Alkyl geopolymer antifouling material and preparation method thereof

The alkyl polymer material modified by sodium methyl silicate combines nano-scale materials and antibacterial peptides to form an antifouling coating with superhydrophobic properties and inhibits microbial growth, solving the hydrophobicity of antifouling coatings in building structures in marine environments The problem of insufficient properties and anti-biological adhesion ability has achieved efficient and environmentally friendly anti-fouling effect.

CN119019118AInactive Publication Date: 2024-11-26ZHEJIANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310591581.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has insufficient hydrophobicity and anti-biological adhesion ability of antifouling coatings in the protection of military underwater building structures in marine environments, and traditional methods have a great impact on the marine environment and are difficult to use for a long time.

Method used

Using sodium methyl silicate modified alkyl polymer materials, combined with silicon-aluminum gel and nanoscale materials through chemical grafting and bonding of organic groups, to form an antifouling coating with superhydrophobicity and inhibition of microbial growth. , and use antimicrobial peptides and zeolite imidazole ester skeletons (ZIFs) to enhance antifouling performance.

Benefits of technology

It realizes low surface tension and low elastic modulus of the material surface, significantly improves antifouling performance and durability, reduces the water absorption and corrosion risks of the material, is suitable for antifouling coatings in marine engineering structures, and has an environmentally friendly and low production process. pollute.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004245699250000121
    Figure BDA0004245699250000121
Patent Text Reader

Abstract

The invention discloses an alkyl geopolymer antifouling material, which is prepared from the following raw materials in parts by weight: 55 to 60 parts of silicon-aluminum mineral raw materials, 10 to 15 parts of sodium hydroxide solid, 120 to 125 parts of silicate solution, 5 to 10 parts of methyl sodium silicate, 10 to 15 parts of nano titanium dioxide hydrosol, 5 to 10 parts of nano silicon dioxide aerogel, 10 to 15 parts of antibacterial peptide and 5 to 7 parts of semiconductor metal oxide. The water-based paint is prepared from the following components in parts by weight: 5-10 parts of a silane coupling agent, 5-10 parts of a zeolite imidazate framework, 20-25 parts of hydrophobic metakaolin particles, 5-6 parts of an additive, 15-20 parts of deionized water and 1-2 parts of a grinding aid. The invention also discloses a preparation method of the alkyl geopolymer antifouling material. When the geopolymer is prepared, an organic methyl sodium silicate solution is added into an alkali activator, and organic functional groups are combined into a matrix through chemical and physical technologies to generate an organic geopolymer material with antifouling property; through cooperation of the sodium methyl silicate and the silane coupling agent, an organic matrix-silane coupling agent-inorganic matrix bonding layer is formed between the interfaces of the organic material and the inorganic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials and relates to a novel geopolymer material, in particular to an organic antifouling geopolymer material and a preparation method thereof. Background Art

[0002] Military underwater structures under marine environmental conditions are different from structures on the water. They are often eroded by salt, marine organisms, and continuous dry / wet alternating environments. Building structures that are in high humidity and high salt environments for a long time are very prone to corrosion and are easily fouled by marine organisms, which directly affects the safety of the building structures and significantly reduces their durability. At the same time, it also brings a heavy burden to maintenance work and generates expensive maintenance costs. The corrosion environment of military building structures in the marine environment is harsh and complex. The prevention of biofouling in military buildings is not only about eliminating fouling during the maintenance and repair stages, but also not a simple defouling or insignificant issue. It requires in-depth research on the characteristics of the corrosion environment of my country's military underwater building structures, creating antifouling technology suitable for underwater military structures, and ensuring that my country's antifouling control technology reaches the international advanced level.

[0003] Seawater itself is a highly corrosive medium. Waves, tides, currents will produce low-frequency reciprocating forces and impacts on metal components. In addition, marine microorganisms, attached organisms and biological metabolites will also directly or indirectly accelerate the corrosion process. Marine microorganisms in seawater attach to the surface of underwater structures to produce marine biofouling. The impact of biofouling on safety is mainly reflected in the biocorrosion of metals and concrete, because the polluting organisms will secrete biological acids and deteriorate the materials. Biocorrosion will affect the normal operation of military underwater structures and shorten their service life. Military docks, military tidal power stations and offshore oil exploration platforms may be damaged by biocorrosion. In short, biofouling will lead to the destruction of military building structures and increase the risk of safety accidents. Therefore, inhibiting the attachment of microorganisms and reducing marine biofouling will play a key role in the healthy development of marine military.

[0004] Currently, there are three main methods of protection against marine biofouling: the first is physical cleaning, which uses professional instruments and equipment to scrape off attached microorganisms, such as ionizing radiation, microwave elimination, mechanical elimination, etc., but this method requires complex equipment and cumbersome maintenance, which limits its further application; the second is chemical cleaning, which is a more widely used anti-fouling method, but the chemical substances released by this method usually have adverse effects on the surrounding environment and are not conducive to the sustainable development of marine ecology; the third is self-cleaning material anti-fouling method, that is, by improving the performance of materials, a series of environmentally friendly anti-fouling technologies or materials are developed.

[0005] At present, antifouling coatings are the most widely used method, because they are not only an effective measure to prevent marine organisms from attaching and growing on metal components and preventing corrosion on the surface of metal components, but also have the advantages of high efficiency, low cost, and easy maintenance. Traditional organic antifouling coatings are expensive, highly volatile, and even toxic. Long-term use is bound to have adverse effects on marine organisms and the marine environment.

[0006] The Chinese patent application number CN201810204800.3 is "A photocatalytic self-cleaning cement material, its preparation method and application". This invention adds semiconductor metal oxide components to the photocatalytic self-cleaning cement material to give the cement-based material excellent photocatalytic properties. It can be used to degrade organic pollutants in water bodies and nitrogen oxides, sulfides, etc. in the atmosphere, but its ability to prevent metal structures from being corroded by the marine environment is relatively low.

[0007] The Chinese patent application number CN202210381699.5, "A side-chain polydimethylsiloxane-based polyurethane and its preparation method and use", relates to a side-chain polydimethylsiloxane-based polyurethane and its preparation method and use. The side-chain polydimethylsiloxane-based polyurethane provided by the invention can be used to prepare a solid ultra-slip surface antifouling coating with surface lubrication and high stability. The side-chain polydimethylsiloxane grafted by chemical bonds can give the coating a longer-lasting performance in preventing and controlling marine biofouling, but its antifouling ability is poor and the antifouling rate is not high.

[0008] The Chinese patent application number CN202210278669.1, "Mucus-secreting organosilicon marine antifouling coating and its preparation method", relates to a mucus-secreting organosilicon marine antifouling coating and its preparation method. The hydrogen bonding between the special molecular structure of the synthetic modified polysiloxane resin side chains ensures a firm bond between the coating and the substrate such as the ship, and can drive the directional migration and release of the bionic mucus. The coating overcomes the disadvantage of poor adhesion between the traditional organosilicon marine antifouling coating and the substrate, but the coating surface has poor anti-biological adhesion ability.

[0009] In view of the defects of the existing antifouling coating, the present invention provides a bionic geopolymer antifouling material with super hydrophobicity and microbial growth inhibition ability that can be applied in the marine environment and a preparation method thereof. Ordinary geopolymer materials are not only hydrophobic due to the chemical composition of the material surface, but also have a rich microporous structure and a lot of water transmission channels and water storage spaces inside the material, which do not constitute the conditions for being an antifouling coating. However, the present invention modifies ordinary geopolymers with sodium methyl silicate, adopts a preparation mechanism combining organic materials and inorganic materials, and forms a new type of alkyl geopolymer material through new chemical grafting and bonding of organic groups (alkyl groups), effectively changing the inherent pore structure and wettability of the geopolymer material, so that it has both the mechanical strength of inorganic materials and the chemical properties of organic materials, achieving both hydrophobicity and microbial growth inhibition on the material surface, and blocking water transmission and inhibiting water absorption inside the material. The antifouling coating prepared by the material has low surface tension and low elastic modulus, so that a low-energy surface can be achieved, and fouling organisms can hardly adhere to the surface of the antifouling coating. Even if they adhere, they are easily removed due to weak adhesion. The antifouling geopolymer material modified by sodium methyl silicate overcomes the technical defect that the antifouling grade of general organic materials does not meet the requirements due to its stable physical and chemical properties and good antifouling performance. It can be used to prepare bionic non-smooth antifouling coatings with super hydrophobic stability, and is expected to become a new direction for the future development of building antifouling materials. Summary of the invention

[0010] In order to overcome the shortcomings of the prior art, the present invention provides an alkyl geopolymer antifouling material and a preparation method thereof, which combines an organic group (alkyl) on a silica-alumina gel by chemical grafting and bonding through a geopolymer reaction, so that the alkyl geopolymer has better hydrophobicity, higher mechanical strength, stronger durability and better antifouling performance. The alkyl geopolymer can be used to prepare an antifouling coating for marine engineering structures to resist erosion and damage to ships and underwater structures by the marine environment. At the same time, the preparation method thereof is relatively easy, has lower pollution to the environment, and is green and environmentally friendly.

[0011] The technical solution adopted by the present invention to solve the technical problem is: an alkyl geopolymer antifouling material comprises the following raw materials in parts by weight: 55-60 parts of silicoaluminous mineral raw materials, 10-15 parts of sodium hydroxide solid, 120-125 parts of silicate solution, 5-10 parts of sodium methyl silicate, 10-15 parts of nano titanium dioxide (TiO2) hydrosol, 5-10 parts of nano silicon dioxide (SiO2) aerogel, 10-15 parts of antimicrobial peptides, 5-7 parts of semiconductor metal oxides, 5-10 parts of silane coupling agents, 5-10 parts of zeolite imidazolate frameworks (ZIF), 20-25 parts of hydrophobic metakaolin particles, 5-6 parts of additives, 15-20 parts of deionized water and 1-2 parts of grinding aids.

[0012] Preferably, the silica-alumina mineral raw material is a composite material, which includes 15-30 parts of metakaolin, 10-20 parts of silica fume, and 25-35 parts of fly ash.

[0013] Preferably, the sodium hydroxide solid includes but is not limited to blocks, flakes, powder and the like, and has a purity greater than 95%.

[0014] Preferably, the silicate solution is silicate solid and the water content of the solution is 50-70%.

[0015] Preferably, the particle size of the sodium methyl silicate is maintained in the range of 20-100 nanometers, and the purity is greater than 99%.

[0016] Preferably, the particle size of the nano-TiO2 powder is maintained in the range of 10-50 nanometers, and the purity is greater than 98%.

[0017] Preferably, the nano-TiO2 hydrosol is composed of nano-TiO2 particles, glyoxylic acid or pyruvic acid, a surfactant, a bactericide and deionized water. The particle size of the nano-TiO2 powder is maintained in the range of 10-50 nanometers, and the purity is greater than 98%.

[0018] Preferably, the antimicrobial peptide is added in powder form.

[0019] Preferably, the nano-SiO2 aerogel composite material is composed of nano-SiO2 aerogel particles, fibers and adhesives; the dry density of the nano-SiO2 aerogel composite material is 0.1-0.25 g / cm 3 The volume percentage of the nano-SiO2 aerogel particles is 20%-50%.

[0020] Preferably, the fiber is composed of polyvinyl alcohol fiber, silica glass fiber, silicon carbide fiber and steel fiber, the volume ratio of the four fibers is 3:3:3:1, the average diameter is maintained in the range of 20-70 microns, the length is maintained in the range of 5.0mm-10.0mm, and the apparent density is 110-140kg / m 3 .

[0021] Preferably, the semiconductor metal oxide includes but is not limited to NiO, CoO, FeO and the like.

[0022] Preferably, the hydrophobic metakaolin particles are produced by mixing 100-120 g of dried metakaolin, 5-10 g of siloxane, 180-200 ml of ethanol, 5-10 ml of ammonia (AR, 25%) and 40-60 ml of deionized water, stirring the mixture magnetically at 500-600 rpm for 8-12 hours, and placing it in a vacuum drying oven set at 55-60° C. to remove any residual solvent. The functionalized particles are dried at 100-110° C. for another 10-12 hours and then stored in a desiccator, wherein the drying temperature of the metakaolin is 100-105° C. and the drying time is 36-48 hours.

[0023] Preferably, the angle of T-imidazole-T in the zeolite imidazolate framework (ZIF) is 145°.

[0024] Preferably, the admixture is composed of the following components in weight percentage: waterproofing agent 75-85%, water reducing agent 8-10%, retarder 6-15%, and water retaining agent 0-1%.

[0025] The present invention also discloses a method for preparing an alkyl geopolymer antifouling material, comprising the following steps:

[0026] 1) Preparation of alkaline activator: 10-15 parts of sodium hydroxide solid and 120-125 parts of silicate solution are mixed and stirred until the mixture is uniform and clear and the total water content reaches 35-45%, and then the mixture is poured into a plastic container and sealed for 20-24 hours to obtain an alkaline activator;

[0027] 2) Preparation of sodium methyl silicate-alkali activator solution: 5-10 parts of sodium methyl silicate and the alkali activator obtained in step 1) are mixed, and ultrasonically dispersed at 50-60 Hz for 70-90 minutes to obtain a sodium methyl silicate-alkali activator solution;

[0028] 3) Preparation of solid raw materials: 55-60 parts of silica-alumina mineral raw materials, 20-25 parts of hydrophobic metakaolin particles, 10-15 parts of antimicrobial peptides, 5-10 parts of zeolite imidazolate framework (ZIF), 5-7 parts of semiconductor metal oxides and 1-2 parts of grinding aids are mixed and stirred and ground for 50-70 minutes to obtain a solid raw material;

[0029] 4) Preparation of additive solution: 10-15 parts of nano-TiO2 hydrosol, 5-10 parts of nano-SiO2 aerogel, 5-10 parts of silane coupling agent, 15-20 parts of deionized water, and 5-6 parts of additive are mixed and dispersed by 60-70 Hz ultrasonic dispersion for 60-90 minutes to obtain an additive solution;

[0030] 5) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 800-1000 rpm for 30-40 minutes to obtain an organic antifouling geopolymer material;

[0031] 6) Pour the alkyl geopolymer slurry obtained in step 4) into a mold for curing, first in an oven or vacuum drying oven at 40-60 degrees Celsius for 24-48 hours, and then naturally cure at room temperature for 3-28 days after demolding to obtain the finished product.

[0032] In the present invention, sodium methyl silicate participates in the chemical reaction as a part of the alkali activator, and is combined with the silica-alumina gel in the form of chemical grafting and bonding through processes such as hydrolysis, polymerization, and recombination. The organic silicon in the sodium methyl silicate replaces the inorganic silicon in the inorganic metakaolin and inorganic water glass, and the organic methyl group hydrophobically modifies the fiber in the nano-TiO2 hydrosol. The creative combination of sodium methyl silicate and the silane coupling agent forms a bonding layer of an organic matrix-silane coupling agent-inorganic matrix between the interface of the organic material and the inorganic material, and the combination of the nano-scale material changes the pore structure and wettability inside the material, thereby inhibiting the water absorption and transmission of the material, and improving the durability and super-hydrophobicity of the material. The silica-alumina mineral raw material and the alkali activator are mixed in an ideal ratio to prepare a material with a high degree of polymerization, a high matrix density, and a high mechanical strength. The mixing of metakaolin, fly ash and silica fume as the main raw materials is conducive to filling the pores of the material and reducing the porosity of the macropores of the material; in addition to the filling effect, silica fume can also improve the fluidity of the slurry and promote the dispersion and mutual reaction of solid raw materials. Hydrophobic metakaolin particles can provide electrostatic force or spatial repulsion to increase the viscosity and superhydrophobicity of the material. In addition, hydrophobic particles can also increase the tortuosity and average path of water migration inside the material, and can even cut off the water transmission path of the capillary, so that the material can have fewer water absorption channels to retain moisture, which can reduce the water absorption of the material. ZIF and nano-scale materials work together to achieve high antifouling properties by changing the size of the surface texture on the material surface, and produce excellent air interception capacity at the interface surface grooves along the direction of the building composite material blocks, thereby optimizing the long-term durability of the antifouling coating surface. High anti-seepage properties are achieved by improving the bonding strength of the composite structural units of the material inside the material. Stable nano-TiO2 hydrosol can be mixed into water like a water reducer, fully reacting and blending with geopolymer materials. It has a large specific surface area and high photocatalytic performance, and can work in synergy with the photocatalytic performance of semiconductor metal oxides to exert better bactericidal performance and reduce microbial attachment. Antimicrobial peptides achieve antifouling effects by inhibiting bacterial attachment and biofilm formation through charge action. TiO2 hydrosol particles in nano-TiO2 also carry positive charges in the hydrosol. Unlike the agglomeration and surface charge distribution of ordinary TiO2 nanopowders in aqueous solutions, stable nano-TiO2 hydrosols and surface-fixed antimicrobial peptides can cooperate with each other to destroy bacterial microorganisms with different penetration levels, inactivate bacterial proteins, and prevent organisms from attaching.

[0033] The beneficial effects of the present invention are as follows: 1) the present invention innovatively utilizes organic silicate as a part of the alkali activator, and combines the organic functional group in the matrix by chemical grafting and bonding through processes such as hydrolysis, polymerization, and recombination to form an alkyl geopolymer material with antifouling performance; 2) the addition of raw materials, antimicrobial peptides, zeolite imidazole framework (ZIF), semiconductor metal oxides, silane coupling agents, nanomaterials, fibers, etc. makes the material of the present invention have high strength, dense structure, strong durability, good hydrophobicity, and strong antifouling ability, which can meet the performance requirements of the antifouling material; 3) the present invention utilizes waste raw materials such as fly ash, slag, and silica fume, and the product production cycle is short, the process is green and safe, and high temperature and other conditions are not required, which meets the requirements of energy conservation, environmental protection and sustainable development strategies; 4) the present invention can be used as a new type of alkyl geopolymer antifouling coating on metal or concrete surfaces to protect marine ships or underwater structures from seawater corrosion and biological attachment. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0035] Embodiment 1

[0036] An alkyl geopolymer antifouling material is characterized by comprising the following raw materials in parts by weight: 25 parts of metakaolin, 10 parts of silica fume, 25 parts of fly ash, 10 parts of solid sodium hydroxide, 120 parts of silicate solution, 7 parts of sodium methyl silicate, 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 15 parts of antimicrobial peptides, 8 parts of zeolite imidazolate framework (ZIF), 5 parts of semiconductor metal oxide NiO, 5 parts of silane coupling agent, 24 parts of hydrophobic metakaolin particles, 5 parts of admixture, 20 parts of deionized water and 1 part of grinding aid.

[0037] The silicate solution is a mixed solution of silicate solid and deionized water, and its water content is 50%; the particle size of sodium methyl silicate is about 50nm, and the water content of the solution is 70%; the volume percentage of nano-SiO2 aerogel particles is 20%, the volume ratio of the four fibers is 3:3:3:1, the average fiber diameter is 40 microns, and the length is 5 mm; NiO is selected as the semiconductor metal oxide; the admixture is composed of the following components in weight percentage: 75% waterproofing agent, 10% water reducing agent, 14% retarder, and 1% water retaining agent, and existing commonly used reagents are selected without specific limitation.

[0038] The preparation method of the alkyl geopolymer antifouling material comprises the following steps:

[0039] 1) Preparation of alkaline activator: 10 parts of sodium hydroxide solid and 120 parts of silicate solution were mixed and stirred until uniform and clear, and the total water content reached 40%, and then poured into a plastic container and sealed for 20 hours to obtain an alkaline activator;

[0040] 2) Preparation of sodium methyl silicate-alkali activator solution: 7 parts of sodium methyl silicate and the alkali activator obtained in step 1) were mixed, and ultrasonically dispersed at 50 Hz for 80 minutes to obtain a sodium methyl silicate-alkali activator solution;

[0041] 3) Preparation of solid raw materials: 60 parts of silica-alumina mineral raw materials, 24 parts of hydrophobic metakaolin particles, 15 parts of antimicrobial peptides, 8 parts of zeolite imidazolate framework (ZIF), 5 parts of semiconductor metal oxide NiO and 1 part of grinding aid were mixed and stirred and ground for 50 minutes to obtain a solid raw material;

[0042] 4) Preparation of additive solution: 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 5 parts of silane coupling agent, 20 parts of deionized water and 5 parts of additive were mixed and dispersed by 60 Hz ultrasound for 60 minutes to obtain an additive solution.

[0043] 5) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 800 rpm for 40 minutes to obtain an alkyl geopolymer antifouling slurry;

[0044] 6) Pour the alkyl geopolymer slurry obtained in step 5) into a mold for curing, first in an oven or vacuum drying oven at 40 degrees Celsius for 48 hours, and then naturally cure at room temperature for 7 days after demolding to obtain the finished product.

[0045] Embodiment 2

[0046] An alkyl geopolymer antifouling material is characterized by comprising the following raw materials in parts by weight: 20 parts of metakaolin, 10 parts of silica fume, 28 parts of fly ash, 12 parts of solid sodium hydroxide, 125 parts of silicate solution, 8 parts of sodium methyl silicate, 12 parts of nano-TiO2 hydrosol, 8 parts of nano-SiO2 aerogel, 10 parts of antimicrobial peptides, 7 parts of zeolite imidazolate framework (ZIF), 6 parts of semiconductor metal oxide FeO, 8 parts of silane coupling agent, 25 parts of hydrophobic metakaolin particles, 5 parts of admixture, 15 parts of deionized water, and 1 part of grinding aid.

[0047] The water content of the silicate solution is 55%; the particle size of sodium methyl silicate is about 30nm, and the water content of the solution is 75%; the volume percentage of nano-SiO2 aerogel particles is 30%, the volume ratio of the four fibers is 3:3:3:1, the average fiber diameter is 30 microns, and the length is 5 mm; FeO is selected as the semiconductor metal oxide; the admixture is composed of the following components in weight percentage: 80% waterproofing agent, 9% water reducing agent, 10% retarder, and 1% water retaining agent.

[0048] The preparation method of the alkyl geopolymer antifouling material comprises the following steps:

[0049] 1) Preparation of alkaline activator: 12 parts of sodium hydroxide solid and 125 parts of silicate solution were mixed and stirred until uniform and clear, and the total water content reached 40%, and then poured into a plastic container and sealed for 24 hours to obtain an alkaline activator;

[0050] 2) Preparation of sodium methyl silicate-alkali activator solution: sodium methyl silicate and the alkali activator obtained in step 1) are mixed, and ultrasonically dispersed at 55 Hz for 80 minutes to obtain a sodium methyl silicate-alkali activator solution;

[0051] 3) Preparation of solid raw materials: 58 parts of silica-alumina mineral raw materials, 25 parts of hydrophobic metakaolin particles, 10 parts of antimicrobial peptides, 7 parts of zeolite imidazolate framework (ZIF), 6 parts of semiconductor metal oxide FeO and 1 part of grinding aid were mixed and stirred and ground for 60 minutes to obtain a solid raw material;

[0052] 4) Preparation of additive solution: 12 parts of nano-TiO2 hydrosol, 8 parts of nano-SiO2 aerogel, 8 parts of silane coupling agent, 15 parts of deionized water and 5 parts of additive were mixed and dispersed by 60 Hz ultrasound for 70 minutes to obtain an additive solution.

[0053] 5) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 900 rpm for 30 minutes to obtain an alkyl geopolymer antifouling slurry;

[0054] 6) Pour the alkyl geopolymer slurry obtained in step 5) into a mold for curing, first in an oven or vacuum drying oven at 50 degrees Celsius for 36 hours, and then naturally cure at room temperature for 14 days after demolding to obtain the final product.

[0055] Embodiment 3

[0056] An alkyl geopolymer antifouling material is characterized by comprising the following raw materials in parts by weight: 18 parts of metakaolin, 11 parts of silica fume, 26 parts of fly ash, 15 parts of solid sodium hydroxide, 122 parts of silicate solution, 10 parts of sodium methyl silicate, 10 parts of nano-TiO2 hydrosol, 10 parts of nano-SiO2 aerogel, 11 parts of antimicrobial peptides, 5 parts of zeolite imidazolate framework (ZIF), 7 parts of semiconductor metal oxide CoO, 10 parts of silane coupling agent, 20 parts of hydrophobic metakaolin particles, 6 parts of admixture, 17 parts of deionized water and 2 parts of grinding aid.

[0057] The water content of the silicate solution is 70%; the particle size of sodium methyl silicate is about 60nm, and the water content of the solution is 75%; the volume percentage of nano-SiO2 aerogel particles is 30%, the average fiber diameter is 60 microns, and the length is 9 mm; the semiconductor metal oxide is CoO; the admixture is composed of the following components in weight percentage: waterproofing agent 85%, water reducing agent 8%, retarder 6%, and water retaining agent 1%.

[0058] The preparation method of the alkyl geopolymer antifouling material comprises the following steps:

[0059] 1) Preparation of alkaline activator: 15 parts of sodium hydroxide solid and 122 parts of silicate solution were mixed and stirred until uniform and clear, and the total water content reached 45%, and then poured into a plastic container and sealed for 24 hours to obtain an alkaline activator;

[0060] 2) Preparation of sodium methyl silicate-alkali activator solution: sodium methyl silicate and the alkali activator obtained in step 1) are mixed, and ultrasonically dispersed at 60 Hz for 90 minutes to obtain a sodium methyl silicate-alkali activator solution;

[0061] 3) Preparation of solid raw materials: 55 parts of silica-alumina mineral raw materials, 20 parts of hydrophobic metakaolin particles, 11 parts of antimicrobial peptides, 5 parts of zeolite imidazolate framework (ZIF), 7 parts of semiconductor metal oxide CoO and 2 parts of grinding aids were mixed and stirred and ground for 70 minutes to obtain a solid raw material;

[0062] 4) Preparation of additive solution: 10 parts of nano-TiO2 hydrosol, 10 parts of nano-SiO2 aerogel, 10 parts of silane coupling agent, 17 parts of deionized water and 6 parts of additive were mixed and dispersed by 70 Hz ultrasound for 60 minutes to obtain an additive solution.

[0063] 5) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 1000 rpm for 35 minutes to obtain an alkyl geopolymer antifouling slurry;

[0064] 6) Pour the alkyl geopolymer slurry obtained in step 5) into a mold for curing, first in a 60 degree Celsius oven or vacuum drying oven for 24 hours, and then naturally cure at room temperature for 28 days after demoulding to obtain the final product. Comparative Example 4 (without sodium methyl silicate)

[0065] An alkyl geopolymer antifouling material is characterized by comprising the following raw materials in parts by weight: 25 parts of metakaolin, 10 parts of silica fume, 25 parts of fly ash, 10 parts of solid sodium hydroxide, 120 parts of silicate solution, 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 15 parts of antimicrobial peptides, 8 parts of zeolite imidazolate framework (ZIF), 5 parts of semiconductor metal oxide NiO, 5 parts of silane coupling agent, 24 parts of hydrophobic metakaolin particles, 5 parts of admixture, 20 parts of deionized water and 1 part of grinding aid.

[0066] The water content of the silicate solution is 50%; the volume percentage of the nano-SiO2 aerogel particles is 20%, the volume ratio of the four fibers is 3:3:3:1, the average fiber diameter is 40 microns, and the length is 5 mm; NiO is selected as the semiconductor metal oxide; the admixture is composed of the following components in weight percentage: 75% waterproofing agent, 10% water reducing agent, 14% retarder, and 1% water retaining agent.

[0067] The preparation method of the alkyl geopolymer antifouling material comprises the following steps:

[0068] 1) Preparation of alkaline activator: 10 parts of sodium hydroxide solid and 120 parts of silicate solution were mixed and stirred until uniform and clear, and the total water content reached 40%, and then poured into a plastic container and sealed for 20 hours to obtain an alkaline activator;

[0069] 2) Preparation of solid raw materials: 60 parts of silica-alumina mineral raw materials, 24 parts of hydrophobic metakaolin particles, 15 parts of antimicrobial peptides, 8 parts of zeolite imidazolate framework (ZIF), 5 parts of semiconductor metal oxide NiO and 1 part of grinding aid were mixed and stirred and ground for 50 minutes to obtain a solid raw material;

[0070] 3) Preparation of additive solution: 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 5 parts of silane coupling agent, 20 parts of deionized water and 5 parts of additive were mixed and dispersed by 60 Hz ultrasound for 60 minutes to obtain an additive solution.

[0071] 4) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 800 rpm for 40 minutes to obtain an alkyl geopolymer antifouling slurry;

[0072] 5) Pour the alkyl geopolymer slurry obtained in step 5) into a mold for curing, first in an oven or vacuum drying oven at 40 degrees Celsius for 48 hours, and then naturally cure at room temperature for 7 days after demoulding to obtain the finished product.

[0073] Comparative Example 5 (without antimicrobial peptide)

[0074] An alkyl geopolymer antifouling material is characterized by comprising the following raw materials in parts by weight: 25 parts of metakaolin, 10 parts of silica fume, 25 parts of fly ash, 10 parts of solid sodium hydroxide, 120 parts of silicate solution, 7 parts of sodium methyl silicate, 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 8 parts of zeolite imidazolate framework (ZIF), 5 parts of semiconductor metal oxide NiO, 5 parts of silane coupling agent, 24 parts of hydrophobic metakaolin particles, 5 parts of additive, 20 parts of deionized water and 1 part of grinding aid.

[0075] The water content of the silicate solution is 50%; the particle size of sodium methyl silicate is about 50nm, and the water content of the solution is 70%; the volume percentage of nano-SiO2 aerogel particles is 20%, the volume ratio of the four fibers is 3:3:3:1, the average fiber diameter is 40 microns, and the length is 5 mm; NiO is selected as the semiconductor metal oxide; the admixture is composed of the following components in weight percentage: waterproofing agent 75%, water reducing agent 10%, retarder 14%, and water retaining agent 1%.

[0076] The preparation method of the alkyl geopolymer antifouling material comprises the following steps:

[0077] 1) Preparation of alkaline activator: 10 parts of sodium hydroxide solid and 120 parts of silicate solution were mixed and stirred until uniform and clear, and the total water content reached 40%, and then poured into a plastic container and sealed for 20 hours to obtain an alkaline activator;

[0078] 2) Preparation of sodium methyl silicate-alkali activator solution: 7 parts of sodium methyl silicate and the alkali activator obtained in step 1) were mixed, and ultrasonically dispersed at 50 Hz for 80 minutes to obtain a sodium methyl silicate-alkali activator solution;

[0079] 3) Preparation of solid raw materials: 60 parts of silica-alumina mineral raw materials, 24 parts of hydrophobic metakaolin particles, 8 parts of zeolite imidazolate framework (ZIF), 5 parts of semiconductor metal oxide NiO and 1 part of grinding aid were mixed and stirred and ground for 50 minutes to obtain a solid raw material;

[0080] 4) Preparation of additive solution: 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 5 parts of silane coupling agent, 20 parts of deionized water and 5 parts of additive were mixed and dispersed by 60 Hz ultrasound for 60 minutes to obtain an additive solution.

[0081] 5) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 800 rpm for 40 minutes to obtain an alkyl geopolymer antifouling slurry;

[0082] 6) Pour the alkyl geopolymer slurry obtained in step 5) into a mold for curing, first in an oven or vacuum drying oven at 40 degrees Celsius for 48 hours, and then naturally cure at room temperature for 7 days after demolding to obtain the finished product.

[0083] Comparative Example 6 (without ZIF)

[0084] An alkyl geopolymer antifouling material is characterized by comprising the following raw materials in parts by weight: 25 parts of metakaolin, 10 parts of silica fume, 25 parts of fly ash, 10 parts of solid sodium hydroxide, 120 parts of silicate solution, 7 parts of methyl sodium silicate, 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 15 parts of antimicrobial peptides, 5 parts of semiconductor metal oxide NiO, 5 parts of silane coupling agent, 24 parts of hydrophobic metakaolin particles, 5 parts of admixture, 20 parts of deionized water and 1 part of grinding aid.

[0085] The water content of the silicate solution is 50%; the particle size of sodium methyl silicate is about 50nm, and the water content of the solution is 70%; the volume percentage of nano-SiO2 aerogel particles is 20%, the volume ratio of the four fibers is 3:3:3:1, the average fiber diameter is 40 microns, and the length is 5 mm; NiO is selected as the semiconductor metal oxide; the admixture is composed of the following components in weight percentage: waterproofing agent 75%, water reducing agent 10%, retarder 14%, and water retaining agent 1%.

[0086] The preparation method of the alkyl geopolymer antifouling material comprises the following steps:

[0087] 1) Preparation of alkaline activator: 10 parts of sodium hydroxide solid and 120 parts of silicate solution were mixed and stirred until uniform and clear, and the total water content reached 40%, and then poured into a plastic container and sealed for 20 hours to obtain an alkaline activator;

[0088] 2) Preparation of sodium methyl silicate-alkali activator solution: 7 parts of sodium methyl silicate and the alkali activator obtained in step 1) were mixed, and ultrasonically dispersed at 50 Hz for 80 minutes to obtain a sodium methyl silicate-alkali activator solution;

[0089] 3) Preparation of solid raw materials: 60 parts of silica-alumina mineral raw materials, 24 parts of hydrophobic metakaolin particles, 15 parts of antimicrobial peptides, 5 parts of semiconductor metal oxide NiO and 1 part of grinding aid were mixed and stirred and ground for 50 minutes to obtain a solid raw material;

[0090] 4) Preparation of additive solution: 15 parts of nano-TiO2 hydrosol, 5 parts of nano-SiO2 aerogel, 5 parts of silane coupling agent, 20 parts of deionized water and 5 parts of additive were mixed and dispersed by 60 Hz ultrasound for 60 minutes to obtain an additive solution.

[0091] 5) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 800 rpm for 40 minutes to obtain an alkyl geopolymer antifouling slurry;

[0092] 6) Pour the alkyl geopolymer slurry obtained in step 5) into a mold for curing, first in an oven or vacuum drying oven at 40 degrees Celsius for 48 hours, and then naturally cure at room temperature for 7 days after demolding to obtain the finished product.

[0093] In order to verify the mechanical properties and corrosion resistance of the alkyl geopolymer antifouling self-cleaning material of the present invention, carbon black ash collection experiment, viscosity test, contact angle test, water absorption and anti-seepage test were carried out. The specific methods and results are as follows:

[0094] (1) Carbon black dust collection test: Spread carbon black evenly on the test surface, tilt the surface at 45 degrees, use a sampler to suck 0.3mL of distilled water and drop it on the upper end of the test surface, a total of 5 points, and conduct a dust collection test. On the surface of a non-self-cleaning coating, water droplets will spread and cannot take away the carbon black powder; on the surface of a self-cleaning coating, water droplets are spherical and easy to roll down, and can take away all the carbon black powder on the track. Whether the material is qualified for hydrophobicity and antifouling is determined based on whether more than 98% of the carbon black powder is taken away.

[0095] (2) Chlorella staining test: Artificial seawater (ASW) free of heavy metals was prepared according to ASTM D1141-98 (2013), and Chlorella (95 wt%, Anhui Zisheng Technology Co., Ltd.) was selected to evaluate the corrosion resistance of the material surface. The surface was vertically immersed in the Chlorella solution, incubated for 2 h, given sufficient light, incubated at room temperature for 1 week, and taken out for use. After cleaning the surface with distilled water, 4 observation points were randomly selected on different surfaces for quantitative counting under an optical microscope. All flushing tests were performed four times.

[0096] (3) Viscosity test: The alkyl geopolymer antifouling self-cleaning materials prepared in the examples and comparative examples were taken as test samples, and the viscosity of the slurry just after mixing was measured by a NDJ-8S digital viscosity tester.

[0097] (4) Contact angle test: The alkyl geopolymer antifouling self-cleaning materials prepared in the examples and comparative examples were taken as test samples, dried naturally and then cut open, and their surface and internal hydrophobic and oleophobic contact angles were tested respectively.

[0098] (5) Anti-seepage test: The alkyl geopolymer anti-fouling self-cleaning materials prepared in the examples and comparative examples were taken as samples. According to T0568-2005 "Test Method for Anti-seepage Performance of Cement Concrete", the samples were placed on a permeameter. The water pressure was increased by 0.1 MPa every 8 hours from 0.1 MPa until water seepage was found on the surface of 3 out of 6 test pieces. The water pressure at this time was recorded and the test was stopped. When the pressure was increased to the designed anti-seepage grade and the third test piece still did not seep water after 8 hours, it indicated that the concrete had met the design requirements and the test was stopped.

[0099] (6) Antibacterial test: Artificial seawater (ASW) was prepared according to the requirements of ASTM D1141-98, and Staphylococcus aureus was selected as a typical marine organism for adhesion test. The strain was cultured in sterile 2216E medium (1 g yeast extract and 5 g fish meal peptone dissolved in 1 L ASW). The bacteria used for adhesion determination were in the exponential growth phase. The bacterial concentration was adjusted to approximately 1×10 6 CFU / mL, the samples were immersed in the two bacterial solutions respectively and incubated at 37°C and 80rpm shaking. After incubation for 24h, the samples were washed three times with sterile ASW to remove any non-adherent or loosely adherent bacteria. Some samples were immersed in glutaraldehyde (2.5%) at 4°C for 2h, dehydrated with 25%, 50%, 75%, 90%, and 100% ethanol solutions (10min / concentration) in sequence, and then the bacteria were characterized by SEM. Other samples were immersed in PI solution (50μg / mL, PI dissolved in ASW) for 30 minutes at room temperature in the dark. The samples were cleaned with sterile ASW to remove the dye, and the attached bacteria were imaged by CLSM. ImageJ software was used for statistical analysis of bacterial adhesion on stainless steel. The coverage of bacteria is the percentage of adhesion, defined as: percentage of adhesion = bacterial adhesion area / total area of ​​the field of view × 100%. After importing the image, adjust the threshold using the "Image-Adjust-Threshold" procedure so that all attached bacteria appear red (the same threshold range must be selected when analyzing different samples). Then, apply the ImageJ math function "Analyze-Analyzeparticles" to the thresholded image, and the adhesion percentage result can be obtained from the "summary".

[0100] Table 1: Test results of alkyl geopolymer antifouling self-cleaning surface coating

[0101]

[0102] The test results of Experimental Examples 1, 2 and 3 show that as an alkyl geopolymer antifouling material, its viscosity is greater than 12500 mPa·s. This material has qualified hydrophobic antifouling ability under the joint action of composite raw materials, nano TiO2 hydrosol, nano SiO2 aerogel, semiconductor metal oxide, hydrophobic metakaolin particles, antimicrobial peptides, ZIF, silane coupling agents and other materials. The surface of this material is hydrophobic, and the contact angle of the experimental water drop surface is greater than 150°, the internal contact angle is greater than 140°, and the rolling angle is greater than 6.5°. The carbon black ash collection experiment and the bacterial test can well illustrate that the material has achieved good hydrophobic modification from the matrix under the action of sodium methyl silicate, in the fusion of organic and inorganic hybridization, and under the coordinated action of antimicrobial peptides and ZIF, and has formed excellent antifouling properties from the surface, indicating that the material can be prepared into an antifouling coating for the anticorrosion and anti-biological attachment of hydraulic structures in marine environments.

[0103] The test results of comparative example 4 show that for the geopolymer material without the addition of sodium methyl silicate, its hydrophobicity is significantly reduced, and the bacterial adhesion rate in the bacterial experiment and the number of bacteria adhered in the Chlorella staining test are both high, indicating that the geopolymer material without the addition of sodium methyl silicate does not meet the conditions for becoming an antifouling coating.

[0104] The test results of comparative example 5 show that for the alkyl geopolymer without adding antimicrobial peptides, the hydrophobic antifouling ability of its surface does not meet the requirements, and the bacterial adhesion rate in the bacterial experiment and the number of bacterial adhesion in the Chlorella staining test are slightly increased, indicating that the geopolymer material without adding antimicrobial peptides does not meet the conditions for becoming an antifouling coating.

[0105] The test results of comparative example 6 show that, for the alkyl geopolymer without adding ZIF, the hydrophobicity of its surface meets the requirements of hydrophobicity of the antifouling coating, but the bacterial experiment and the Chlorella staining test show that the material does not meet the requirements of antibacterial property of the antifouling coating, indicating that the geopolymer material without adding ZIF does not meet the conditions for becoming an antifouling coating.

[0106] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An alkyl geopolymer antifouling material, characterized in that The invention comprises the following raw materials in parts by weight: 55-60 parts of silicoaluminate mineral raw materials, 10-15 parts of sodium hydroxide solid, 120-125 parts of silicate solution, 5-10 parts of sodium methyl silicate, 10-15 parts of nano titanium dioxide hydrosol, 5-10 parts of nano silicon dioxide aerogel, 10-15 parts of antimicrobial peptides, 5-7 parts of semiconductor metal oxides, 5-10 parts of silane coupling agents, 5-10 parts of zeolite imidazole ester skeletons, 20-25 parts of hydrophobic metakaolin particles, 5-6 parts of additives, 15-20 parts of deionized water and 1-2 parts of grinding aids.

2. The alkyl geopolymer antifouling material according to claim 1, characterized in that: The silicon-alumina mineral raw material is a composite material, which includes 15-30 parts of metakaolin, 10-20 parts of silica fume and 25-35 parts of fly ash.

3. The alkyl geopolymer antifouling material according to claim 1, characterized in that: The silicate solution is a mixed solution of silicate solid and deionized water, and the water content of the solution is 50-70%.

4. The alkyl geopolymer antifouling material according to claim 1, characterized in that: The particle size of the sodium methyl silicate is maintained in the range of 20-100 nanometers, and the purity is greater than 99%.

5. The alkyl geopolymer antifouling material according to claim 1, characterized in that: The nano TiO2 hydrosol is composed of nano TiO2 particles, glyoxylic acid or pyruvic acid, surfactant, bactericide and deionized water. The particle size of the nano TiO2 powder is kept in the range of 10-50 nanometers, and the purity is greater than 98%.

6. The alkyl geopolymer antifouling material according to claim 1, characterized in that: The nano-SiO2 aerogel composite material is composed of nano-SiO2 aerogel particles, fibers and adhesives; the dry density of the nano-SiO2 aerogel composite material is 0.1-0.25 g / cm 3 ; The volume percentage of the nano-SiO2 aerogel particles is 20%-50%.

7. The nano-SiO2 aerogel composite material according to claim 6, characterized in that: The fiber is composed of polyvinyl alcohol fiber, silica glass fiber, silicon carbide fiber and steel fiber. The volume ratio of the four fibers is 3:3:3:

1. The average diameter is maintained in the range of 20-70 microns, the length is maintained in the range of 5.0 mm-10.0 mm, and the apparent density is 110-140 kg / m 3 .

8. The alkyl geopolymer antifouling material according to claim 1, characterized in that: The production process of hydrophobic kaolin particles is to mix 100-120g of dried kaolin, 5-10g of siloxane, 180-200ml of ethanol, 5-10ml of ammonia water and 40-60ml of deionized water, stir the mixture magnetically at 500-600rpm for 8-12 hours, place it in a vacuum drying oven set at 55-60°C to remove any residual solvent, and dry the functionalized particles at 100-110°C for another 10-12 hours, and then store them in a desiccator, wherein the drying temperature of the kaolin is 100-105°C and the drying time is 36-48 hours.

9. The alkyl geopolymer antifouling material according to claim 1, characterized in that: The admixture is composed of the following components in percentage by weight: 75-85% of waterproofing agent, 8-10% of water reducing agent, 6-15% of retarder, and 0-1% of water retaining agent.

10. A method for preparing an alkyl geopolymer antifouling material, characterized in that: The following steps are involved: 1) Preparation of alkaline activator: 10-15 parts of sodium hydroxide solid and 120-125 parts of silicate solution are mixed and stirred until the mixture is uniform and clear and the total water content reaches 35-45%, and then the mixture is poured into a plastic container and sealed for 20-24 hours to obtain an alkaline activator; 2) Preparation of sodium methyl silicate-alkali activator solution: 5-10 parts of sodium methyl silicate and the alkali activator obtained in step 1) are mixed, and ultrasonically dispersed at 50-60 Hz for 70-90 minutes to obtain a sodium methyl silicate-alkali activator solution; 3) Preparation of solid raw materials: 55-60 parts of silica-alumina mineral raw materials, 20-25 parts of hydrophobic metakaolin particles, 10-15 parts of antimicrobial peptides, 5-10 parts of zeolite imidazolate frameworks, 5-7 parts of semiconductor metal oxides and 1-2 parts of grinding aids are mixed and stirred and ground for 50-70 minutes to obtain a solid raw material; 4) Preparation of additive solution: 10-15 parts of nano-TiO2 hydrosol, 5-10 parts of nano-SiO2 aerogel, 5-10 parts of silane coupling agent, 15-20 parts of deionized water, and 5-6 parts of additive are mixed and dispersed by 60-70 Hz ultrasonic dispersion for 60-90 minutes to obtain an additive solution; 5) Preparation of alkyl geopolymer slurry: Mix the sodium methyl silicate-alkali activator solution obtained in step 2), the solid raw material obtained in step 3) and the additive solution obtained in step 4), and mechanically stir at a speed of 800-1000 rpm for 30-40 minutes to obtain an organic antifouling geopolymer material; 6) Pour the alkyl geopolymer slurry obtained in step 4) into a mold for curing, first in an oven or vacuum drying oven at 40-60 degrees Celsius for 24-48 hours, and then naturally cure at room temperature for 3-28 days after demolding to obtain the finished product.

Citation Information

Patent Citations

  • Ecological cement high-strength grouting material and preparation method thereof

    CN111807770A

  • Siloxane-modified super-hydrophobic geopolymer anticorrosive material and preparation method thereof

    CN112079593A

  • Gelling activity exciting agent suitable for red mud-based cementing material for traffic engineering