Modified graphene composite sealing agent, preparation method and application thereof, impregnated bond paper and veneer artificial board

Through the use of modified graphene composite sealing agent, combined with the synergistic effect of nanotitanium dioxide and modified graphene, the problem of formaldehyde and VOC gas release in artificial board decoration materials is solved, and efficient sealing and degradation is achieved, achieving environmental protection and excellent performance effect.

CN119019891APending Publication Date: 2024-11-26DONGGUAN BEIHUI DECORATION MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410813765.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art has limited effect in reducing the release of formaldehyde and VOC gas in artificial board decorative materials, and the isolation principle of the sealant is single, making it difficult to effectively improve the isolation rate.

Method used

Modified graphene composite sealing agent is adopted, which is co-doped with chitin, O, N, S, modified graphene, nanotitanium dioxide, polyethylene terephthalate, dicyclohexylmethane diisocyanate and 4 It consists of materials such as -ethyl-4-soybean ethyl sulfate morpholine, prepared by stirring and sonication, forming a sealing agent with high specific surface area and catalytic activity, used to impregnate adhesive film paper and decorative artificial boards.

Benefits of technology

The sealing properties of formaldehyde and VOC gases are significantly improved, and the photocatalytic performance of nanotitanium dioxide and the adsorption performance of modified graphene are achieved efficient degradation and purification, reducing the formaldehyde and VOC release of artificial boards, reaching the E0 standard.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019891A_ABST
    Figure CN119019891A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of environment-friendly decorative materials, and particularly relates to a modified graphene composite sealing agent, a preparation method and application thereof, impregnated bond paper and a veneer artificial board. The invention provides a modified graphene composite sealing agent. The modified graphene composite sealing agent is prepared from the following preparation raw materials in parts by mass: 260 to 520 parts of chitin, 80 to 110 parts of modified graphene, 30 to 60 parts of nano titanium dioxide, 5 to 40 parts of polyethylene glycol terephthalate, 5 to 40 parts of dicyclohexylmethane diisocyanate, 5 to 40 parts of 4-ethyl-4-soybean-based ethyl sulfate morpholine and 500 to 2000 parts of water. The modified graphene is O, N and S co-doped modified graphene; the particle size of the nano titanium dioxide is 5 to 500 nm. The modified graphene composite sealing agent provided by the invention not only has excellent sealing performance on formaldehyde and VOC pollution gas, but also can efficiently degrade formaldehyde and VOC pollution gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmentally friendly decorative materials, and particularly relates to a modified graphene composite sealant, a preparation method and application thereof, impregnated adhesive film paper and a facing artificial board. Background Art

[0002] Formaldehyde is a typical indoor air pollutant, mainly derived from panel furniture and artificial board decorative materials. Long-term exposure to low-concentration formaldehyde environment will pose a great threat to human health. Therefore, reducing the release of formaldehyde in panel furniture and artificial board decorative materials is of great significance to improving indoor air quality. With the strengthening of people's environmental awareness and the improvement of free formaldehyde emission standards for furniture decorative materials in various countries around the world, decorative materials with low formaldehyde and low VOC release are favored by people. How to improve the performance of veneer artificial boards and produce veneer artificial boards with low formaldehyde and low VOC release is the direction that current manufacturers and researchers need to work together.

[0003] The sealant is generally prepared from a film-forming resin, and after being sprayed onto the surface of the board, a closed film is formed to block the release of formaldehyde gas. The Chinese patent with publication number CN110951349A discloses an environmentally friendly board sealant and a preparation method thereof, wherein the environmentally friendly board sealant comprises at least 80 to 100 parts of film-forming agent, 0.2 to 1 part of pH stabilizer, 0.1 to 0.3 parts of emulsifier, and 3 to 10 parts of solvent in parts by weight; the film-forming agent comprises acrylic resin and vinyl acetate-ethylene copolymer. The above-mentioned sealant only isolates the release of formaldehyde through the closed film formed by film formation. It can be seen that the above-mentioned sealant has only a single isolation principle, resulting in the isolation rate of formaldehyde to be further improved. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a modified graphene composite sealant and its preparation method and application, impregnated film paper and veneer artificial board. The modified graphene composite sealant provided by the present invention has excellent sealing performance and can efficiently degrade formaldehyde and VOC gas.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] A modified graphene composite sealant comprises the following raw materials in parts by weight:

[0007] 260-520 parts of chitosan, 80-110 parts of modified graphene, 30-60 parts of nano titanium dioxide, 5-40 parts of polyethylene terephthalate, 5-40 parts of dicyclohexylmethane diisocyanate, 5-40 parts of 4-ethyl-4-soyyl ethyl sulfate morpholine, and 500-2000 parts of water;

[0008] The modified graphene is O, N, S co-doped modified graphene;

[0009] The particle size of the nano titanium dioxide is 5 to 500 nm.

[0010] Preferably, the method for preparing the modified graphene comprises the following steps:

[0011] The aqueous dispersion of graphene is mixed with 1-cysteine ​​and polyethylene glycol to obtain a mixed solution;

[0012] After mixing the mixed solution with isopropanol, adjusting the mixture to be alkaline to obtain a graphene-modified precursor;

[0013] The graphene-modified precursor is irradiated to obtain the modified graphene.

[0014] Preferably, the usage ratio of the graphene aqueous dispersion, 1-cysteine, polyethylene glycol and isopropanol is 100-2000mL: 0.1-2g: 15-300mL: 4-80mL; the concentration of the graphene aqueous dispersion is 0.04-1.0g / L;

[0015] The alkaline pH value is 8 to 10;

[0016] The irradiation dose is 70 to 280 kGy.

[0017] Preferably, the method for preparing nano titanium dioxide comprises the following steps:

[0018] Mix tetrabutyl titanate, anhydrous ethanol and water to obtain solution A;

[0019] The acetic acid aqueous solution is mixed with the A solution and subjected to hydrothermal treatment to obtain the nano titanium dioxide.

[0020] Preferably, the volume concentration of the acetic acid aqueous solution is 0.001% to 28%; the dosage ratio of tetrabutyl titanate, anhydrous ethanol and water in the A solution is 0.1 to 1 mL: 4 to 40 mL: 20 to 68 mL;

[0021] The temperature of the hydrothermal treatment is 150-300° C., and the time is 8-24 hours.

[0022] The present invention provides a method for preparing the modified graphene composite sealing agent, comprising the following steps:

[0023] Chitosan, modified graphene, nano titanium dioxide, polyethylene terephthalate, dicyclohexylmethane diisocyanate, 4-ethyl-4-soyyl ethyl sulfate morpholine and water are mixed, stirred and ultrasonically treated to obtain the modified graphene composite sealing agent.

[0024] Preferably, the stirring speed is 1000-9000 r / min; the ultrasonic power is 2000-8000 W; the stirring and ultrasonic treatment are carried out simultaneously, and the time of the stirring and ultrasonic treatment is 20-240 min.

[0025] The present invention provides the use of the modified graphene composite sealant described in the above technical solution as a coating material.

[0026] The present invention also provides an impregnated film paper, wherein the impregnated film paper is obtained by impregnating a film material in a coating material and drying the film material;

[0027] The membrane material includes one or more of α-cellulose-based modified paper, plastic film and leather;

[0028] The coating material includes a sealant;

[0029] The sealing agent is the modified graphene composite sealing agent described in the above technical solution.

[0030] The present invention also provides a facing artificial board, which comprises a base board, a thin board and facing paper which are stacked in sequence;

[0031] The facing paper is the impregnated adhesive film paper described in the above technical solution.

[0032] The invention provides a modified graphene composite sealing agent, which comprises the following raw materials in parts by mass: 260-520 parts of chitin, 80-110 parts of modified graphene, 30-60 parts of nano titanium dioxide, 5-40 parts of polyethylene terephthalate, 5-40 parts of dicyclohexylmethane diisocyanate, 5-40 parts of 4-ethyl-4-soyyl ethyl sulfate morpholine, and 500-2000 parts of water; the modified graphene is O, N, S co-doped modified graphene; and the particle size of the nano titanium dioxide is 5-500nm.

[0033] In the present invention, nano titanium dioxide has a small particle size and high dispersion, is a full-spectrum absorption titanium dioxide, has higher catalytic activity, and can effectively catalyze and degrade formaldehyde and VOC released in the veneer artificial board. The O, N, and S co-doped modified graphene overcomes the problem of sheet stacking caused by oxidation and interlayer van der Waals force of ordinary graphene. The modified graphene increases the specific surface area and has a strong adsorption performance for formaldehyde and VOC released in the veneer artificial board, and is particularly suitable for decorative material sealants with increasingly stringent environmental protection requirements. Moreover, the electrons of the nano titanium dioxide in the modified graphene composite sealant provided by the present invention penetrate from the metal core to the modified graphene, which can effectively regulate the electron distribution on the graphene surface and its activation ability to oxygen. The synergistic effect of nano titanium dioxide and modified graphene not only improves the photocatalytic performance of titanium dioxide, but also improves the activation adsorption performance of modified graphene to formaldehyde and VOC gases. In the present invention, chitosan has adsorption properties and can be used for formaldehyde and VOC gas purification. Chitosan also has good biocompatibility and natural antibacterial effects, a high spectral antibacterial rate, and can inhibit a variety of bacterial microorganisms. In addition, chitosan has good mechanical strength and is an environmentally friendly material with excellent performance. The modified graphene composite sealant provided by the present invention has excellent sealing performance for formaldehyde and VOC polluted gases and can efficiently degrade formaldehyde and VOC polluted gases. In addition, polyethylene terephthalate is a highly crystalline polymer with a smooth and glossy surface. It has excellent physical and mechanical properties in a wide temperature range. The operating temperature can reach 120°C, and it has good creep resistance, fatigue resistance, friction resistance and dimensional stability. Dicyclohexylmethane diisocyanate is suitable for the production of materials with excellent light stability, weather resistance and mechanical properties. It also has excellent hydrolysis resistance and chemical resistance. It is used in architectural decoration materials such as impregnated film paper and veneer artificial boards to improve the mechanical properties, appearance and service life of the materials. Polyethylene terephthalate and dicyclohexylmethane diisocyanate have good sealing properties after curing into films, which can effectively improve the sealing properties of modified graphene sealants. The 4-ethyl-4-soyyl ethyl sulfate morpholine molecule has a large surface activity and can physically adsorb and wrap odor gas molecules, thereby reducing the concentration of harmful gases in the air and reducing the intensity of the odor. In addition, the sulfate group in the 4-ethyl-4-soyyl ethyl sulfate morpholine molecule has a strong electrophilicity and can effectively remove odors in the air and improve air quality.

[0034] The test results of Tables 1 to 3 of the present invention show that the specific surface area of ​​the modified graphene prepared by the present invention is much larger than the specific surface area of ​​the commercially available ordinary graphene, providing a large number of adsorption centers for the enrichment and catalytic degradation of formaldehyde and VOC volatile organic compounds. The modified graphene composite sealant prepared by Application Example 1 of the present invention using an irradiation dose of 140kGy has the lowest formaldehyde emission of the veneer artificial board; the formaldehyde emission of the veneer artificial board prepared by Application Examples 2 and 3 is equivalent to that of Application Example 1; according to the national standard GB / T 39600-2021 "Grading of Formaldehyde Emission of Artificial Boards and Their Products", the formaldehyde emission of the veneer artificial board prepared by Application Examples 1 to 3 of the present invention is equivalent to E0 grade. The veneer artificial board prepared by the modified graphene composite sealant of the present invention can effectively reduce VOC emission.

[0035] The present invention also provides an impregnated adhesive film paper, which is obtained by impregnating a film material in a coating material and drying it; the film material includes one or more of α-cellulose-based decorative paper, plastic film and leather; the coating material includes a sealant; the sealant is the modified graphene composite sealant described in the above technical solution. The surface of the impregnated adhesive film paper provided by the present invention is coated with a sealant, and a dense film is formed on the surface of the adhesive film paper, which can effectively prevent the volatilization of volatile organic pollutants and has excellent sealing performance. In addition, the impregnated adhesive film paper provided by the present invention has strong adsorption performance and catalytic degradation effect, can effectively absorb and degrade formaldehyde and organic pollutants VOC released by the base board, is a convenient and environmentally friendly decorative material, and has a wide range of application value.

[0036] The present invention also provides a veneer artificial board, the veneer artificial board comprises a base board, a thin board and a veneer paper which are stacked in sequence; the veneer paper is the impregnated film paper described in the above technical solution. In the present invention, the veneer artificial board is covered with impregnated film paper on both sides, which can not only play a sealing role to reduce the release of formaldehyde and VOC, but also effectively absorb and degrade the formaldehyde and VOC harmful gases released by the base board and the thin board. The preparation method provided by the present invention is simple to operate, low in cost, and suitable for industrial production applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic diagram of a veneer panel;

[0038] Figure 2 This is a SEM image of the nano-titanium dioxide prepared in Example 4;

[0039] Figure 3 This is the element distribution diagram of the impregnated film paper prepared in Application Example 1;

[0040] Figure 4This is the SEM image of the impregnated film paper prepared in Application Example 1;

[0041] Figure 5 This is the SEM image of the cross section of the impregnated film paper prepared in Application Example 1.

[0042] Figure 6 A dryer for measuring formaldehyde emission. DETAILED DESCRIPTION

[0043] The present invention provides a modified graphene composite sealing agent, comprising the following raw materials in parts by weight:

[0044] 260-520 parts of chitosan, 80-110 parts of modified graphene, 30-60 parts of nano titanium dioxide, 5-40 parts of polyethylene terephthalate, 5-40 parts of dicyclohexylmethane diisocyanate, 5-40 parts of 4-ethyl-4-soyyl ethyl sulfate morpholine, and 500-2000 parts of water;

[0045] The modified graphene is O, N, S co-doped modified graphene;

[0046] The particle size of the nano titanium dioxide is 5 to 500 nm.

[0047] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.

[0048] The raw materials for preparing the modified graphene composite sealing agent provided by the present invention include 260 to 520 parts by mass of chitosan, preferably 260 to 450 parts by mass, and more preferably 260 to 350 parts by mass.

[0049] The raw materials for preparing the modified graphene composite sealant provided by the present invention include 80 to 110 parts by mass of modified graphene, preferably 80 to 100 parts by mass, and more preferably 80 to 95 parts by mass. In the present invention, the preparation method of the modified graphene comprises the following steps:

[0050] The aqueous dispersion of graphene is mixed with 1-cysteine ​​and polyethylene glycol to obtain a mixed solution;

[0051] After mixing the mixed solution with isopropanol, adjusting the mixture to be alkaline to obtain a graphene-modified precursor;

[0052] The graphene-modified precursor is irradiated to obtain the modified graphene.

[0053] The invention mixes a water dispersion of graphene with 1-cysteine ​​and polyethylene glycol to obtain a mixed solution.

[0054] In the present invention, the graphene is preferably commercially available industrial-grade graphene. In the present invention, the concentration of the aqueous dispersion of graphene is preferably 0.04 to 1.0 g / L, more preferably 0.04 to 0.5 g / L. In the present invention, the aqueous dispersion of graphene is obtained by adding graphene to water, preferably by ultrasonic dispersion for 1 to 2 hours. In the present invention, the water is preferably deionized water or pure water.

[0055] In the present invention, the mixing is preferably carried out under ultrasonic conditions, and the mixing time is preferably 30 to 100 min. In the present invention, the average molecular weight of the polyethylene glycol is preferably 1500 to 1800, more preferably 1500. The present invention uses polyethylene glycol as a solvent, which can be miscible with the aqueous dispersion of graphene and 1-cysteine, has good dispersibility, and the polyethylene glycol has stable performance, non-toxicity, non-irritation, and the decomposition products after irradiation are all volatile, and no secondary pollution will be generated. In the present invention, the 1-cysteine ​​is a donor of O, N, and S in the modified graphene. After irradiation, 1-cysteine ​​is excited to decompose and release free radical fragments containing O, N, and S, which are attached and embedded in the surface and interlayer of graphene, overcoming the problem of sheet stacking caused by oxidation and interlayer van der Waals force of ordinary graphene, improving the interlayer structure of graphene, and enhancing the electronegativity of modified graphene, so that the modified graphene has a strong adsorption performance for formaldehyde and VOC.

[0056] After obtaining the mixed solution, the present invention mixes the mixed solution with isopropanol and adjusts it to alkalinity to obtain a graphene modified precursor. In the present invention, the alkaline pH value is preferably 8 to 10, and more preferably 9. In the present invention, the amount ratio of the aqueous dispersion of graphene, 1-cysteine, polyethylene glycol and isopropanol is preferably 100 to 2000 mL: 0.1 to 2 g: 15 to 300 mL: 4 to 80 mL, and more preferably 200 to 1000 mL: 0.1 to 2 g: 15 to 300 mL: 4 to 80 mL.

[0057] In the present invention, the isopropanol is a free radical quencher, which has the function of delaying, inhibiting and blocking the oxidative damage of active oxygen and oxygen free radicals, and protects the raw graphene body from oxidative damage during the preparation of modified graphene.

[0058] After obtaining the graphene modified precursor, the present invention irradiates the graphene modified precursor to obtain the modified graphene. In the present invention, the irradiation is preferably carried out in an irradiation bag, preferably using a GJ-2-II electron accelerator for irradiation, preferably using X-rays and / or electron beams for irradiation. In the present invention, the irradiation dose is preferably 70 to 280 kGy, more preferably 70 to 240 kGy.

[0059] In the present invention, after the irradiation is completed, centrifugation, washing and freeze drying are preferably further performed. In the present invention, the centrifugation is preferably performed using a high-speed centrifuge. In the present invention, the speed of the centrifugation is preferably 8000 to 15000 r / min. In the present invention, the washing preferably includes washing with anhydrous ethanol and deionized water in sequence. In the present invention, the freeze drying time is preferably 10 to 24 hours.

[0060] The diameter of the modified graphene prepared by the present invention is preferably 0.8 to 20 μm, and the thickness is preferably 0.6 to 25 nm. In the present invention, the mixed system is irradiated so that the surface of the modified graphene can load a large amount of O / N / S free radicals, so that the surface of the modified graphene is electronegative, which is more conducive to combining with formaldehyde and VOC gases, so that the modified graphene has better absorption performance and can absorb formaldehyde and VOC more effectively.

[0061] The raw materials for preparing the modified graphene composite sealant provided by the present invention include 30 to 60 parts by mass of nano titanium dioxide, preferably 30 to 55 parts by mass, and more preferably 30 to 50 parts by mass. In the present invention, the particle size of the nano titanium dioxide is 5 to 500 nm. The present invention provides a method for preparing the nano titanium dioxide, comprising the following steps:

[0062] Mix tetrabutyl titanate, anhydrous ethanol and water to obtain solution A;

[0063] The acetic acid aqueous solution is mixed with the A solution and subjected to hydrothermal treatment to obtain the nano titanium dioxide.

[0064] The present invention stirs and mixes acetic acid and water to obtain the acetic acid aqueous solution. In the present invention, the water is preferably deionized water or pure water. In the present invention, the volume concentration of the acetic acid aqueous solution is preferably 0.001% to 28%, more preferably 1% to 15%. In the present invention, the time for stirring and mixing the acetic acid and water is preferably 10 to 60 minutes, more preferably 30 minutes, and the stirring and mixing speed is preferably 500 to 1000 r / min, more preferably 800 to 1000 r / min.

[0065] The present invention mixes tetrabutyl titanate, anhydrous ethanol and water to obtain solution A. In the present invention, the dosage ratio of tetrabutyl titanate, anhydrous ethanol and water is preferably 0.1-1 mL: 4-40 mL: 20-68 mL, and more preferably 0.1-0.8 mL: 8-36 mL: 20-36 mL. In the present invention, the mixing is preferably carried out in an ultrasonic manner. In the present invention, the ultrasonic time is preferably 10-30 min.

[0066] After obtaining solution A, the present invention mixes an acetic acid aqueous solution with solution A and performs hydrothermal treatment to obtain the nano titanium dioxide. In the present invention, the hydrothermal treatment is preferably carried out in an autoclave. In the present invention, the temperature of the hydrothermal treatment is preferably 150 to 300°C, more preferably 180 to 200°C. In the present invention, the time of the hydrothermal treatment is preferably 8 to 24 hours, more preferably 10 to 20 hours. In the present invention, the hydrothermal treatment preferably also includes drying, the drying temperature is preferably 50 to 80°C, and the drying time is preferably 10 to 15 hours. In the present invention, adding a small amount of anhydrous ethanol and acetic acid helps to reduce the hydrolysis of nano titanium dioxide. The hydrothermal treatment of the present invention can improve the crystallinity of nano titanium dioxide, making the particle size of nano titanium dioxide finer and more uniform.

[0067] The particle size of the nano titanium dioxide prepared by the present invention is 5 to 500 nm. The nano titanium dioxide prepared by the present application is different from the common commercially available titanium dioxide. The commonly used commercially available titanium dioxide can only absorb ultraviolet light, and ultraviolet light only accounts for about 5% of the full spectrum energy of sunlight. The nano titanium dioxide provided by the present invention absorbs the entire spectrum and can perform photocatalysis under the full spectrum conditions (wavelength of 380 to 780 nm), and has excellent catalytic degradation of formaldehyde and VOC gases.

[0068] The nano titanium dioxide prepared by the present invention is added to the modified graphene composite sealant. On the one hand, under the action of visible light, the dielectric material generates positive and negative electron charges, generates a strong catalytic degradation function, and can effectively decompose the formaldehyde and VOC gases released from the veneer artificial board. On the other hand, the dense nano titanium dioxide has good barrier properties, which can improve the sealing performance, thereby reducing the release of formaldehyde and VOC in the veneer artificial board. In addition, the nano titanium dioxide can kill a variety of bacteria, decompose and harmlessly treat toxins released by bacteria or fungi; at the same time, it also has the functions of removing formaldehyde, deodorizing, sterilizing, self-cleaning and anti-fouling, and purifying air.

[0069] The raw materials for preparing the modified graphene composite sealing agent provided by the present invention include 5 to 40 parts by mass of polyethylene terephthalate, preferably 6 to 32 parts by mass, and more preferably 6 to 25 parts by mass.

[0070] The raw materials for preparing the modified graphene composite sealing agent provided by the present invention include 5 to 40 parts by mass of dicyclohexylmethane diisocyanate, preferably 8 to 33 parts by mass, and more preferably 8 to 28 parts by mass.

[0071] The raw materials for preparing the modified graphene composite sealing agent provided by the present invention include 5 to 40 parts by mass of 4-ethyl-4-soyyl sulfate ethyl morpholine, preferably 11 to 29 parts by mass, and more preferably 13 to 25 parts by mass.

[0072] The raw materials for preparing the modified graphene composite sealant provided by the present invention include 500 to 2000 parts by mass of water, preferably 500 to 1890 parts by mass, and more preferably 650 to 1560 parts by mass. In the present invention, the water is preferably one of deionized water, distilled water or pure water.

[0073] The present invention also provides a method for preparing the modified graphene composite sealing agent, comprising the following steps:

[0074] Chitosan, modified graphene, nano titanium dioxide, polyethylene terephthalate, dicyclohexylmethane diisocyanate, 4-ethyl-4-soyyl ethyl sulfate morpholine and water are mixed, stirred and ultrasonically treated to obtain the modified graphene composite sealing agent.

[0075] In the present invention, the stirring speed is preferably 1000-9000 r / min, more preferably 7000-8500 r / min. In the present invention, the power of the ultrasound is preferably 2000-8000 W, more preferably 3000-6000 W. In the present invention, the stirring and ultrasound are preferably performed simultaneously, and the time of the stirring and ultrasound treatment is preferably 20-240 min, more preferably 30-150 min.

[0076] The present invention provides the use of the modified graphene composite sealant described in the above technical solution as a coating material.

[0077] The present invention also provides an impregnated adhesive film paper, which is obtained by impregnating a film material in a coating material and drying the impregnated adhesive film paper.

[0078] In the present invention, the membrane material preferably includes one or more of α-cellulose based decorative paper, plastic film and leather, and more preferably α-cellulose based decorative paper.

[0079] In the present invention, the coating material includes a sealant, and the sealant is the modified graphene composite sealant described in the above technical solution or the modified graphene composite sealant prepared by the preparation method. In the present invention, the coating material preferably uses only the modified graphene composite sealant described in the above technical solution. In the present invention, the use of the coating material preferably includes one or more of brushing, spraying and dipping. In the present invention, if the viscosity of the coating material is high and cannot meet the use requirements, the coating material can be diluted. In the present invention, the diluent used for the dilution preferably includes a 50wt% ethanol aqueous solution. The present invention does not specifically limit the dilution, and it can be carried out according to conventional operations in the field.

[0080] In the present invention, the amount of glue applied to the coating material on the impregnated glue film paper is preferably 40 to 200 g / m 2 .

[0081] In the present invention, the method for preparing the impregnated glue film paper preferably comprises the following steps:

[0082] The film material is impregnated into the coating material, taken out and pressed and dried to obtain the impregnated adhesive film paper.

[0083] In the present invention, the impregnation temperature is preferably 100-180°C, and the time is preferably 10-30 min. In the present invention, the pressing time is preferably 60-230 s, and the pressing pressure is preferably 2.0-3.0 MPa. In the present invention, the drying temperature is preferably 120-150°C, and the time is preferably 100-180 s.

[0084] The present invention also provides a facing artificial board, which comprises a base board, a thin board and facing paper which are stacked in sequence; the facing paper is the impregnated adhesive film paper described in the above technical solution.

[0085] In the present invention, the base board preferably includes one or more of a particle board, a wood board and a compressed board.

[0086] In the present invention, the thin board preferably comprises a wood thin board and / or a medium density fiberboard. In the present invention, the thickness of the thin board is preferably 10 to 26 mm.

[0087] In the present invention, the method for preparing the veneer artificial board comprises the following steps:

[0088] Grinding the base plate to obtain a pre-treated base plate;

[0089] Pasting thin plates to both sides of the pre-treated base plate to obtain a flat plate;

[0090] The facing paper is placed on both sides of the flat board and pressed to obtain the facing artificial board.

[0091] The present invention grinds the base plate to obtain a pre-treated base plate.

[0092] In the present invention, the grinding is preferably carried out using sandpaper with a grit of 50-80-100. In the present invention, the base plate is ground until the surface is smooth without obvious bumps and pits.

[0093] After obtaining the pre-treated base plate, the present invention adheres the thin plates to both sides of the pre-treated base plate to obtain a flat plate.

[0094] In the present invention, the pasting can be performed according to conventional operations in the art.

[0095] After obtaining the flat board, the present invention places facing paper on both sides of the flat board and presses it to obtain the facing artificial board.

[0096] In the present invention, the facing paper is preferably the impregnated glue film paper prepared by the above technical solution. In the present invention, the pressing temperature is preferably 150-200°C, more preferably 170°C. In the present invention, the pressing time is preferably 30-60s, more preferably 40s. In the present invention, the pressing pressure is preferably 2-5MPa, more preferably 3MPa.

[0097] In the present invention, during the pressing process, the facing paper can be self-adhesive to the resin-free flat board, and at the same time, a resin-rich coating is formed on the surface of the flat board. After the coating material impregnated on the facing paper is cured, a dense film layer is formed, which can effectively reduce and absorb formaldehyde and VOC gases released by the board.

[0098] In the present invention, the veneer artificial board is preferably cured under the conditions of 20° C. and 65% relative humidity.

[0099] Figure 1 This is a schematic diagram of the veneer panel. Figure 1 The middle substrate is the pre-treated base board described in the above scheme, with thin boards pasted on both sides, and the outer sides of the thin boards are covered with impregnated film paper, and the facing artificial board is obtained after pressing.

[0100] The technical solution of the present invention is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0101] The raw materials chitosan, tetrabutyl titanate, and graphene were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0102] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.

[0103] Example 1

[0104] 0.5g of graphene was dispersed in 500mL of deionized water, and ultrasonicated for 1 hour to obtain an aqueous dispersion of graphene with a concentration of 1g / L; 0.5g of l-cysteine ​​and 75mL of polyethylene glycol (PEG-1500) were added, and ultrasonicated for 30min to obtain a mixture; 20mL of isopropanol was added to the obtained mixture as a free radical quencher, and the pH value of the solution was adjusted to 9 with ammonia water to obtain a graphene-modified precursor; the obtained graphene-modified precursor was encapsulated in a homemade polyethylene irradiation bag, and irradiated using a GJ-2-II electron accelerator, with an irradiation dose of 140kGy. The product was separated using a high-speed centrifuge (10000r / min), washed with anhydrous ethanol and deionized water, and finally freeze-dried to obtain modified graphene.

[0105] Example 2

[0106] The only difference from Example 1 is that the irradiation dose is 210 kGy.

[0107] Example 3

[0108] The only difference from Example 1 is that 1 g of l-cysteine ​​and 100 mL of polyethylene glycol (PEG-1500) are added.

[0109] Example 4

[0110] 100 μL of acetic acid was added dropwise into 20 mL of deionized water and stirred for 30 min at a stirring speed of 800 r / min to obtain an acetic acid aqueous solution with a volume concentration of 0.5%.

[0111] 0.25 mL of tetrabutyl titanate was ultrasonically dispersed in a mixed solution of 10 mL of ethanol and 25 mL of water, and ultrasonic treatment was performed for 15 min to obtain solution A. The obtained acetic acid aqueous solution and solution A were stirred and mixed evenly, and then transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and hydrothermally treated at 180°C for 12 hours, and then dried at 60°C for 12 hours to obtain nano titanium dioxide.

[0112] Figure 2 This is the SEM image of the nano-titanium dioxide prepared in Example 4. Figure 2 It can be seen that the nano-titanium dioxide particles are spherical and have evenly distributed holes on the surface, indicating that the prepared nano-titanium dioxide has a large specific surface area, can absorb visible light, and has a high activity in photocatalytic degradation of formaldehyde and VOC gases.

[0113] Example 5

[0114] 260 parts by mass of chitosan, 82 parts by mass of modified graphene prepared in Example 1, 46 parts by mass of nano-titanium dioxide prepared in Example 4, 23 parts by mass of polyethylene terephthalate, 10 parts by mass of dicyclohexylmethane diisocyanate, 22 parts by mass of 4-ethyl-4-soyyl sulfate ethyl morpholine and 800 parts by mass of deionized water were mixed, stirred and ultrasonically treated at a stirring speed of 3000 r / min, an ultrasonic power of 2000 W, and a stirring and ultrasonic treatment time of 180 min to obtain a modified graphene composite sealing agent.

[0115] Example 6

[0116] The only difference from Example 5 is that the modified graphene prepared in Example 2 is used to prepare the modified graphene composite sealing agent.

[0117] Example 7

[0118] The only difference from Example 5 is that the modified graphene prepared in Example 3 is used to prepare the modified graphene composite sealing agent.

[0119] Comparative Example 1

[0120] Compared with Example 5, the difference is that unmodified ordinary graphene is added.

[0121] Comparative Example 2

[0122] Compared with Example 5, the difference is that no nano titanium dioxide is added.

[0123] Application Example 1

[0124] The modified graphene composite sealant prepared in Example 5 was heated to 120° C., and then the α-cellulose-based modified paper was immersed in the modified graphene composite sealant for 30 minutes. After being taken out, it was pressed at a pressure of 3.0 MPa for 60 seconds, and then dried at 150° C. for 180 seconds to obtain an impregnated film paper.

[0125] The particle board was polished with sandpaper of 50, 80 and 100 grits in sequence to obtain a pretreated base board; a wooden veneer was pasted to both sides of the pretreated base board to obtain a flat board; the prepared impregnated film paper was placed on both sides of the flat board, and pressed at 150°C for 40s with a pressure of 3MPa to obtain a veneered artificial board.

[0126] Energy dispersive X-ray spectrometer (EDS) was used to test the chemical composition of the prepared impregnated film paper. The test results are as follows: Figure 3 shown. Figure 3 This is the element distribution diagram of the impregnated film paper prepared in Application Example 1. Figure 3 It can be seen that the element content is C>N>S>O, and the O, N, and S elements are evenly distributed in the modified graphene. The O, N, and S co-doped modified graphene overcomes the problem of sheet stacking caused by oxidation and interlayer van der Waals force of ordinary graphene, making the surface of the modified graphene electronegative, which is more conducive to combining with formaldehyde and VOC gases, improving the activation ability of formaldehyde and VOC gases, and making the modified graphene have better absorption performance and can absorb formaldehyde and VOC more effectively. Figure 3 The Ti elements are evenly distributed in the nanometer scale and can perform photocatalysis in the entire spectrum, thus improving the performance of the modified graphene composite sealer and impregnated adhesive film paper in degrading formaldehyde and VOC.

[0127] The impregnated film paper obtained by scanning electron microscope (SEM) test was randomly cut into 0.5mm×0.5mm samples at any position, bonded to the sample holder of SEM, and subjected to gold spraying. The surface microstructure was observed using SEM. The test results are shown in the figure. Figure 4 shown. Figure 4 This is the SEM image of the impregnated film paper prepared in Application Example 1. Figure 4 Figure a and Figure 4 It can be seen from Figure b that the surface of the impregnated film paper is relatively smooth, indicating that the modified graphene composite sealant coated on the surface of the impregnated film paper forms a continuous, flat film without holes, has good film-forming properties, and can effectively isolate formaldehyde and VOCs and reduce their release.

[0128] Figure 5 This is the SEM image of the cross section of the impregnated film paper prepared in Application Example 1. Figure 5 It can be clearly seen that the modified graphene composite sealant is tightly combined with the membrane material without cracks, indicating that the modified graphene has good compatibility and adhesion with the membrane material, and can form a dense film layer, thereby blocking the release of formaldehyde and VOC.

[0129] The formaldehyde emission of the veneer artificial board prepared in Application Example 1 was tested according to the standard GB15516-1995 “Determination of formaldehyde in air quality - Acetylacetone spectrophotometry”. The test results are shown in Table 1.

[0130] According to the standard HJ759-2015 “Determination of volatile organic compounds in ambient air: tank sampling / gas chromatography-mass spectrometry”, the VOC emission of the veneer artificial board prepared in Application Example 1 was tested. The test results are shown in Table 2.

[0131] Application Example 2

[0132] The difference from Application Example 1 is that the modified graphene composite sealant prepared in Example 6 is used to prepare the impregnated film paper; and the obtained impregnated film paper is prepared into a veneer artificial board.

[0133] The formaldehyde emission of the prepared facing artificial board was tested according to standard GB15516-1995 “Determination of formaldehyde in air quality—Acetylacetone spectrophotometric method”. The test results are shown in Table 1.

[0134] Application Example 3

[0135] The difference from Application Example 1 is that the modified graphene composite sealant prepared in Example 7 is used to prepare the impregnated film paper; and the obtained impregnated film paper is prepared into a veneer artificial board.

[0136] The formaldehyde emission of the prepared facing artificial board was tested according to standard GB15516-1995 “Determination of formaldehyde in air quality—Acetylacetone spectrophotometric method”. The test results are shown in Table 1.

[0137] Application Example 4

[0138] The difference from Application Example 1 is that medium-density fiberboard is used to prepare the veneer artificial board.

[0139] Application Comparative Example 1

[0140] The difference from Application Example 1 is that the graphene composite sealant prepared in Comparative Example 1 is used to prepare the impregnated film paper and the veneer artificial board.

[0141] According to standard GB15516-1995 "Determination of formaldehyde in air quality - Acetylacetone spectrophotometric method", the formaldehyde emission of the facing artificial board prepared in comparative example 1 was tested. The test results are shown in Table 1.

[0142] According to standard HJ759-2015 “Determination of volatile organic compounds in ambient air: tank sampling / gas chromatography-mass spectrometry”, the VOC emission of the veneer artificial board prepared by comparative example 1 was tested. The test results are shown in Table 2.

[0143] Application Comparative Example 2

[0144] The difference from Application Example 1 is that the graphene composite sealant prepared in Comparative Example 2 is used to prepare the impregnated film paper and the veneer artificial board.

[0145] The formaldehyde emission of the prepared facing artificial board was tested according to standard GB15516-1995 “Determination of formaldehyde in air quality—Acetylacetone spectrophotometric method”. The test results are shown in Table 1.

[0146] Test analysis

[0147] Test equipment:

[0148] Gas chromatograph-mass spectrometer (GC-MS), Agilent, USA; several stainless steel vacuum SUMMA tanks from ENTECH; UV / visible spectrophotometer (UV-1600PC), Mepda; magnetic stirrer, IKA Instrument Equipment Co., Ltd., Germany; blast oven, Hangzhou Yijie Technology Co., Ltd.; scanning electron microscope (SEM), Hitachi Scientific Instruments Co., Ltd.

[0149] The prepared veneer artificial board was edge-sealed using aluminum tape. The exposed area of ​​the sample after edge-sealing was 500 cm 2 Before the test, the edge-sealed samples were divided into two groups, and one group was irradiated under visible light for 6 hours to stimulate the photocatalytic degradation activity of titanium dioxide in the modified graphene composite sealant.

[0150] (1) Determination method of formaldehyde emission from veneer panels:

[0151] According to the standards GB / T17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels" and GB15516-1995 "Determination of formaldehyde in air quality - acetylacetone spectrophotometry", the dryer-spectrophotometry method was used to determine the formaldehyde emission of laminated panels.

[0152] The specific operation of the desiccant-spectrophotometric method for measuring formaldehyde content is as follows: the edge-sealed veneer artificial board is processed into a test block of 5 cm × 15 cm, and the test block is placed in a desiccant (volume 9 to 11 L), and distilled water (such as Figure 6 The dryer was placed in an environment of 20±2°C for 24 hours, 7 days and 30 days, and samples were taken respectively, so that the formaldehyde released by the veneer wood-based panel was fully absorbed by the distilled water to obtain the absorption liquid sample. The formaldehyde content in the absorption liquid sample was determined by acetylacetone spectrophotometry.

[0153] Each sample was measured three times in parallel to ensure the authenticity and reliability of the experimental data. The formaldehyde emission results of the veneer wood-based panels are shown in Table 1.

[0154] Table 1 Formaldehyde emission of veneer panels

[0155]

[0156]

[0157] It can be seen from Table 1 that: 1. The modified graphene composite sealant prepared by Application Example 1 using an irradiation dose of 140 kGy has the lowest formaldehyde emission; the formaldehyde emission of the veneer panels prepared by Application Examples 2 and 3 is equivalent to that of Application Example 1; according to the national standard GB / T39600-2021 "Grading of Formaldehyde Emission of Artificial Boards and Their Products", the formaldehyde emission of the veneer panels prepared by Application Examples 1 to 3 of the present invention is equivalent to E0 grade. 2. With the extension of time, the formaldehyde emission and degradation amount gradually increase, and the formaldehyde emission of the veneer panels prepared by Comparative Examples 1 and 2 is high.

[0158] (2) Determination of volatile organic compound (VOC) emissions from veneer panels

[0159] Before the VOC emission measurement, the edge-sealed veneer wood-based panel samples were placed in sealed bags and placed in an environment at 20±2°C for 24h, 7 days and 30 days, and samples were taken respectively.

[0160] The present invention adopts the vacuum tank sampling method for sampling, and the specific operation includes: cleaning and drying the stainless steel vacuum SUMMA tank before sampling. Evacuating the stainless steel vacuum SUMMA tank to make its internal pressure ≥6Pa, then injecting high-purity nitrogen (99.99%) to clean the tank body, pressurizing it to 0.4MPa, repeating the above steps 4 times, and finally evacuating the stainless steel vacuum SUMMA tank to make its internal pressure ≥10Pa, and the stainless steel vacuum SUMMA sampling tank is ready.

[0161] After cleaning 20 stainless steel vacuum SUMMA tanks, one is extracted and injected with high-purity nitrogen for analysis to determine whether the cleaning process is clean. If the stainless steel vacuum SUMMA tank is tested for high concentration of contaminants, after cleaning, it is necessary to analyze the local contamination before the next use.

[0162] The above-mentioned stainless steel vacuum SUMMA sampling cans are used to take samples from the sealed bags containing the veneer wood-based panel samples.

[0163] The collected samples were tested and analyzed for VOC according to the standard HJ759-2015 "Determination of Volatile Organic Compounds in Ambient Air: Canister Sampling / Gas Chromatography-Mass Spectrometry". The test results are shown in Table 2.

[0164] Table 2 VOC emission of veneer panels

[0165]

[0166]

[0167] It can be seen from Table 2 that a variety of VOC volatile compounds were detected, including carcinogenic pollutants such as toluene, benzaldehyde, ethyltoluene, and p-xylene. The test results show that the VOC gas release of the veneer artificial board prepared by modified graphene in Application Example 1 of the present invention is significantly reduced compared with the veneer artificial board prepared by ordinary graphene in Application Comparative Example 1, proving that the veneer artificial board prepared by the modified graphene composite sealant provided by the present invention can effectively reduce the VOC release.

[0168] (3) Graphene specific surface area (BET) test

[0169] The modified graphene prepared in Example 1 and the ordinary graphene used in Comparative Example 1 were degassed at 300° C. under vacuum for 4 h. According to the standard GB / T19587-2004 "Determination of specific surface area of ​​solid substances by gas adsorption BET method", the specific surface area of ​​graphene was tested using a specific surface area and pore size distribution instrument. The test results are shown in Table 3.

[0170] Table 3 Test results of specific surface area of ​​graphene

[0171] sample <![CDATA[Specific surface area, m 2 / g]]> Modified graphene prepared in Example 1 3728.6 Comparative Example 1: Ordinary Graphene 2536.2

[0172] It can be seen from Table 3 that the specific surface area of ​​the modified graphene is much larger than that of the ordinary graphene. The modified graphene prepared by the present invention has a high specific surface area, which provides a large number of adsorption centers for the enrichment and catalytic degradation of formaldehyde and VOC volatile organic compounds.

[0173] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A modified graphene composite sealing agent, characterized in that: The preparation comprises the following raw materials in parts by weight: 260-520 parts of chitosan, 80-110 parts of modified graphene, 30-60 parts of nano titanium dioxide, 5-40 parts of polyethylene terephthalate, 5-40 parts of dicyclohexylmethane diisocyanate, 5-40 parts of 4-ethyl-4-soyyl ethyl sulfate morpholine, and 500-2000 parts of water; The modified graphene is O, N, S co-doped modified graphene; The particle size of the nano titanium dioxide is 5 to 500 nm.

2. The modified graphene composite sealing agent according to claim 1, characterized in that: The preparation method of the modified graphene comprises the following steps: The aqueous dispersion of graphene is mixed with 1-cysteine ​​and polyethylene glycol to obtain a mixed solution; After mixing the mixed solution with isopropanol, adjusting the mixture to be alkaline to obtain a graphene-modified precursor; The graphene-modified precursor is irradiated to obtain the modified graphene.

3. The modified graphene composite sealing agent according to claim 2, characterized in that: The usage ratio of the graphene aqueous dispersion, 1-cysteine, polyethylene glycol and isopropanol is 100-2000mL: 0.1-2g: 15-300mL: 4-80mL; the concentration of the graphene aqueous dispersion is 0.04-1.0g / L; The alkaline pH value is 8 to 10; The irradiation dose is 70 to 280 kGy.

4. The modified graphene composite sealing agent according to claim 1, characterized in that: The preparation method of nano titanium dioxide comprises the following steps: Mix tetrabutyl titanate, anhydrous ethanol and water to obtain solution A; The acetic acid aqueous solution is mixed with the A solution and subjected to hydrothermal treatment to obtain the nano titanium dioxide.

5. The modified graphene composite sealing agent according to claim 4, characterized in that: The volume concentration of the acetic acid aqueous solution is 0.001% to 28%; the dosage ratio of tetrabutyl titanate, anhydrous ethanol and water in the A solution is 0.1 to 1 mL: 4 to 40 mL: 20 to 68 mL; The temperature of the hydrothermal treatment is 150-300° C., and the time is 8-24 hours.

6. The method for preparing the modified graphene composite sealing agent according to any one of claims 1 to 5, characterized in that: The following steps are involved: Chitosan, modified graphene, nano titanium dioxide, polyethylene terephthalate, dicyclohexylmethane diisocyanate, 4-ethyl-4-soyyl ethyl sulfate morpholine and water are mixed, stirred and ultrasonically treated to obtain the modified graphene composite sealing agent.

7. The preparation method according to claim 6, characterized in that: The stirring speed is 1000-9000 r / min; the ultrasonic power is 2000-8000 W; the stirring and ultrasonic treatment are carried out simultaneously, and the time of the stirring and ultrasonic treatment is 20-240 min.

8. Use of the modified graphene composite sealing agent described in any one of claims 1 to 5 or the modified graphene composite sealing agent prepared by the preparation method described in any one of claims 6 to 7 as a coating material.

9. An impregnated film paper, characterized in that: The impregnated adhesive film paper is obtained by impregnating the film material in the coating material and drying; The membrane material includes one or more of α-cellulose-based modified paper, plastic film and leather; The coating material includes a sealant; The sealing agent is the modified graphene composite sealing agent described in any one of claims 1 to 5 or the modified graphene composite sealing agent prepared by the preparation method described in any one of claims 6 to 7.

10. A facing artificial board, characterized in that: The facing artificial board comprises a base board, a thin board and a facing paper which are stacked in sequence; The facing paper is the impregnated adhesive film paper as described in claim 9.

Citation Information

Patent Citations

  • Synthesis method of sulfur-doped reduced graphene used for adsorbing organic pollutants

    CN106975446A

  • Photocatalyst suspension, anti-adhesion self-cleaning artificial board decorative paper and preparation method thereof

    CN107151941A

  • Graphene / titanium dioxide composite material, preparation method and application thereof

    CN108160064A

  • Preparation method of graphene oxide / titanium dioxide composite coating material

    CN108624203A

  • Composite deodorant as well as preparation method and application thereof

    CN115595048A