Preparation method of light-colored copper hydroxyphosphate laser welding material
By adjusting the pH value of the reaction system and carrying out hydrothermal reaction, a copper hydroxyphosphate laser welding material with a color close to white was prepared, which solved the problem of material color difference and uneven particle, improved the application prospects and thermal stability of the product, and reduced the Wastewater volume and production cost.
Patent Information
- Application Number
- CN202411133213.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing copper hydroxyphosphate materials used for laser welding have color difference between light green and white or transparent plastic products, and the particles are uneven in coarse and fineness, which affects industrial production and welding applications.
By adjusting the pH value to 4.2-4.8 in the reaction system, performing a primary or secondary hydrothermal reaction, a copper hydroxyphosphate laser welding material with a color closer to white is prepared, and the particle size distribution is controlled uniformly. Saturated solution and ammonia water droplet addition technology is used. To reduce the amount of wastewater and increase the conversion rate of copper ions.
The color of copper hydroxyphosphate is nearly white, reducing the impact on the appearance of plastic products, uniform particle size distribution, reducing wastewater volume and production costs, and improving the thermal stability and application prospects of the product.
Smart Images

Figure HDA0004998555150000011 
Figure HDA0004998555150000012 
Figure HDA0004998555150000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laser welding materials, in particular to a method for preparing a light-colored copper hydroxyphosphate laser welding material. Background Art
[0002] Due to process or structural considerations, many plastic products or plastic parts may be assembled from parts of different materials and functions, and two parts need to be connected for a second time to be assembled together. There are many ways to connect plastics. Laser welding is the main way to connect thermoplastic parts. This method has accurate connection areas, a small impact range, high efficiency and no contact, and is suitable for large-scale industrial production. In laser welding, welding additives are one of the important additives. The additives are generally colored organic or inorganic pigments, which can increase the absorption of lasers and generate heat to weld plastics together. Among them, inorganic pigments are popular because of their good dispersibility and good thermal stability. Under the same input power, metal Cu with high thermal conductivity will produce molecular diffusion and entangled ideal thermal field distribution during welding, which is conducive to increasing welding strength. And copper hydroxyphosphate (Cu2(OH)PO4) containing high thermal conductivity Cu shows strong absorption in the near-infrared region, so it has good prospects in plastic welding.
[0003] Nowadays, most of the hydroxy copper phosphate used for laser welding materials is light green, which has a more obvious color difference compared with white or transparent plastics, and will affect the appearance of white or transparent plastic products to a certain extent. Therefore, it is very necessary to study a preparation method of hydroxy copper phosphate with a lighter color to improve the appearance of plastic products. In addition, the hydroxy copper phosphate currently available for laser welding materials still has the problem of uneven particle size, which also causes certain difficulties in its industrial production and welding applications. If this problem can be further improved, then hydroxy copper phosphate will have a better application prospect in the field of plastic welding. Summary of the invention
[0004] The invention provides a method for preparing a light-colored copper hydroxyphosphate laser welding material, which can make the color of the prepared copper hydroxyphosphate closer to white, thereby minimizing the impact on the appearance of plastic products.
[0005] To achieve the above object, the technical solution of the present invention is: A method for preparing a light-colored copper hydroxyphosphate laser welding material specifically comprises the following steps: mixing an excess soluble phosphate solution with a soluble copper salt solution, adjusting the pH to 4.2-4.8, performing a hydrothermal reaction, filtering after the reaction, separating a filtrate and a precipitate, washing and drying the precipitate, and preparing the copper hydroxyphosphate laser welding material.
[0006] Furthermore, the preparation method of the above-mentioned light-colored copper hydroxyphosphate laser welding material comprises the following steps: (1) Weigh a soluble copper salt and a soluble phosphate according to a molar ratio of Cu:P=1:1-3.5, dissolve them in deionized water, and mix them to obtain solution A; (2) slowly adding an alkaline solution to the solution A to adjust the pH value of the solution to 4.2-4.8, to obtain a solution B; (3) Transfer solution B into a polytetrafluoroethylene-lined reactor and conduct a hydrothermal reaction at a temperature of 120-180 °C for a reaction time of 2-6 h; (4) After the primary hydrothermal reaction is completed, the reaction is filtered to separate the primary filtrate and the primary precipitate, and the primary precipitate is washed and dried to obtain the hydroxy copper phosphate laser welding material.
[0007] Furthermore, during the primary hydrothermal reaction, the soluble phosphate solution and the soluble copper salt solution used are both saturated solutions.
[0008] Furthermore, the method further comprises step (5), wherein step (5) specifically comprises: adding a phosphate solution to the primary filtrate, adjusting the pH value to 4.2-4.8 with an alkaline solution, transferring the filtrate into a reactor lined with polytetrafluoroethylene, and performing a secondary hydrothermal reaction at a reaction temperature of 120-180°C for a reaction time of 2-6 h; filtering after the secondary hydrothermal reaction to separate a secondary filtrate and a secondary precipitate; washing and drying the secondary precipitate to obtain a hydroxy copper phosphate laser welding material.
[0009] Furthermore, in step (2), the alkaline solution is aqueous ammonia.
[0010] Furthermore, in step (5), the alkaline solution is aqueous ammonia.
[0011] Furthermore, in step (2), the alkaline solution is slowly added by a peristaltic pump, and the addition is completed within 25-35 minutes.
[0012] Furthermore, in step (5), the alkaline solution is slowly added by a peristaltic pump, and the addition is completed within 25-35 minutes.
[0013] Furthermore, in step (4), drying is carried out in an oven at a temperature of 80-100°C.
[0014] Furthermore, in step (5), drying is carried out in an oven at a temperature of 80-100°C.
[0015] The above-mentioned preparation method of the light-colored copper hydroxyphosphate laser welding material has the following advantages: The present invention can further adjust the color depth of copper hydroxyphosphate by adjusting the pH of the reaction system. When the pH of the reaction system is controlled at 4.2-4.8, the color of copper hydroxyphosphate is close to white. During laser welding, light-colored additives can be better used in the welding of white or transparent plastics, thereby minimizing the impact on the appearance of plastic products.
[0016] (2) The present invention further uses ammonia water to slowly adjust the pH value of the reaction system, so that the particle size distribution of the final precipitate obtained after drying is more uniform and can be used for laser welding without additional treatment.
[0017] (3) The present invention further uses a saturated copper salt solution and a phosphate solution to prepare copper hydroxyphosphate. When used in industrial production, the amount of wastewater generated will be relatively small, thus saving production costs, reducing the amount of wastewater, and being more energy-saving and environmentally friendly.
[0018] (4) After the first hydrothermal reaction is completed, the present invention adds soluble phosphate to carry out a secondary hydrothermal reaction, and the waste liquid containing copper ions can be reused. The conversion rate of copper ions is improved through the secondary hydrothermal reaction, and the copper ion content in the wastewater can be reduced. The process route is more environmentally friendly.
[0019] (5) The preparation method of the present invention is simple, and the product obtained has better thermal stability, which is conducive to better promotion and application in plastic laser welding. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is the XRD pattern of sample 1-7.
[0021] Figure 2 is the SEM image of sample 1.
[0022] Figure 3 It is a comparison of the thermogravimetric spectra of sample 1 and commercially available copper hydroxyphosphate at 50-680 °C.
[0023] Figure 4 This is a comparison chart of the particle size distribution of sample 1 and sample 7.
[0024] Figure 5 These are photographs of commercially available copper hydroxyphosphate and samples 1, 2, 5, and 6.
[0025] Figure 6 These are photographs of the primary filtrate and the secondary filtrate in Example 3. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following embodiments. Example 1
[0027] (1) Copper sulfate pentahydrate and ammonium dihydrogen phosphate were weighed according to a molar ratio of Cu:P=1:1, and dissolved in deionized water to prepare saturated solutions. The mixture was mixed by magnetic stirring to obtain solution A.
[0028] (2) Slowly add an aqueous ammonia solution to the solution A using a peristaltic pump, adjust the pH value of the solution to 4.7, and control the addition of the aqueous ammonia solution to be completed over 25 minutes to obtain a solution B.
[0029] (3) Solution B was transferred into a polytetrafluoroethylene-lined reactor and placed in an oven for a hydrothermal reaction at a temperature of 150 °C for 2 h.
[0030] (4) After the first hydrothermal reaction is completed, the reaction mixture is filtered to separate a first filtrate and a first precipitate. The first precipitate is washed and dried. The washing step is performed by washing with distilled water twice. The drying step is performed by drying in an oven at a temperature of 100 °C to obtain a hydroxy copper phosphate laser welding material. Example 2
[0031] (1) Copper acetate monohydrate and ammonium dihydrogen phosphate were weighed according to a molar ratio of Cu:P=1:3, and dissolved in deionized water to prepare saturated solutions. The mixture was mixed by magnetic stirring to obtain solution A.
[0032] (2) Slowly add an ammonia solution to the solution A using a peristaltic pump to adjust the pH value of the solution to 4.2. The ammonia solution is added over 30 min to obtain a solution B.
[0033] (3) Solution B was transferred into a polytetrafluoroethylene-lined reactor and placed in an oven for a hydrothermal reaction at a temperature of 180 °C for 2 h.
[0034] (4) After the first hydrothermal reaction is completed, the reaction mixture is filtered to separate a first filtrate and a first precipitate. The first precipitate is washed and dried. The washing step is performed by washing with distilled water twice. The drying step is performed by drying in an oven at a temperature of 100 °C to obtain a hydroxy copper phosphate laser welding material. Example 3
[0035] Example 3 is basically the same as Example 1, but based on Example 1, step (5) is added: (5) Add an appropriate amount of ammonium dihydrogen phosphate solution to the primary filtrate, adjust the pH value to 4.7 with an ammonia solution, control the addition of the ammonia solution for 25 minutes, transfer it to a reactor lined with polytetrafluoroethylene, and place it in an oven for a secondary hydrothermal reaction at a reaction temperature of 150 °C for a reaction time of 2 h. After the secondary hydrothermal reaction, filter and separate the secondary filtrate and the secondary precipitate. Wash and dry the secondary precipitate. Washing is performed by washing with distilled water twice. Drying is performed by oven drying at a drying temperature of 100 °C. Combine the primary precipitate and the secondary precipitate after washing and drying to obtain hydroxy copper phosphate laser welding material. Example 4
[0036] (1) Copper sulfate pentahydrate and ammonium dihydrogen phosphate were weighed according to a molar ratio of Cu:P=1:3.5, respectively, and dissolved in deionized water to prepare a saturated solution. The mixture was mixed by magnetic stirring to obtain solution A.
[0037] (2) Slowly add an ammonia solution to the solution A using a peristaltic pump to adjust the pH value of the solution to 4.2. The ammonia solution is added over 30 min to obtain a solution B.
[0038] (3) Solution B was transferred into a polytetrafluoroethylene-lined reactor and placed in a muffle furnace for a hydrothermal reaction at a temperature of 180 °C for 2 h.
[0039] (4) After the first hydrothermal reaction is completed, the reaction mixture is filtered to separate a first filtrate and a first precipitate. The first precipitate is washed and dried. The washing step is performed by washing with distilled water twice. The drying step is performed by drying in an oven at a temperature of 100 °C.
[0040] (5) Add an appropriate amount of ammonium dihydrogen phosphate solution to the primary filtrate, adjust the pH value to 4.2 with an alkaline solution, control the addition of ammonia solution for 30 minutes, transfer it to a reactor lined with polytetrafluoroethylene, and place it in a muffle furnace for a secondary hydrothermal reaction at a reaction temperature of 180 °C for a reaction time of 2 h. After the secondary hydrothermal reaction, filter and separate the secondary filtrate and the secondary precipitate. Wash and dry the secondary precipitate. Washing is performed by washing with distilled water twice. Drying is performed by oven drying at a drying temperature of 100 °C. Combine the primary precipitate and the secondary precipitate after washing and drying to obtain hydroxy copper phosphate laser welding material.
[0041] Comparative Example 1 (1) Copper acetate monohydrate and ammonium dihydrogen phosphate were weighed according to a molar ratio of Cu:P=1:3, and dissolved in deionized water to prepare saturated solutions. The mixture was mixed by magnetic stirring to obtain solution A.
[0042] (2) Slowly add aqueous ammonia solution to the solution A using a peristaltic pump to adjust the pH value of the solution to 5.5 to obtain solution B.
[0043] (3) Solution B was transferred into a polytetrafluoroethylene-lined reactor and placed in a muffle furnace for hydrothermal reaction at a temperature of 180 °C for 2 h.
[0044] (4) After the hydrothermal reaction, the reaction mixture was filtered and the separated precipitate was washed and dried. The washing step was performed by washing with distilled water twice. The drying step was performed by drying in an oven at a temperature of 100 °C to obtain hydroxy copper phosphate laser welding material.
[0045] Comparative Example 2 (1) Copper sulfate pentahydrate and ammonium dihydrogen phosphate were weighed according to a molar ratio of Cu:P=1:1, and dissolved in deionized water to prepare saturated solutions. The mixture was mixed by magnetic stirring to obtain solution A.
[0046] (2) Slowly add an aqueous ammonia solution to the solution A using a peristaltic pump to adjust the pH value of the solution to 6.0 to obtain a solution B.
[0047] (3) Solution B was transferred into a polytetrafluoroethylene-lined reactor and placed in a muffle furnace for hydrothermal reaction at a temperature of 180 °C for 2 h.
[0048] (4) After the hydrothermal reaction, the reaction mixture was filtered and the separated precipitate was washed and dried. The washing step was performed by washing with distilled water twice. The drying step was performed by drying in an oven at a temperature of 100 °C to obtain hydroxy copper phosphate laser welding material.
[0049] Comparative Example 3 Comparative Example 3 is substantially the same as Example 1, but in step (2), the aqueous ammonia solution is added to Solution A while stirring, and the addition is completed within 2 minutes.
[0050] The hydroxy copper phosphate laser welding materials prepared in Example 1, Example 2, Example 3, and Example 4 are marked as Sample 1, Sample 2, Sample 3, and Sample 4, respectively. The hydroxy copper phosphate laser welding materials prepared in Comparative Example 1, Comparative Example 2, and Comparative Example 3 are marked as Sample 5, Sample 6, and Sample 7, respectively. XRD detection is performed, and the obtained XRD spectrum of hydroxy copper phosphate is as follows: Figure 1 As shown, samples 1-7 are all pure phase copper hydroxyphosphate.
[0051] Take sample 1 and scan it with a scanning electron microscope. The SEM spectrum of hydroxy copper phosphate is as follows: Figure 2 As shown, the sample morphology is small prisms with smooth surfaces, one end of the small prisms are linked together, and the other end is blooming in a flower shape. The particle size of the small prisms is about 2-4 μm long and about 0.5-1 μm in diameter.
[0052] The thermogravimetric spectra of sample 1 and commercially available copper hydroxyphosphate laser welding materials were compared at 50-680 °C (air atmosphere, heating rate of 10 °C / min). Figure 3 As shown, sample 1 starts to lose weight at 550°C and loses 3% at 680°C; the commercial product starts to lose weight at 200°C and loses 25% at 680°C. Obviously, the product prepared in Example 1 has better thermal stability.
[0053] Figure 4 is a comparison of the particle size distribution of sample 7 and sample 1. Figure 4 It can be seen that the particle size distribution of sample 1 prepared by slowly adding ammonia water in Example 1 is more concentrated and the particle size is smaller.
[0054] Figure 5 are photos of the appearance of the samples, from left to right are photos of the commercially available product, sample 1, sample 2, sample 5, and sample 6. By comparison, it can be seen that the samples 1 and 2 prepared in Example 1 and Example 2 are lighter in color. When laser welding is performed, light-colored additives can be better used in the welding of white or transparent plastics to minimize the impact on the appearance of the plastic products.
[0055] Figure 6 is the color comparison of the primary filtrate and the secondary filtrate in Example 3, Figure 6 It can be seen that after the first hydrothermal reaction, a large amount of copper ions still remain in the filtrate. After the second hydrothermal reaction, the copper ions have basically reacted with phosphate and combined with Figure 1 The XRD test results of sample 3 indicate that hydroxy copper phosphate can continue to be produced by continuing to add soluble phosphate to the reaction.
Claims
1. A method for preparing a light-colored copper hydroxyphosphate laser welding material, characterized in that: An excess soluble phosphate solution is mixed with a soluble copper salt solution, the pH is adjusted to 4.2-4.8, a hydrothermal reaction is carried out, and after the reaction, a filtrate and a precipitate are separated, and the precipitate is washed and dried to obtain a hydroxy copper phosphate laser welding material.
2. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 1, characterized in that The following steps are involved: (1) Weigh a soluble copper salt and a soluble phosphate according to a molar ratio of Cu:P=1:1-3.5, dissolve them in deionized water, and mix them to obtain solution A; (2) slowly adding an alkaline solution to the solution A to adjust the pH value of the solution to 4.2-4.8, to obtain a solution B; (3) Transfer solution B into a polytetrafluoroethylene-lined reactor and conduct a hydrothermal reaction at a temperature of 120-180 °C for a reaction time of 2-6 h; (4) After the primary hydrothermal reaction is completed, the reaction is filtered to separate the primary filtrate and the primary precipitate, and the primary precipitate is washed and dried to obtain the hydroxy copper phosphate laser welding material.
3. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 1 or 2, characterized in that: During the primary hydrothermal reaction, the soluble phosphate solution and the soluble copper salt solution used are both saturated solutions.
4. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 2, characterized in that: The method further comprises step (5), wherein the step (5) is specifically as follows: adding a phosphate solution to the primary filtrate, adjusting the pH value to 4.2-4.8 with an alkaline solution, transferring the filtrate into a reactor lined with polytetrafluoroethylene, and performing a secondary hydrothermal reaction at a reaction temperature of 120-180°C for a reaction time of 2-6 h; filtering after the secondary hydrothermal reaction to separate a secondary filtrate and a secondary precipitate; washing and drying the secondary precipitate to obtain a hydroxy copper phosphate laser welding material.
5. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 2, characterized in that: In step (2), the alkaline solution is aqueous ammonia.
6. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 4, characterized in that: In step (5), the alkaline solution is aqueous ammonia.
7. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 2, characterized in that: In step (2), the alkaline solution is slowly added by a peristaltic pump, and the addition is completed within 25-35 minutes.
8. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 4, characterized in that: In step (5), the alkaline solution is slowly added by a peristaltic pump, and the addition is completed within 25-35 minutes.
9. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 2, characterized in that: In step (4), drying is carried out in an oven at a temperature of 80-100°C.
10. The method for preparing the light-colored copper hydroxyphosphate laser welding material according to claim 4, characterized in that: In step (5), drying is carried out in an oven at a temperature of 80-100°C.