Wet recovery process for titanium, vanadium and molybdenum in waste SCR denitration catalyst

Through wet process and electrolytic treatment, the conductive coating is prepared in combination with composite slurry, which solves the problem of low purity of titanium, vanadium and molybdenum recovery in waste SCR denitrification catalysts, and achieves efficient molybdenum and vanadium recycling, enhancing the controllability of the process Sex and efficiency.

CN119020591APending Publication Date: 2024-11-26GANSU YINGHUA ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410436390.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

There is a lack of efficient recycling technology for titanium, vanadium and molybdenum in waste SCR denitrification catalysts, and the existing methods are difficult to control the amount of precipitant, resulting in a decrease in the purity of the recovered product and co-precipitation, which affects the recycling efficiency of molybdenum and vanadium.

Method used

By adopting wet process, the amount of precipitant is controlled through alkali leaching and electrolytic treatment, the amount of precipitation is reduced, the recovery purity of molybdenum and vanadium is improved, the conductive coating is prepared using composite slurry, the electrolytic conditions are optimized, the molybdenum and titanium are trapped, and the Molybdenum remains.

Benefits of technology

The purity of the recycling products of molybdenum and vanadium is improved, the residues of molybdenum and titanium are reduced, and the efficient recycling of titanium, vanadium and molybdenum is achieved, and the controllability and efficiency of the recycling process are enhanced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a wet recovery process for titanium, vanadium and molybdenum in a waste SCR denitration catalyst, and belongs to the technical field of non-ferrous metal recovery, a denitration catalyst body is subjected to soot blowing, crushing and ball milling to form powder, alkaline leaching is performed to obtain a leaching solution and titanium-rich slag, the leaching solution is transferred to a sedimentation tank, and pre-impurity removal treatment is performed to remove calcium silicate precipitate, so that the titanium-rich slag is obtained; carrying out primary filtrate treatment to obtain precipitate CaMoO4, obtaining secondary filtrate, carrying out electrolytic treatment, and then hydrolyzing to recover V2O5 precipitate; by optimizing the adding amount of the calcium chloride powder, when calcium molybdate is precipitated in the primary filtrate, coprecipitation of vanadate radicals is reduced while molybdenum recovery is guaranteed to the maximum extent, the purity of the calcium molybdate is increased, and follow-up recovery is facilitated; the affinity of the 1-butyl-3-methylimidazole chlorine salt to molybdenum is higher than that of vanadium, MoO2 < 2 + > is firstly converted into MoO3 by the conductive coating on the negative plate of the electrolytic bath and the MoO3 is captured, so that the residual molybdenum in the secondary filtrate is reduced, and the purity of V2O5 is favorably increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metal recovery, and in particular relates to a wet recovery process of titanium, vanadium and molybdenum in a discarded SCR denitration catalyst. Background Art

[0002] With the continuous improvement of environmental awareness, in addition to coal-fired power plants, the emission standards of flue gas pollutants in industries such as steel, cement, and waste incineration have successively introduced restrictions on NOx emission concentrations. The selective catalytic reduction (SCR) flue gas denitrification process has been widely used in coal-fired power plants, steel, cement, coking chemistry, etc. due to its high denitrification efficiency and good selectivity. Due to long-term exposure to toxic flue gas without dust removal and desulfurization, fly ash in the flue gas will block the catalyst micropores, and toxic compounds will cause the catalyst to deactivate during operation, shortening its service life.

[0003] Due to the harsh working environment, its service life is usually only 2-3 years. Catalysts that have reduced activity and cannot be restored through regeneration technology will eventually become waste SCR denitrification catalysts. Waste SCR denitrification catalysts are a special type of solid waste with the following characteristics: (1) High toxicity. Waste SCR denitrification catalysts not only contain Class B inorganic highly toxic substances V2O5 and heavy metal oxides MoO3, but also absorb highly toxic elements such as As, Hg, and Pb in flue gas during use. These toxic elements will cause great harm when entering the environment. (2) Large output. According to relevant data estimates, in 2021, the annual output of waste SCR denitrification catalysts generated by thermal power plants alone will reach 110,000 m 3 As the application scope of SCR denitrification technology continues to expand, the output of domestic waste SCR denitrification catalysts will continue to grow. The reasonable disposal of a large number of waste SCR denitrification catalysts will be a severe challenge in the future. (3) There are many high value-added components. The raw materials used in the production of SCR denitrification catalysts are very expensive. (4) Recycling is difficult, and there is a lack of efficient recycling technology.

[0004] The invention with announcement number CN107512734B discloses a method for recovering tungsten, molybdenum, vanadium and titanium dioxide from discarded SCR denitrification catalysts. Molybdenum and vanadium are recovered by chemical precipitation, but the amount of precipitant is often difficult to control. Adding too little will result in incomplete precipitation, while adding too much will lead to co-precipitation, resulting in a decrease in the purity of the recovered molybdenum and vanadium. Summary of the invention

[0005] The purpose of the present invention is to provide a wet recovery process for titanium, vanadium and molybdenum in waste SCR denitration catalysts, reduce the occurrence of co-precipitation by controlling the dosage of precipitant, reduce the residual molybdenum by electrolytic capture, and thus increase the purity of the recovered molybdenum and vanadium products.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A wet recovery process for titanium, vanadium and molybdenum in a waste SCR denitration catalyst comprises the following steps:

[0008] Step 1: Disassemble the SCR denitration catalyst module, collect the denitration catalyst body, use compressed air to blow away the fly ash on the denitration catalyst body, then crush it, and use a planetary ball mill to grind it into a powder of 200-300 mesh; add the powder and a sodium hydroxide solution with a concentration of 50-150g / L into a leaching tank at a mass ratio of 1:3, stir and mix, add an oxidant of 3-6% of the mass of the powder, alkali leaching at 40-100°C for 1-3h, filter, and obtain a leachate containing vanadium and molybdenum and titanium-rich slag, and the titanium-rich slag is used to produce TiO2 products;

[0009] The main reactions include:

[0010] MoO3+2NaOH=Na2MoO4+H2O

[0011] V2O5+2NaOH=2NaVO3+H2O

[0012] Step 2: The leachate is transferred to a sedimentation tank, and the element contents of Si, Mo and vanadium are detected by a plasma emission spectrometer. After pre-impurity treatment to remove calcium silicate precipitate, a primary filtrate is obtained; the pH value of the primary filtrate is adjusted to 9 with hydrochloric acid, and calcium chloride powder is added in an amount of 1:1-1.2 in a molar ratio of Mo to Ca to convert Na2MoO4 into CaMoO4 precipitate, and the CaMoO4 precipitate is recovered by filtration to obtain a secondary filtrate;

[0013] Step 3: Pass the secondary filtrate into the electrolytic cell and adjust the pH value to 2-2.5 with hydrochloric acid. Under this pH condition, Mo and V in the secondary filtrate exist in the form of oxygen-containing cations. The distance between the cathode plate and the anode plate in the electrolytic cell is 5-8 cm. 2 The electrolysis treatment was carried out at a current density of 2-3 hours, and then the secondary filtrate after the electrolysis treatment was transferred to a sedimentation tank and hydrolyzed at 60-70°C for 6-8 hours to make VO 2+ It is hydrolyzed and converted into V2O5, and the V2O5 precipitate is filtered and recovered. The filtered tail liquid is passed into a sewage pool for environmental protection treatment, completing the wet recovery process of titanium, vanadium and molybdenum.

[0014] Furthermore, the oxidant is hydrogen peroxide.

[0015] Furthermore, the anode plate in the electrolytic cell is a titanium-coated ruthenium electrode.

[0016] Further, the cathode plate in the electrolytic cell is prepared by the following steps:

[0017] Add polyvinyl pyrrolidone, carbon nanotubes and N,N-dimethylamide into a stirring kettle and stir for 3-4 hours. Then add polyaniline, 1-butyl-3-methylimidazolium chloride, tributyl phosphate and cellulose triacetate into the reaction kettle, stir for 4-6 hours at 1200-1500r / min, and vacuum degas to obtain a composite slurry. The composite slurry is coated on the surface of a titanium mesh. After the solvent is evaporated and dried, 1-butyl-3-methylimidazolium chloride and other polymers are compositely crystallized and fixed in a polymer matrix to obtain a cathode plate with a 1-1.5mm thick conductive coating.

[0018] Furthermore, the usage ratio of polyvinyl pyrrolidone, carbon nanotubes, N,N-dimethylamide, polyaniline, 1-butyl-3-methylimidazole chloride, tributyl phosphate and cellulose triacetate is 10-12.5g:3-4g:200-250mL:15-18g:10-12.5g:5-6g:0.5-0.6g.

[0019] Further, the method for producing the TiO2 product is as follows:

[0020] The titanium-rich slag is vacuum dried and mixed with deionized water in a mass ratio of 1:3, and then the pH value is adjusted to 2-4 with a 1 mol / L sulfuric acid solution. The mixture is stirred at 20-25°C for 5-8h, filtered, washed with water, dried, and calcined at 550°C for 3-5h to obtain a TiO2 product.

[0021] Furthermore, the specific method of the pre-impurity removal treatment is: adjust the pH value of the leachate to 10.5-11 with hydrochloric acid, add calcium chloride powder at a molar ratio of Si to Ca of 1:1.3-1.5 at 15-25°C, stir and mix for 1-2h, the silicon in the leachate forms a precipitate in the form of calcium silicate, filter, collect the filtrate once, and complete the pre-impurity removal treatment.

[0022] Beneficial effects of the present invention:

[0023] The wet recovery process of titanium, vanadium and molybdenum in the waste SCR denitration catalyst of the present invention is helpful to improve the purity of the recovered products of molybdenum and vanadium. The leachate containing molybdenum and vanadium is wet recovered under leaching of alkaline solution, and calcium silicate is removed from the leachate by pre-impurity precipitation, which is helpful to reduce the residual silicon in the subsequent product; through the preferred addition of calcium chloride powder of the present invention, when calcium molybdate is precipitated from the primary filtrate, the molybdenum recovery is maximized while reducing the co-precipitation of vanadate, which is helpful to increase the purity of calcium molybdate for subsequent recovery.

[0024] After the pH value of the secondary filtrate is adjusted, the Mo and V therein exist in the electrolytic cell in the form of oxygen-containing cations. In the composite slurry, N,N-dimethylamide serves as a solvent, and polyvinyl pyrrolidone helps to increase its film-forming property, thereby increasing the strength of the conductive coating; carbon nanotubes and polyaniline help to increase the conductivity, tributyl phosphate plays a plasticizing role, and cellulose triacetate helps to improve the coating performance of the composite slurry; 1-butyl-3-methylimidazolium chloride and the remaining polymers are mixed evenly and form crystals, thereby combining in the conductive coating, and 1-butyl-3-methylimidazolium chloride has a higher affinity for molybdenum than vanadium. The conductive coating on the cathode plate of the electrolytic cell first converts MoO22+ into MoO3 and captures it, thereby reducing the residual molybdenum in the secondary filtrate and helping to increase the purity of V2O5. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1: This example provides a wet recovery process for titanium, vanadium and molybdenum in a waste SCR denitration catalyst, comprising the following steps:

[0027] Step 1: Disassemble the SCR denitration catalyst module, collect the denitration catalyst body, use compressed air to blow away the fly ash on the denitration catalyst body, then crush it, and use a planetary ball mill to grind it into a 200-mesh powder; add the powder and a sodium hydroxide solution with a concentration of 150g / L into a leaching tank at a mass ratio of 1:3, stir and mix, add 3% hydrogen peroxide by weight of the powder, alkali leaching at 40°C for 1h, filter, and obtain a leachate containing vanadium and molybdenum and titanium-rich slag;

[0028] The titanium-rich slag was vacuum dried and mixed with deionized water in a mass ratio of 1:3, and then the pH value was adjusted to 2 with a 1 mol / L sulfuric acid solution. The mixture was stirred at 20°C for 5 h, filtered, washed with water, and dried, and calcined at 550°C for 3 h to obtain a TiO2 product.

[0029] Step 2: Transfer the leachate to a sedimentation tank, and use an ICP-OES plasma emission spectrometer to detect the element contents of Si, Mo and vanadium; adjust the pH value of the leachate to 10.5 with hydrochloric acid, add calcium chloride powder at a molar ratio of Si to Ca of 1:1.3 at 15°C, stir and mix for 1 hour, and the silicon in the leachate forms a precipitate in the form of calcium silicate. Filter and remove the calcium silicate precipitate to obtain a primary filtrate; adjust the pH value of the primary filtrate to 9 with hydrochloric acid, add calcium chloride powder at a molar ratio of Mo to Ca of 1:1, convert Na2MoO4 into CaMoO4 precipitate, filter and recover the CaMoO4 precipitate to obtain a secondary filtrate.

[0030] Step 3: Add 10kg of polyvinyl pyrrolidone, 3kg of carbon nanotubes and 200L of N,N-dimethylamide into a stirring kettle and stir for 3h, then add 15kg of polyaniline, 10kg of 1-butyl-3-methylimidazolium chloride, 5kg of tributyl phosphate and 0.5kg of cellulose triacetate into the reaction kettle, stir for 4h at 1200r / min, vacuum degassing to obtain a composite slurry, and apply the composite slurry on the surface of the titanium mesh. After the solvent is volatilized, 1-butyl-3-methylimidazolium chloride and the remaining polymers are compositely crystallized and fixed in the polymer matrix to obtain a cathode plate with a 1mm thick conductive coating;

[0031] The secondary filtrate is passed into an electrolytic cell, and the pH value is adjusted to 2 with hydrochloric acid. Under this pH condition, Mo and V in the secondary filtrate exist in the form of oxygen-containing cations. The distance between the cathode plate and the anode plate in the electrolytic cell is 5 cm, and the anode plate is a titanium-coated ruthenium electrode. The electrolysis treatment is carried out at a current density of 40A / m2 for 2 hours to convert MoO22+ into MoO3 and capture it. Then, the secondary filtrate after the electrolysis treatment is transferred to a sedimentation tank and hydrolyzed at 60°C for 6 hours to convert VO2+ into V2O5 by hydrolysis. The V2O5 precipitate is filtered and recovered, and the filtered tail liquid is passed into a sewage pool for environmental protection treatment.

[0032] After detection by plasma emission spectrometer ICP-OES, the recovery rate of vanadium was 93.8%, and the purity of V2O5 was 99.7%; the recovery rate of molybdenum was 95.2%, and the purity of CaMoO4 was 98.3%.

[0033] Example 2: This example provides a wet recovery process for titanium, vanadium and molybdenum in a waste SCR denitration catalyst, comprising the following steps:

[0034] Step 1: disassemble the SCR denitration catalyst module, collect the denitration catalyst body, use compressed air to blow away the fly ash on the denitration catalyst body, then crush it, and use a planetary ball mill to grind it into a 250-mesh powder; add the powder and a sodium hydroxide solution with a concentration of 100g / L into a leaching tank at a mass ratio of 1:3, stir and mix, add 4% hydrogen peroxide by mass of the powder, alkali leaching at 70°C for 2h, filter, and obtain a leachate containing vanadium and molybdenum and titanium-rich slag;

[0035] The titanium-rich slag was vacuum dried and mixed with deionized water in a mass ratio of 1:3, and then the pH value was adjusted to 3 with a 1 mol / L sulfuric acid solution. The mixture was stirred at 22°C for 6.5 h, filtered, washed with water, and dried, and calcined at 550°C for 4 h to obtain a TiO2 product.

[0036] Step 2: Transfer the leachate to a sedimentation tank, and use an ICP-OES plasma emission spectrometer to detect the element contents of Si, Mo and vanadium; adjust the pH value of the leachate to 10.8 with hydrochloric acid, add calcium chloride powder at a molar ratio of Si to Ca of 1:1.4 at 20°C, stir and mix for 1-2 hours, and the silicon in the leachate forms a precipitate in the form of calcium silicate, filter, and remove the calcium silicate precipitate to obtain a primary filtrate; adjust the pH value of the primary filtrate to 9 with hydrochloric acid, add calcium chloride powder at a molar ratio of Mo to Ca of 1:1.1, convert Na2MoO4 into CaMoO4 precipitate, filter and recover the CaMoO4 precipitate to obtain a secondary filtrate.

[0037] Step 3: 11 kg of polyvinyl pyrrolidone, 3.5 kg of carbon nanotubes and 220 L of N, N-dimethylamide are added to a stirring kettle and stirred for 3.5 hours, and then 16.5 kg of polyaniline, 11.2 kg of 1-butyl-3-methylimidazolium chloride, 5.5 kg of tributyl phosphate and 0.55 kg of cellulose triacetate are added to the reaction kettle, and stirred for 5 hours at 1350 r / min, and vacuum degassed to obtain a composite slurry, and the composite slurry is coated on the surface of a titanium mesh. After the solvent is evaporated, 1-butyl-3-methylimidazolium chloride and the remaining polymers are compositely crystallized and fixed in the polymer matrix to obtain a cathode plate with a 1.2 mm thick conductive coating;

[0038] The secondary filtrate is passed into an electrolytic cell, and the pH value is adjusted to 2.3 with hydrochloric acid. Under this pH condition, Mo and V in the secondary filtrate exist in the form of oxygen-containing cations. The distance between the cathode plate and the anode plate in the electrolytic cell is 6.5 cm, and the anode plate is a titanium-coated ruthenium electrode. The electrolysis treatment is carried out at a current density of 50A / m2 for 2.5 hours to convert MoO22+ into MoO3 and capture it. Then, the secondary filtrate after the electrolysis treatment is transferred to a sedimentation tank and hydrolyzed at 65°C for 7 hours to convert VO2+ into V2O5 by hydrolysis. The V2O5 precipitate is filtered and recovered, and the filtered tail liquid is passed into a sewage pool for environmental protection treatment.

[0039] After detection by plasma emission spectrometer ICP-OES, the recovery rate of vanadium was 94.4%, and the purity of V2O5 was 99.7%; the recovery rate of molybdenum was 95.5%, and the purity of CaMoO4 was 98.4%.

[0040] Example 3: This example provides a wet recovery process for titanium, vanadium and molybdenum in a waste SCR denitration catalyst, comprising the following steps:

[0041] Step 1: Disassemble the SCR denitration catalyst module, collect the denitration catalyst body, use compressed air to blow away the fly ash on the denitration catalyst body, then crush it, and use a planetary ball mill to grind it into a 300-mesh powder; add the powder and a 50g / L sodium hydroxide solution in a mass ratio of 1:3 into a leaching tank, stir and mix, add 6% hydrogen peroxide by mass of the powder, alkali leaching at 100°C for 3h, filter, and obtain a leachate containing vanadium and molybdenum and titanium-rich slag;

[0042] The titanium-rich slag was vacuum dried and mixed with deionized water in a mass ratio of 1:3, and then the pH value was adjusted to 4 with a 1 mol / L sulfuric acid solution. The mixture was stirred at 25°C for 8 h, filtered, washed with water, and dried, and calcined at 550°C for 5 h to obtain a TiO2 product.

[0043] Step 2: Transfer the leachate to a sedimentation tank, and use an ICP-OES plasma emission spectrometer to detect the element contents of Si, Mo and vanadium; adjust the pH value of the leachate to 11 with hydrochloric acid, add calcium chloride powder at a molar ratio of Si to Ca of 1:1.5 at 25°C, stir and mix for 2 hours, and the silicon in the leachate forms a precipitate in the form of calcium silicate. Filter and remove the calcium silicate precipitate to obtain a primary filtrate; adjust the pH value of the primary filtrate to 9 with hydrochloric acid, add calcium chloride powder at a molar ratio of Mo to Ca of 1:1.2, convert Na2MoO4 into CaMoO4 precipitate, filter and recover the CaMoO4 precipitate to obtain a secondary filtrate.

[0044] Step 3: Add 12.5 kg of polyvinyl pyrrolidone, 4 kg of carbon nanotubes and 250 L of N, N-dimethylamide into a stirring kettle and stir for 4 hours, then add 18 kg of polyaniline, 12.5 kg of 1-butyl-3-methylimidazolium chloride, 6 kg of tributyl phosphate and 0.6 kg of cellulose triacetate into the reaction kettle, stir for 6 hours at 1500 r / min, and vacuum degas to obtain a composite slurry, and apply the composite slurry on the surface of the titanium mesh. After the solvent is evaporated, 1-butyl-3-methylimidazolium chloride and the remaining polymers are compositely crystallized and fixed in the polymer matrix to obtain a cathode plate with a 1.5 mm thick conductive coating;

[0045] The secondary filtrate is passed into an electrolytic cell, and the pH value is adjusted to 2.5 with hydrochloric acid. Under this pH condition, Mo and V in the secondary filtrate exist in the form of oxygen-containing cations. The distance between the cathode plate and the anode plate in the electrolytic cell is 8 cm, and the anode plate is a titanium-coated ruthenium electrode. The electrolysis treatment is carried out at a current density of 60A / m2 for 3 hours to convert MoO22+ into MoO3 and capture it. Then, the secondary filtrate after the electrolysis treatment is transferred to a sedimentation tank and hydrolyzed at 70°C for 8 hours to convert VO2+ into V2O5 by hydrolysis. The V2O5 precipitate is filtered and recovered, and the filtered tail liquid is passed into a sewage pool for environmental protection treatment.

[0046] After detection by plasma emission spectrometer ICP-OES, the recovery rate of vanadium was 94.8%, and the purity of V2O5 was 99.8%; the recovery rate of molybdenum was 95.8%, and the purity of CaMoO4 was 97.9%.

[0047] Comparative Example 1: Based on Example 3, 1-butyl-3-methylimidazole chloride is not added when preparing the cathode plate in step 3, and the other steps remain unchanged to complete the wet recovery process of titanium, vanadium and molybdenum.

[0048] After detection by plasma emission spectrometer ICP-OES, the recovery rate of vanadium was 94.6%, and the purity of V2O5 was 96.3%; the recovery rate of molybdenum was 95.3%, and the purity of CaMoO4 was 97.7%.

[0049] Comparative Example 2: Based on Example 3, during the primary filtrate treatment, calcium chloride powder was added in an amount with a molar ratio of Mo to Ca of 1:1.5, and the other steps remained unchanged to complete the wet recovery process of titanium, vanadium and molybdenum.

[0050] After detection by plasma emission spectrometer ICP-OES, the recovery rate of vanadium was 93.8%, and the purity of V2O5 was 99.6%; the recovery rate of molybdenum was 95.5%, and the purity of CaMoO4 was 95.2%.

[0051] Comparative Example 3: Based on Example 3, during the primary filtrate treatment, calcium chloride powder was added in an amount with a molar ratio of Mo to Ca of 1:0.7, and the other steps remained unchanged to complete the wet recovery process of titanium, vanadium and molybdenum.

[0052] After detection by plasma emission spectrometer ICP-OES, the recovery rate of vanadium was 94.7%, and the purity of V2O5 was 98.5%; the recovery rate of molybdenum was 93.2%, and the purity of CaMoO4 was 98.0%.

[0053] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A wet recovery process for titanium, vanadium and molybdenum in waste SCR denitration catalyst, characterized in that: The steps include: Step 1: Disassemble the SCR denitration catalyst module, collect the denitration catalyst body, blow off the soot, crush, and ball-mill into 200-300 mesh powder, alkali-leach the powder, filter, and obtain the leaching solution containing vanadium and molybdenum and titanium-rich slag, and the titanium-rich slag is used to produce TiO2 products; Step 2: The leachate is transferred to a sedimentation tank, pre-impurified to remove calcium silicate precipitate, and a primary filtrate is obtained, and the pH value is adjusted to 9 with hydrochloric acid, and calcium chloride powder is added in an amount according to a molar ratio of Mo to Ca of 1:1-1.2, and the CaMoO4 precipitate is recovered by filtration to obtain a secondary filtrate; Step 3: Pass the secondary filtrate into the electrolytic cell, adjust the pH value to 2-2.5 with hydrochloric acid, the distance between the cathode plate and the anode plate in the electrolytic cell is 5-8 cm, and the current is 40-60A / m 2 The electrolysis treatment is carried out at a current density of 2-3 hours, and then the secondary filtrate after the electrolysis treatment is transferred to a sedimentation tank, hydrolyzed at 60-70°C for 6-8 hours, and the V2O5 precipitate is filtered and recovered. The filtered tail liquid is passed into a sewage pool for environmental protection treatment, completing the wet recovery process of titanium, vanadium and molybdenum; The cathode plate is prepared by the following steps: The composite slurry containing 1-butyl-3-methylimidazolium chloride is coated on the surface of the titanium mesh, and after the solvent is volatilized, it is dried to obtain a cathode plate with a conductive coating layer of 1-1.5 mm thickness.

2. The wet recovery process of titanium, vanadium and molybdenum in a waste SCR denitration catalyst according to claim 1, characterized in that: The composite slurry is prepared by the following steps: Add polyvinyl pyrrolidone, carbon nanotubes and N,N-dimethylamide into a stirring kettle and stir for 3-4 hours. Then add polyaniline, 1-butyl-3-methylimidazole chloride, tributyl phosphate and cellulose triacetate into the reaction kettle, stir for 4-6 hours at 1200-1500 r / min, and vacuum degas to obtain a composite slurry.

3. The wet recovery process of titanium, vanadium and molybdenum in a waste SCR denitration catalyst according to claim 2, characterized in that: The dosage ratio of the polyvinyl pyrrolidone, carbon nanotubes, N,N-dimethylamide, polyaniline, 1-butyl-3-methylimidazole chloride, tributyl phosphate and cellulose triacetate is 10-12.5g: 3-4g: 200-250mL: 15-18g: 10-12.5g: 5-6g: 0.5-0.6g.

4. The wet recovery process of titanium, vanadium and molybdenum in a waste SCR denitration catalyst according to claim 1, characterized in that: The specific method of the powder alkali leaching is as follows: The powder and a sodium hydroxide solution with a concentration of 50-150 g / L are added into a leaching tank in a mass ratio of 1:3, and after stirring and mixing, an oxidant with a mass percentage of 3-6% of the powder is added, and alkaline leaching is performed at 40-100° C. for 1-3 hours.

5. The wet recovery process of titanium, vanadium and molybdenum in a waste SCR denitration catalyst according to claim 4, characterized in that: The oxidant is hydrogen peroxide.

6. The wet recovery process of titanium, vanadium and molybdenum in a waste SCR denitration catalyst according to claim 1, characterized in that: The anode plate is a titanium-coated ruthenium electrode.

7. The wet recovery process of titanium, vanadium and molybdenum in a waste SCR denitration catalyst according to claim 1, characterized in that: The method for producing the TiO2 product is as follows: The titanium-rich slag is vacuum dried and mixed with deionized water in a mass ratio of 1:3, and the pH value is adjusted to 2-4 with a 1 mol / L sulfuric acid solution. The mixture is stirred at 20-25°C for 5-8 hours, filtered, washed with water, and dried, and calcined at 550°C for 3-5 hours to obtain a TiO2 product.

8. The wet recovery process of titanium, vanadium and molybdenum in a waste SCR denitration catalyst according to claim 1, characterized in that: The specific method of the pre-impurity removal process is as follows: The pH value of the leaching solution is adjusted to 10.5-11 with hydrochloric acid, and calcium chloride powder is added at a molar ratio of Si to Ca of 1:1.3-1.5 at 15-25°C, and the mixture is stirred for 1-2 hours, filtered, and the filtrate is collected to complete the pre-impurity removal treatment.