Iron-based resistance alloy and preparation method and application thereof

Through Fe55-63 wt%, Cr13-17 wt%, Co20-26 wt%, W1-12 wt%, Vacuum-induced magnetic levitation smelting and homogenization treatment, the problem of high resistance temperature coefficient of the resistance alloy is solved, and the resistance alloy is realized The combination of high resistivity and low resistance temperature coefficient is suitable for precision sensors, reducing production costs and improving processability.

CN119020703AInactive Publication Date: 2024-11-26SHAANXI SCI TECH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410819753.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The current resistance alloy has a high resistance temperature coefficient within the room temperature range and above, which limits the development of high-precision precision electronic products, and has high production costs and poor processability.

Method used

The iron-based resistance alloy of Fe55-63 wt%, Cr13-17 wt%, Co20-26 wt%, W1-12 wt%, prepared by vacuum induction magnetic levitation smelting, casting and homogenization treatment, and W elements are added to increase the resistivity and reduce the resistance. Temperature coefficient.

Benefits of technology

The prepared iron-based resistive alloy has high resistivity and low resistance temperature coefficient. It is suitable for precision resistive strain sensors, meeting the intelligent needs of health inspection, structural inspection and automobile fields, with low cost and good processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020703A_ABST
    Figure CN119020703A_ABST
Patent Text Reader

Abstract

The invention discloses an iron-based resistance alloy and a preparation method and application thereof, and belongs to the technical field of alloy materials. The iron-based resistance alloy is composed of the following components in percentage by mass: 55-63 wt% of Fe, 13-17 wt% of Cr, 20-26 wt% of Co and 1-12 wt% of W, totaling 100%. The iron-based resistance alloy is prepared by carrying out vacuum induction magnetic levitation smelting, casting and homogenization treatment on Fe, Cr, Co and W metal materials. The iron-based resistance alloy provided by the invention has high resistivity and low resistance temperature coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alloy materials, and more specifically to an iron-based resistance alloy and a preparation method and application thereof. Background Art

[0002] High resistance alloys are a type of resistance alloy with high resistivity (≥100μΩ·cm) and low temperature coefficient of resistance (TCR). They are also the core parts of resistive sensors used in aerospace, defense, automotive electronics, mechanical equipment and industrial automatic control. Although alloys of NiCr and NiCrAl systems have good high temperature strength and plasticity, they have low resistivity and high production costs. The plasticity of FeCrAl alloys is poor, which limits their further application areas. The Al reported by researchers 2.08 CoCrFeNi high entropy alloy has high resistivity, but high resistivity and temperature coefficient of resistivity in the range of 4.2-360 K. With the growing industrial development, there is an urgent need for a resistance alloy with low cost, simple preparation, high resistivity, low temperature coefficient of resistivity and good processability.

[0003] FeCrCo alloy has excellent plasticity and machinability, and can be processed into wires, tubes, bars and strips. However, researchers have mainly conducted detailed research on the magnetic properties of FeCrCo alloys, and there are few studies on the electrical properties of FeCrCo alloys. However, with the development of industry, the market demand for intelligent, precise and miniaturized electronic devices is becoming increasingly strong, which requires the development of resistance alloys with excellent electrical properties and good machinability. The literature reports that the resistivity of FeCrCo alloy at room temperature is 90μΩ·cm and the resistance temperature coefficient is 2.6ppm / K. It has a low resistance temperature coefficient, but the resistivity is slightly low. If the resistivity can be increased while still maintaining a low resistance temperature coefficient, this type of resistance alloy will have great development potential.

[0004] Scholars have conducted in-depth theoretical and experimental research on the design of material composition, preparation process and performance regulation, and have developed a number of resistance alloys with excellent performance. For example, Yih-Farn Kao et al. x The electrical properties of the cast (Ax), homogeneous (Hx) and deformed (Dx) CoCrFeNi high entropy alloy at temperatures of 4.2K to 300K show that although the alloy has a high resistivity, fluctuating between 100 and 220μΩ·cm, the temperature coefficient of resistance of the alloy is large, and the minimum temperature coefficient of resistivity is also higher than 80ppm / K.

[0005] M.Egilmez et al. studied Fe 40 Mn 40 Co10 Cr 10 The electrical properties of the alloy are as follows: the resistivities of the undeformed alloy sample (U), the alloy sample deformed at room temperature (D-RT) and the alloy sample deformed under liquid nitrogen (D-LN) are 34μΩ·cm, 38μΩ·cm and 44μΩ·cm, respectively. The alloy has low resistivity and large temperature coefficient of resistance.

[0006] Current research shows that although the resistivity of resistance alloys has increased, the resistance temperature coefficient is still high, which restricts the further development of high-precision precision electronic products. In short, the development of precision resistance alloys with high resistivity and low resistance temperature coefficient at room temperature and above is a severe technical challenge currently faced. Summary of the invention

[0007] In view of the above problems, the present invention provides an iron-based resistance alloy and a preparation method and application thereof. The prepared iron-based resistance alloy has high resistivity and low resistance temperature coefficient.

[0008] The first object of the present invention is to provide an iron-based resistance alloy, which is composed of the following components in mass percentage: Fe55-63wt%, Cr13-17wt%, Co20-26wt%, W1-12wt%, totaling 100%;

[0009] The preparation of the iron-based resistance alloy is obtained by subjecting Fe, Cr, Co, and W metal materials to vacuum induction magnetic levitation melting, casting, and homogenization treatment.

[0010] For example, the mass percentage of Fe in the iron-based resistance alloy is 55wt%, 56wt%, 57wt%, 58wt%, 59wt%, 60wt%, 61wt%, 62wt%, 63wt%, etc.;

[0011] The mass percentage of Cr in the iron-based resistance alloy is 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, etc.;

[0012] The mass percentage of Co in the iron-based resistance alloy is 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, etc.;

[0013] The mass percentage of W in the iron-based resistance alloy is 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, etc.;

[0014] However, it is not limited to the listed values. Other values ​​not listed within the above numerical range are also applicable and will not be detailed here.

[0015] In a preferred embodiment of the present invention, the iron-based resistance alloy consists of the following components in percentage by mass: Fe 56.5wt%, Cr 14wt%, Co 23wt%, and W 6.5wt%.

[0016] A second object of the present invention is to provide a method for preparing an iron-based resistance alloy, comprising the following steps:

[0017] The Fe, Cr, Co and W metal materials are uniformly mixed and then subjected to vacuum induction magnetic levitation melting, and then cast to obtain an alloy ingot;

[0018] Under the protection of inert gas, the alloy is homogenized to obtain the iron-based resistance alloy.

[0019] In a preferred embodiment of the present invention, the vacuum melting temperature is 1773-1975 K. For example, the vacuum melting temperature is 1773 K, 1793 K, 1805 K, 1825 K, 1845 K, 1865 K, 1885 K, 1905 K, 1925 K, 1945 K, 1975 K, etc., but it is not limited to the listed values, and other values ​​not listed in the above range are also applicable, which will not be repeated here.

[0020] In a preferred embodiment of the present invention, the melting times are 4-6 times, for example, 4 times, 5 times or 6 times.

[0021] In a preferred embodiment of the present invention, the casting temperature is 1873-1973K, for example, the casting temperature is 1873K, 1893K, 1913K, 1933K, 1953K, 1973K, etc.; but it is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable, which will not be repeated here.

[0022] In a preferred embodiment of the present invention, the homogenization temperature is 1473-1573K and the time is 2-3h.

[0023] For example, the homogenization treatment temperature is 1473K, 1493K, 1513K, 1533K, 1553K, 1573K, etc.; the time is 2h, 2.5h, 3h, etc., but it is not limited to the listed values. Other unlisted values ​​within the above numerical range are also applicable and will not be repeated here.

[0024] More preferably, the homogenization temperature is 1473 K and the time is 2 h.

[0025] The third object of the present invention is to use the iron-based resistance alloy in precision resistive strain sensors to meet the needs of intelligence in fields such as health detection, structural detection, electronic products and automobiles.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention adds W element when preparing the iron-based resistance alloy. When the W element is dissolved in the FeCrCo alloy, it will cause more lattice distortion, enhance electron scattering, increase the resistivity of the iron-based resistance alloy, and reduce the resistance temperature coefficient. Then, the vacuum melting method is adopted for preparation, and the element distribution of the prepared iron-based resistance alloy is relatively uniform. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is the XRD spectrum of the alloy of Example 1;

[0029] Figure 2 The scanning electron microscope morphology (a) and the X-ray energy spectrum (EDS) scan of Fe (b), Co (c), Cr (d) and W (e) of the alloy in Example 1 are shown;

[0030] Figure 3 This is the tensile curve diagram of the alloy of Example 1;

[0031] Figure 4 is the XRD spectrum of the alloy of Example 2;

[0032] Figure 5 The scanning electron microscope morphology (a) and the X-ray energy spectrum (EDS) scan of Fe (b), Co (c), Cr (d) and W (e) of Example 2;

[0033] Figure 6 is the tensile curve diagram of Example 2;

[0034] Figure 7 is the XRD spectrum of Example 3;

[0035] Figure 8 The scanning electron microscope morphology (a) and the X-ray energy spectrum (EDS) scan of Fe (b), Co (c), Cr (d) and W (e) of Example 3;

[0036] Fig. 9 It is a transmission electron microscope (TEM) analysis diagram of Example 3, wherein Figure a is a high-angle annular dark field image of the precipitated phase Fe2W, Figure b is a Fe element distribution diagram, Figure c is a Cr element distribution diagram, Figure d is a Co element distribution diagram, Figure e is a W element distribution diagram, Figure f is a bright field image of the precipitated phase Fe2W, Figure g is a diffraction analysis diagram of the precipitated phase Fe2W, Figure h is a point scan energy spectrum analysis diagram of the precipitated phase, and Figure i is a Fourier change image and an inverse Fourier change image of the Fe2W type Laves precipitate phase and the matrix BCC phase;

[0037] Fig.10 is the tensile curve diagram of Example 3;

[0038] Fig.11 It is the XRD spectrum of comparative example 1;

[0039] Fig.12 The scanning electron microscope morphology (a) and the X-ray energy spectrum (EDS) scan of Fe (b), Cr (c), Co (d) and W (e) of the alloy in comparative example 1 are shown;

[0040] Fig.13 This is the tensile curve of the alloy of Comparative Example 1. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] In order to develop a precision resistance alloy with high resistivity and low resistance temperature coefficient at room temperature and above, the present invention provides an iron-based resistance alloy and a preparation method and application thereof, and the specific technical scheme is as follows:

[0043] An iron-based resistance alloy, the iron-based resistance alloy is composed of the following components in mass percentage: Fe55-63wt%, Cr13-17wt%, Co20-26wt%, W1-12wt%, totaling 100%;

[0044] The preparation of the iron-based resistance alloy is obtained by subjecting Fe, Cr, Co, and W metal materials to vacuum induction magnetic levitation melting, casting, and homogenization treatment.

[0045] The present invention adds W element during preparation, and based on quantum mechanics, it is proved that resistivity is the average effect of the statistics of the action of electrons and phonons. According to the band theory, it is believed that electrons move in a strict periodic potential field, and the movement of electrons will not be affected by any "resistance". Only when factors such as atomic vibration or impurity defects cause the crystal potential field to deviate from the periodic potential field, collision scattering will occur in the movement of electrons. The resistance of general metals is caused by the scattering of electrons by lattice atomic vibration (phonon). Since the atomic radius of the W element is much larger than the atomic radius of Fe, Cr, and Co elements, when the W element is dissolved in the FeCrCo alloy, more lattice distortion will be caused, which will aggravate electron scattering and cause the resistivity of the alloy to increase. The present invention adopts vacuum melting method for preparation, and the prepared iron-based resistance alloy element distribution is relatively uniform.

[0046] The raw materials used in the present invention are small pure metal particles of iron, chromium, cobalt and tungsten with a purity greater than 99.90%, which are purchased from Beijing Yanbang New Material Technology Co., Ltd.

[0047] When W element is added to a certain amount, W element combines with Fe element to form a metal compound Fe2W phase. Therefore, the iron-based resistance alloy prepared by adding W element to FeCrCo alloy has high resistivity and low resistance temperature coefficient, which not only expands the practical application of FeCrCo alloy, but also provides a certain technical breakthrough for the development of resistance alloy with high cost performance, high resistivity and low resistance temperature coefficient within a certain temperature range.

[0048] In a preferred embodiment of the present invention, the composition is composed of the following components in mass percentage: Fe 56.5wt%, Cr 14wt%, Co 23wt%, W 6.5wt%,

[0049] The present invention provides a method for preparing the above-mentioned iron-based resistance alloy, comprising the following steps:

[0050] Weigh the following components by weight respectively: 55-63wt% Fe, 13-17wt% Cr, 20-26wt% Co, and 1-12wt% W; mix Fe, Cr, Co, and W metal materials uniformly, perform vacuum induction magnetic suspension melting, and then cast to obtain an alloy ingot;

[0051] Under the protection of inert gas, the alloy is homogenized to obtain the iron-based resistance alloy.

[0052] In a preferred embodiment of the present invention, the vacuum melting temperature is 1773-1975K and the vacuum degree is 10 -3 Pa; When the temperature of vacuum induction magnetic levitation melting is too high or too low, new phases may be generated in the alloy, and the mechanical and electrical properties of the alloy will be affected after the structure changes.

[0053] In a preferred embodiment of the present invention, the melting times are 4 to 6. When the melting times are too few, the elements in the alloy are unevenly distributed, and when the melting times are too many, energy is consumed and new phases may be easily generated, thereby affecting the mechanical and electrical properties of the alloy.

[0054] In a preferred embodiment of the present invention, the casting temperature is 1873-1973 K. If the casting temperature is too low, there will be too many defects in the alloy, forming an uneven structure and reducing the performance of the alloy.

[0055] In a preferred embodiment of the present invention, the homogenization temperature is 1473-1573K and the time is 2-3h. If the homogenization temperature is too short, the alloy defects will be more and the element distribution will be uneven; if the time is too short, the purpose of uniform distribution of elements cannot be achieved, and if the time is too long, new phases are likely to be generated.

[0056] More preferably, the homogenization temperature is 1473 K and the time is 2 h.

[0057] The vacuum induction magnetic levitation melting furnace used in the present invention was purchased from Hefei Kejing Material Technology Co., Ltd., model AM800-3, and the homogenization treatment was carried out in a box furnace with model KSL-1800x-A1-W.

[0058] Example 1

[0059] Step 1: According to the chemical formula Fe 61.2 Cr 15.3 Co 23.1 W 2.5 (mass percentage) for batching, the raw materials use metal particles corresponding to the purity of each element greater than 99.90%;

[0060] Step 2: Use vacuum induction magnetic levitation melting furnace for melting, and wait until the vacuum degree reaches 10 -3 After 300 Pa, argon gas was filled in until the pressure returned to normal (i.e. 0Pa), the melting temperature was 1773K, the melting was repeated 6 times, and the rectangular alloy ingot was cast at 1873K;

[0061] Step 3: After obtaining the smelted ingot, the alloy is homogenized in an argon protective atmosphere at a temperature of 1473K for 2 hours, and then cooled in the furnace to obtain an iron-based resistance alloy, which is recorded as Fe 61.7 Cr 15.3 Co 23.1 W 2.5 alloy.

[0062] Example 2

[0063] Step 1: According to the chemical formula Fe 56.5 Cr 14 Co 23 W 6.5 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.90%;

[0064] Step 2: Use a vacuum induction magnetic levitation melting furnace (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After 300 Pa, argon gas was filled in until the pressure returned to normal (i.e., 0 Pa), the melting temperature was 1773 K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873 K;

[0065] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a temperature of 1473K for 2 hours. The iron-based resistance alloy is obtained by cooling the ingot, which is recorded as Fe 56.5 Cr 14 Co 23 W 6.5 alloy.

[0066] Example 3

[0067] Step 1: According to the chemical formula Fe 56.3 Cr 16.3 Co 24.0 W 10.5 (mass percentage) for batching, the raw materials use small particles corresponding to the purity of each element greater than 99.90%;

[0068] Step 2: Use vacuum induction magnetic levitation melting furnace for melting, and wait until the vacuum degree reaches 10 -3 After 300 Pa, argon gas was filled in until the pressure returned to normal (i.e. 0Pa), the melting temperature was 1773K, the melting was repeated 6 times, and the rectangular alloy ingot was cast at 1873K;

[0069] Step 3: After obtaining the smelted ingot, the alloy is homogenized in an argon protective atmosphere at a temperature of 1473K for 2 hours, and then cooled in the furnace to obtain an iron-based resistance alloy, which is recorded as Fe 56.3 Cr 16.3 Co 24.0 alloy;

[0070] Example 4

[0071] Step 1: According to the chemical formula Fe 55 Cr 13 Co 20 W 12 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.90%;

[0072] Step 2: Use a vacuum induction magnetic levitation melting furnace (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After 300 Pa, argon gas was filled in until the pressure returned to normal (i.e. 0Pa), the melting temperature was 1975K, the melting was repeated 6 times, and the rectangular alloy ingot was cast at 1973K;

[0073] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a temperature of 1573K for 2 hours. The iron-based resistance alloy is obtained by cooling the ingot, which is recorded as Fe 55 Cr 13 Co 20 W 12 alloy.

[0074] Example 5

[0075] Step 1: According to the chemical formula Fe 63 Cr 13 Co 20 W4 (mass percentage) is used for batching, and the raw materials use blocks corresponding to the purity of each element greater than 99.90%;

[0076] Step 2: Use a vacuum induction magnetic levitation melting furnace (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After 300 Pa, argon gas was filled in until the pressure returned to normal (i.e. 0Pa), the melting temperature was 1865K, the melting was repeated 5 times, and the rectangular alloy ingot was cast at 1950K;

[0077] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a temperature of 1530K for 2.5 hours. The iron-based resistance alloy is obtained by cooling the ingot, which is recorded as Fe 63 Cr 13 Co 20 W4 alloy.

[0078] Example 6

[0079] Step 1: According to the chemical formula Fe 60 Cr 13 Co 26 W1 (mass percentage) is used for batching, and the raw materials use blocks corresponding to the purity of each element greater than 99.90%;

[0080] Step 2: Use a vacuum induction magnetic levitation melting furnace (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After 300 Pa, argon gas was filled in until the pressure returned to normal (i.e. 0Pa), the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1953K;

[0081] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a temperature of 1520K for 3 hours. The iron-based resistance alloy is obtained by cooling the ingot, which is recorded as Fe 60 Cr 13 Co 26 W1 alloy.

[0082] Comparative Example 1

[0083] Step 1: According to the chemical formula Fe 61.2 Cr 15.3 Co 23.1 W 2.5 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.8%;

[0084] Step 2: Use vacuum arc melting to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After 300 Pa, argon gas was filled in until the pressure returned to normal slightly. The melting temperature was 1773K. The melting was repeated 6 times and the rectangular alloy ingot was cast at 1873K.

[0085] Step 3: After obtaining the smelted ingot, the alloy is homogenized in an argon protective atmosphere at a temperature of 1473K for 1 hour, and the iron-based resistance alloy is obtained by cooling in the furnace.

[0086] Next, small cubes were cut out from the iron-based resistance alloys prepared in Examples 1 to 3 and Comparative Example 1 for microstructure observation and performance testing.

[0087] Example 1 Preparation of Fe 61.7 Cr 15.3 Co 23.1 W 2.5 The XRD spectrum of the alloy is as follows Figure 1 As shown. Figure 1 It can be seen from the XRD spectrum that the alloy mainly exhibits a body-centered cubic (BCC) structure.

[0088] Microstructure scanning electron microscope morphology and X-ray energy spectrum (EDS) surface scan, such as Figure 2 shown. Figure 2 The image shows that the W element is evenly distributed in the Fe 61.7 Cr 15.3 Co 23.1 There is no obvious element segregation at the micron level in the alloy.

[0089] Figure 3 Fe 61.2 Cr 15.3 Co23.1 W 2.5 The engineering stress-strain tensile curve of the alloy is given by Figure 3 It can be seen that Fe 61.2 Cr 15.3 Co 23.1 W 2.5 The alloy has a yield strength of 157 MPa, a tensile strength of 738 MPa, and a uniform elongation of 6.8%. 61.2 Cr 15.3 Co 23.1 W 2.5 The resistivity of the alloy is 101 μm·cm, and the temperature coefficient of resistance is -0.0073 ppm / K.

[0090] Example 2 Preparation of Fe 56.5 Cr 14 Co 23 W 6.5 The XRD spectrum of the alloy is as follows Figure 4 As shown. Figure 4 It can be seen from the XRD spectrum that the alloy exhibits a body-centered cubic (BCC) structure, but a small amount of Fe2W-type Laves phase is also produced at 41.1°.

[0091] Microstructure scanning electron microscope morphology and X-ray energy spectrum (EDS) surface scan, such as Figure 5 As shown, Figure 5 The image shows that the W element is evenly distributed in the Fe 61.7 Cr 15.3 Co 23.1 There is no obvious element segregation at the micron level in the alloy.

[0092] Figure 6 Fe 56.5 Cr 14 Co 23 W 6.5 Alloy tensile curve. Figure 6 It can be seen that Fe 56.5 Cr 14 Co 23 W 6.5 The alloy has a yield strength of 185 MPa, a tensile strength of 978 MPa, and a uniform elongation of 13.5%. 56.5 Cr 14 Co 23 W 6.5 The resistivity of the alloy reaches 120μm·cm, and the temperature coefficient of resistance is -0.0073ppm / K.

[0093] Example 3 Preparation of Fe 56.3 Cr 16.3 Co 24.0The XRD spectrum of the alloy is as follows Figure 7 As shown. Figure 7 The XRD spectrum of the alloy showed a body-centered cubic (BCC) structure with a small amount of Fe2W-type Laves phase.

[0094] Microstructure scanning electron microscope morphology and X-ray energy spectrum (EDS) surface scan, such as Figure 8 shown. Figure 8 The image shows that the W element is evenly distributed in the Fe 56.3 Cr 16.3 Co 24.0 There is no obvious element segregation at the micron level in the alloy.

[0095] Fig. 9 FeCrCoW 10.5 TEM characterization of Fe2W type Laves phase in the alloy. Fig. 9 Figure a is a high-angle annular dark field (HAADF) image of the precipitated phase Fe2W. It can be seen that the shape of Fe2W is mostly strip-shaped, with a particle size between 300 and 800 nm. The overall distribution is relatively dispersed, and the spacing between each precipitated phase is large. Fig. 9 Figures b to e are the STEM-EDS surface scan element (Fe, Cr, Co and W elements) distribution diagrams, from which it can be seen that Fe and W elements are relatively enriched.

[0096] Fig. 9 Figure f is the bright field (BF) image of the precipitated phase Fe2W. Fig. 9 The precipitate phase pointed by the yellow arrow in Figure f is subjected to diffraction analysis. The inset in the upper right corner is the calibration of selected area electron diffraction (SAED), as shown in Figure 2. Fig. 9 As shown in the g-graph, it can be determined that the precipitated phase is Fe2W, which is consistent with the XRD test results. At the same time, the precipitated phase (green point) was subjected to point scanning energy spectrum analysis, and it was found that the atomic ratio of Fe and W elements was close to 2:1, as shown in Figure 2. Fig. 9 As shown in the h figure, it is further verified that the precipitated phase is Fe2W type Laves phase. Fig. 9 The i-figure is the Fourier transform image (FFT) and inverse Fourier transform image (IFFT) of the Fe2W type Laves precipitate phase and the matrix BCC phase. It can be seen from the upper right FFT illustration that the orientation of the BCC phase matrix and the precipitate phase is consistent. Due to (110) BCC The interplanar spacing is 0.152nm and (110) Fe2W There is a difference of 0.387nm in the interplanar spacing, which leads to lattice distortion at the grain boundary between the two phases. Fig. 9The yellow square dotted frame part in the i figure is subjected to inverse Fourier transform to obtain the IFFT diagram (see the lower right corner). It can be seen that the precipitated phase and the BCC phase matrix have a typical incoherent interface.

[0097] TEM analysis revealed that Fe 56.3 Cr 16.3 Co 24.0 W 10.5 The Fe2W type Laves precipitated phase in the alloy and the BCC phase matrix are incoherent interfaces, indicating that the corresponding phase boundary bonding is weak. The precipitation of the Laves phase at the grain boundary makes it very susceptible to stress concentration, thus inducing cracking at the grain boundary during deformation. 10.5 The shortest distance between the precipitated phases in the alloy is 236 nm, which is much larger than the mean free path of Fe electrons (116 nm), resulting in weakened electron scattering and making FeCrCoW 10.5 The resistivity of the alloy is significantly reduced. Therefore, FeCrCoW 10.5 The strength and resistivity of the alloy are reduced.

[0098] And according to XRD calculation of the interplanar spacing, it was found that Fe 56.3 Cr 16.3 Co 24.0 W 10.5 The crystal plane constant of the alloy is 0.2880, which is much larger than the lattice constant of the standard BCC phase (0.2866nm), so it is believed that the addition of W element causes lattice distortion. However, the transmission diagram does not indicate that lattice distortion occurs. It is generally believed that lattice distortion will aggravate electron scattering under normal circumstances, but there is no way to confirm electron scattering. Electron scattering is a microscopic phenomenon, and the macroscopic quantity of resistivity is generally used to determine whether the electron scattering of the alloy under the modified composition is severe.

[0099] Fig.10 Fe 56.3 Cr 16.3 Co 24.0 W 10.5 Alloy engineering stress-strain tensile curve, from Fig.10 It can be seen that Fe 56.3 Cr 16.3 Co 24.0 W 10.5 The alloy has a yield strength of 120 MPa, a tensile strength of 882 MPa, and a uniform elongation of 8.5%. 56.3 Cr 16.3 Co 24.0 W 10.5 The resistivity is 114μm·cm and the temperature coefficient of resistance is -0.0051ppm / K.

[0100] Fe obtained in Comparative Example 1 61.7 Cr 15.3 Co 23.1 W 2.5 The XRD spectrum of the alloy is as follows Fig.11 As shown. Fig.11 The XRD spectrum shows that the alloy mainly exhibits a body-centered cubic (BCC) structure. The microstructure scanning electron microscope morphology and X-ray energy spectrum (EDS) surface scan Fig.12 As shown, Fig.12 The image shows that the W element is evenly distributed in the Fe 61.7 Cr 15.3 Co 23.1 There is no obvious element segregation at the micron level in the alloy. Fig.13 Fe 61.7 Cr 15.3 Co 23.1 W 2.5 Alloy tensile curve. Fig.13 It can be seen that Fe 61.7 Cr 15.3 Co 23.1 W 2.5 The alloy has a yield strength of 237 MPa, a tensile strength of 687 MPa, and a uniform elongation of 5.0%. 61.7 Cr 15.3 Co 23.1 W 2.5 The resistivity of the alloy reaches 96 μm·cm, and the temperature coefficient of resistance is -0.045 ppm / K. Compared with Comparative Example 1, the uniform elongation and resistivity of Example 1 are increased by 26% and 5.0%, respectively, and the temperature coefficient of resistance is decreased by 38%, indicating that the elements can be effectively dissolved in the alloy by prolonging the homogenization treatment time, further improving the resistivity and uniform elongation of the alloy and reducing the temperature coefficient of resistance.

[0101] In the paper published by Yin Fuyan et al. in Sensor World, “Japan’s research on high strain sensitivity coefficient strain sensitive materials (Part 1)”, it is shown that FeCr 15 Co 35 The resistivity of the alloy is 90 μm·cm, and the temperature coefficient of resistance is 2.6 ppm / °C. The present invention further increases the resistivity of the alloy and reduces the temperature coefficient of resistance by adding W element.

[0102] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0103] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An iron-based resistance alloy, It is characterized in that The iron-based resistance alloy is composed of the following components in mass percentage: Fe55-63wt%, Cr13-17wt%, Co20-26wt%, W1-12wt%, which is 100% in total; The preparation of the iron-based resistance alloy is obtained by subjecting Fe, Cr, Co, and W metal materials to vacuum induction magnetic levitation melting, casting, and homogenization treatment.

2. An iron-based resistance alloy according to claim 1, It is characterized in that The iron-based resistance alloy consists of the following components in mass percentage: Fe 56.5wt%, Cr 14wt%, Co 23wt%, and W 6.5wt%.

3. A method for preparing an iron-based resistance alloy according to claim 1, The following steps are involved: Weigh the components according to the following mass percentages: Fe 55-63wt%, Cr 13-17wt%, Co 20-26wt%, W 1-12wt%; The Fe, Cr, Co and W metal materials are uniformly mixed and then subjected to vacuum induction magnetic levitation melting, and then cast to obtain an alloy ingot; Under the protection of inert gas, the alloy is homogenized to obtain the iron-based resistance alloy.

4. The method for preparing the iron-based resistance alloy according to claim 3, It is characterized in that The vacuum melting temperature is 1773-1975K.

5. The method for preparing the iron-based resistance alloy according to claim 3, It is characterized in that The smelting times are 4-6 times.

6. The method for preparing the iron-based resistance alloy according to claim 3, It is characterized in that The casting temperature is 1873-1973K.

7. The method for preparing the iron-based resistance alloy according to claim 3, It is characterized in that The homogenization temperature is 1473-1573K and the time is 2-3h.

8. The method for preparing the iron-based resistance alloy according to claim 7, It is characterized in that The homogenization temperature is 1473K and the time is 2h.

9. Use of the iron-based resistance alloy according to claim 1 or 2 in the preparation of a precision resistive strain sensor.

Citation Information

Patent Citations

  • Thin strip of permanent magnet and manufacture thereof

    JP1984061004A

  • Manufacture of alloy for strain gauge and strain gauge itself

    JP1986015914A