large in size. To prepare an identical giant bearing seat again, it needs to be customized. However, this giant steel rolling mill is imported equipment from abroad. It costs about several million to customize a giant bearing seat, and it is difficult to transport it back from abroad, which further increases the cost.
[0003] Therefore, the existing method of repairing the giant bearing seat is to repair a rectangular bearing seat at a cost of only hundreds of thousands. The existing method of repairing the giant bearing seat is to repair the worn parts and supplement the worn size by welding the same material. Although this method can also repair the giant bearing seat, it does not take the approach of completely repairing the giant bearing seat, resulting in poor matching effect between the giant bearing seat and the giant bearing during use. At the same time, the environment in which the giant bearing seat is used is poor, generally in a high temperature, high humidity and corrosive environment, and the number of times it is used every day reaches tens of thousands, so the giant bearing seat is severely worn, resulting in the giant bearing seat needing to be replaced every 1-2 years. Therefore, in order to solve the above-mentioned technical problems, the technical solution of the present application is set up. Summary of the invention
[0004] The purpose of the present invention is to provide a method for laser repairing a giant bearing seat, thereby solving the above-mentioned technical problems.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A method for laser repairing a giant bearing seat comprises the following steps:
[0007] S1: Remove impurities
[0008] First, place the giant bearing seat horizontally, and then use the cleaning tool to remove most of the impurities on the outer wall and the upper end of the giant bearing seat. Then place the giant bearing seat vertically, and then use the cleaning tool to remove most of the impurities on the bottom of the outer wall of the giant bearing seat, and also use it to remove impurities on the inner wall of the giant bearing seat.
[0009] S2: Remove impurities
[0010] The impurities on the outer wall and inner wall of the giant bearing seat are fully removed by cleaning equipment, so that the outer wall is completely exposed to the cast iron material, and the inner wall is also completely exposed to the cast iron material;
[0011] S3: Remove moisture
[0012] The moisture on the inner wall of the giant bearing seat is absorbed by the absorbent cloth, and then the entire giant bearing seat is placed horizontally to completely remove the moisture on the inner wall of the giant bearing seat;
[0013] S4: Turning inner wall
[0014] Place the entire giant bearing seat vertically, and then insert the turning tool into the inner wall of the giant bearing seat for turning, remove the holes and scratches on the inner wall of the giant bearing seat, and make the size of the inner wall of the giant bearing seat uniform;
[0015] S5: Welding Design
[0016] By measuring the inner wall of the giant bearing seat after turning, the welding route and number of welding times for the inner wall of the giant bearing seat are designed, and the welding position is designed according to the size of the laser welding machine;
[0017] S6: Laser welding
[0018] A multi-angle laser welding machine is used. According to the size of the giant bearing seat, a plan for simultaneous welding on both sides is designed. Two sets of identical laser welding machines weld from the two outer sides of the inner wall of the giant bearing seat to the inner side respectively. After each welding intersection, welding is performed again from the outer side to the inner side.
[0019] S7: Turning allowance
[0020] After the giant bearing seat is welded, the dimensions between the inner walls of the giant bearing seat are measured again and calculated with the required dimensions. The required dimensions of the inner wall of the giant bearing seat are obtained by cutting the excess with a turning tool.
[0021] The working principle of the present invention is as follows: the present invention welds a wear-resistant and corrosion-resistant cobalt-based alloy on the inner wall of the giant bearing seat, the thickness of the laser welding cladding layer is 1+0.5mm, the surface hardness is HRC40-45, and the mechanical properties are as follows: R m ≥900N / mm 2 , R el ≥700N / mm 2 , Z≥50%, A5≥12%, A KDVM≥50J, which improves the corrosion resistance of the giant bearing seat, and also improves the wear resistance of the giant bearing seat, ultimately greatly extending the service life of the giant bearing seat, avoiding the problem of the giant bearing seat needing to be prepared or customized after wear. At the same time, after the welded cladding layer of the present application is worn, it is only necessary to repeat the process steps of the present application, so that the giant bearing seat can be reused, thereby greatly reducing the cost and life of the giant rolling mill.
[0022] Furthermore: the cleaning tool includes a scraper, the impurities include a mixture of engine oil, lubricating oil, mud, and dust, and the impurities also include rust on the outer wall of the giant bearing seat.
[0023] Furthermore: the cleaning equipment includes a high-pressure water gun, which is used to remove the mixture of engine oil, lubricating oil, mud, and dust on the outer wall and inner wall of the giant bearing seat, thereby completely removing the rust.
[0024] Furthermore: one side of the outer wall of the giant bearing seat is turned by a turning tool, and the turning tool is taken out after turning to a predetermined position, and the orientation of the giant bearing seat is turned, so that the other side of the inner wall of the giant bearing seat is turned, and the length of the turning tool is increased, and the turning is performed multiple times with a small allowance.
[0025] Further: The thickness of the laser welding cladding layer is 1+0.5mm, the surface hardness is HRC40-45, and the mechanical properties requirements are: R m ≥900N / mm 2 , R el ≥700N / mm 2 , Z≥50%, A5≥12%, A KDVM ≥50J.
[0026] Furthermore: after turning, the edges and burrs are removed, and after the removal, the inner wall of the giant bearing seat is subjected to non-destructive testing, and the non-destructive testing is carried out according to the level 2 acceptance specified in the EZB / N31-2002 standard.
[0027] Furthermore: the material for laser welding is a cobalt-based alloy.
[0028] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0029] 1. A method for laser repairing a giant bearing seat. This application aims to solve the problem of the large size of the giant bearing seat by setting a welding route to use two identical laser welding machines, both of which are multi-angle welding machines. The two welding machines weld from the two outer sides of the inner wall of the giant bearing seat to the inner side respectively, and weld from the outer side to the inner side again after each welding intersection connection;
[0030] 2. In the present invention, the inner wall of the giant bearing seat is cleaned by a turning tool, and the holes and scratches on the inner wall of the giant bearing seat are cleaned by the turning tool, so that the size of the inner wall of the giant bearing seat is uniform, which avoids the inability to repair the holes and scratches during laser welding, resulting in the welded cladding layer only covering the surface;
[0031] 3. In the present invention, the method of the application improves the corrosion resistance of the giant bearing seat by welding a wear-resistant and corrosion-resistant cobalt-based alloy on the inner wall of the giant bearing seat, and also improves the wear resistance of the giant bearing seat, thereby greatly extending the service life of the giant bearing seat. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative work, among which:
[0033] Figure 1 , Figure 2 , Figure 3 This is a real picture of the giant bearing seat in the present invention before being repaired. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations.
[0035] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0036] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0037] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0038] Embodiment 1
[0039] The present invention provides a method for laser repairing a giant bearing seat, such as Figure 1 , Figure 2 , Figure 3 As shown, the giant bearing seat is first placed horizontally, and then the cleaning tool is used to remove most of the impurities on the outer wall and the upper end of the giant bearing seat. Then the giant bearing seat is placed vertically, and then the cleaning tool is used to remove most of the impurities on the bottom of the outer wall of the giant bearing seat, and the impurities on the inner wall of the giant bearing seat are also removed.
[0040] The impurities on the outer wall and inner wall of the giant bearing seat are fully removed by cleaning equipment, so that the outer wall is completely exposed to the cast iron material, and the inner wall is also completely exposed to the cast iron material;
[0041] The moisture on the inner wall of the giant bearing seat is absorbed by the absorbent cloth, and then the entire giant bearing seat is placed horizontally to completely remove the moisture on the inner wall of the giant bearing seat;
[0042] Place the entire giant bearing seat vertically, and then insert the turning tool into the inner wall of the giant bearing seat for turning, remove the holes and scratches on the inner wall of the giant bearing seat, and make the size of the inner wall of the giant bearing seat uniform;
[0043] By measuring the inner wall of the giant bearing seat after turning, the welding route and number of welding times for the inner wall of the giant bearing seat are designed, and the welding position is designed according to the size of the laser welding machine;
[0044] A multi-angle laser welding machine is used. According to the size of the giant bearing seat, a plan for simultaneous welding on both sides is designed. Two sets of identical laser welding machines weld from the two outer sides of the inner wall of the giant bearing seat to the inner side respectively. After each welding intersection, welding is performed again from the outer side to the inner side.
[0045] After the giant bearing seat is welded, the dimensions between the inner walls of the giant bearing seat are measured again and calculated with the required dimensions. The required dimensions of the inner wall of the giant bearing seat are obtained by cutting the excess with a turning tool.
[0046] The specific implementation method of this embodiment is as follows: before welding the giant bearing seat, impurities are removed first. The impurities include a mixture of engine oil, lubricating oil, mud, and dust. The impurities also include rust, a mixture of rust and engine oil or lubricating oil. The purpose of removing these impurities is to ensure that the part of the giant bearing seat that needs to be welded is clean and directly welded to the inner wall of the giant bearing seat, thereby avoiding impurities between the inner wall of the giant bearing seat and the welded laser cladding layer. These impurities will affect the stability of the laser cladding layer welding, thereby affecting the coordinated use of the giant bearing seat and the giant bearing, and at the same time affecting the performance of the giant bearing seat. Removing impurities avoids the problem of damage to the laser cladding layer due to wear after a period of use, thereby causing rupture.
[0047] The rust between the inner walls of the giant bearing seat is removed through rust removal treatment, so that the inner walls of the giant bearing seat are all smooth cast iron surfaces, and the laser cladding layer is directly welded to the smooth cast iron surface, thereby avoiding the rust from affecting the quality and stability of the laser welding layer. After cleaning, the inner wall of the giant bearing seat is dried by absorbing water and drying, avoiding moisture adhering to the inner wall of the giant bearing seat during welding, and further avoiding affecting the quality and stability of the laser welding layer.
[0048] After the impurities on the inner wall of the giant bearing seat are cleaned, the inner wall of the giant bearing seat is first cleaned with a turning tool. The holes and scratches on the inner wall of the giant bearing seat are removed by the turning tool, so that the size of the inner wall of the giant bearing seat is uniform, avoiding the inability to repair the holes and scratches during laser welding, resulting in the welding cladding layer only covering the surface, while the holes and scratches on the inner wall of the giant bearing seat still exist, resulting in the problem that the giant bearing seat is easy to cooperate poorly with the giant bearing after being used for a period of time.
[0049] In order to solve the problem of large size of giant bearing seats, the present application sets the welding route to use two identical laser welding machines, both of which are multi-angle welding machines. The two welding machines respectively weld from the two outer sides of the inner wall of the giant bearing seat to the inner side, and weld from the outer side to the inner side again after each welding intersection. By completing the designed number of welding times, all welding of the inner wall of the giant bearing seat is completed. This welding method avoids the problem that the inner wall of the giant bearing seat is welded at different time periods, resulting in different welding performance and abnormalities at the intersection. The present application adopts synchronous welding on both sides, so that the cooling time of the laser welding is the same and the connection performance at the intersection is better, which is convenient to meet the welding requirements of the giant bearing seat.
[0050] This application welds a wear-resistant and corrosion-resistant cobalt-based alloy on the inner wall of a giant bearing seat. The thickness of the laser welding cladding layer is 1+0.5mm, the surface hardness is HRC40-45, and the mechanical properties are required to be: R m ≥900N / mm 2 , R el ≥700N / mm 2 , Z≥50%, A5≥12%, A KDVM ≥50J, which improves the corrosion resistance of the giant bearing seat, and also improves the wear resistance of the giant bearing seat, ultimately greatly extending the service life of the giant bearing seat, avoiding the problem of the giant bearing seat needing to be prepared or customized after wear. At the same time, after the welded cladding layer of the present application is worn, it is only necessary to repeat the process steps of the present application, so that the giant bearing seat can be reused, thereby greatly reducing the cost and life of the giant rolling mill.
[0051] The present application adopts multiple times and small allowance processing for the giant bearing seat after welding, and first turns one side of the outer wall of the giant bearing seat by a turning tool, takes out the turning tool after turning to a predetermined position, and at the same time turns the orientation of the giant bearing seat so that the other side of the inner wall of the giant bearing seat is turned, and at the same time increases the length of the turning tool so that the synchronization of turning the giant bearing seat is met, removes the edges and burrs after turning, and performs non-destructive testing on the inner wall of the giant bearing seat after removal, and the non-destructive testing is carried out according to the level 2 acceptance specified in the EZB / N31-2002 standard.
[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made by any technician familiar with the field within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for laser repairing a giant bearing seat, characterized in that: The following steps are involved: S1: Remove impurities First, place the giant bearing seat horizontally, and then use the cleaning tool to remove most of the impurities on the outer wall and the upper end of the giant bearing seat. Then place the giant bearing seat vertically, and then use the cleaning tool to remove most of the impurities on the bottom of the outer wall of the giant bearing seat, and also use it to remove impurities on the inner wall of the giant bearing seat. S2: Remove impurities The impurities on the outer wall and inner wall of the giant bearing seat are fully removed by cleaning equipment, so that the outer wall is completely exposed to the cast iron material, and the inner wall is also completely exposed to the cast iron material; S3: Remove moisture The moisture on the inner wall of the giant bearing seat is absorbed by the absorbent cloth, and then the entire giant bearing seat is placed horizontally to completely remove the moisture on the inner wall of the giant bearing seat; S4: Turning inner wall Place the entire giant bearing seat vertically, and then insert the turning tool into the inner wall of the giant bearing seat for turning, remove the holes and scratches on the inner wall of the giant bearing seat, and make the size of the inner wall of the giant bearing seat uniform; S5: Welding Design By measuring the inner wall of the giant bearing seat after turning, the welding route and number of welding times for the inner wall of the giant bearing seat are designed, and the welding position is designed according to the size of the laser welding machine; S6: Laser welding A multi-angle laser welding machine is used. According to the size of the giant bearing seat, a plan for simultaneous welding on both sides is designed. Two sets of identical laser welding machines weld from the two outer sides of the inner wall of the giant bearing seat to the inner side respectively. After each welding intersection, welding is performed again from the outer side to the inner side. S7: Turning allowance After the giant bearing seat is welded, the dimensions between the inner walls of the giant bearing seat are measured again and calculated with the required dimensions. The required dimensions of the inner wall of the giant bearing seat are obtained by cutting the excess with a turning tool.
2. The method for laser repairing a giant bearing seat according to claim 1, characterized in that: Cleaning tools include scrapers, and impurities include a mixture of engine oil, lubricating oil, mud, dust, and impurities also include rust on the outer wall of the giant bearing seat.
3. The method for laser repairing a giant bearing seat according to claim 1, characterized in that: The cleaning equipment includes a high-pressure water gun, which is used to remove the mixture of engine oil, lubricating oil, mud, and dust on the outer and inner walls of the giant bearing seat, thereby completely removing the rust.
4. The method for laser repairing a giant bearing seat according to claim 1, characterized in that: The turning tool is used to turn one side of the outer wall of the giant bearing seat first. After turning to the predetermined position, the turning tool is taken out and the orientation of the giant bearing seat is turned so that the other side of the inner wall of the giant bearing seat is turned. At the same time, the length of the turning tool is increased and the turning is performed multiple times with small allowances.
5. The method for laser repairing a giant bearing seat according to claim 1, characterized in that: The thickness of the laser welding cladding layer is 1+0.5mm, the surface hardness is HRC40-45, and the mechanical properties requirements are: R m ≥900N / mm 2 , R el ≥700N / mm 2 , Z≥50%, A5≥12%, A KDVM ≥50J.
6. The method for laser repairing a giant bearing seat according to claim 1, characterized in that: After turning, the edges and burrs are removed. After removal, the inner wall of the giant bearing seat is subjected to non-destructive testing. The non-destructive testing is carried out according to the level 2 acceptance specified in the EZB / N31-2002 standard.
7. The method for laser repairing a giant bearing seat according to claim 1, characterized in that: The material for laser welding is cobalt-based alloy.
Citation Information
Patent Citations
Laser repair method for abraded centrifugal fan bearing block
CN102031519A
Repairing method for bearing seat
CN104801919A
Repair method for hot rolling of large rolling mill bearing seat
CN114918611A
Dual light beams welding method for laser welding
CN1657222A
Method for repairing surface cracks of shaft parts