Voltage-withstanding tantalum capacitor and preparation method of voltage-withstanding dielectric layer of voltage-withstanding tantalum capacitor

By applying a high voltage and a high current density to form a voltage withstand dielectric layer, the problem of insufficient voltage withstandability of tantalum capacitors in the prior art is solved, and the voltage withstandability and reliability of the capacitor are significantly improved.

CN119028737APending Publication Date: 2024-11-26CHINA ZHENHUA GRP XINYUN ELECTRONICS COMP ANDDEV CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411351448.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing chip solid electrolyte tantalum capacitors have insufficient voltage withstandability, especially in miniaturized and lightweight designs, the formation voltage is only 2 to 3 times the rated voltage, resulting in insufficient voltage withstandability.

Method used

The tantalum core is formed at a specific voltage and current density to form a voltage-withstanding dielectric layer, including the application of high voltage and high current density, to form an oxide film, and to enhance the formation of the dielectric layer by spraying, washing and cooling steps.

Benefits of technology

The voltage withstandability of the capacitor is significantly improved, especially for chip solid electrolyte tantalum capacitors with voltages less than 3 times, which enhances its voltage withstandability and reliability and expands its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005062479050000061
    Figure BDA0005062479050000061
  • Figure BDA0005062479050000071
    Figure BDA0005062479050000071
  • Figure BDA0005062479050000072
    Figure BDA0005062479050000072
Patent Text Reader

Abstract

The invention discloses a voltage-withstanding tantalum capacitor and a preparation method of a voltage-withstanding dielectric layer of the voltage-withstanding tantalum capacitor. According to the method, the voltage-resistant dielectric layer can be generated on the surface of the tantalum core, the dielectric layer is an oxidation film, and the voltage-resistant capability of the capacitor is greatly improved by generating the dielectric oxidation film. Especially for the chip-type solid electrolyte tantalum capacitor of which the formation voltage is lower than 3 times of the rated voltage, the preparation method of the dielectric oxide film can improve the voltage endurance capability of the chip-type solid electrolyte tantalum capacitor. The method can be used for manufacturing the chip-type solid electrolyte tantalum capacitor with strong voltage endurance capability and high reliability, and is beneficial to expanding the application range of the chip-type solid electrolyte tantalum capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electronic component manufacturing, and in particular relates to a method for preparing a voltage-resistant tantalum capacitor and a voltage-resistant dielectric layer thereof. Background Art

[0002] The withstand voltage of chip-type solid electrolyte tantalum capacitors is primarily determined by the thickness of the dielectric oxide film, which in turn is determined by the voltage generated during the formation process. Theoretically, for chip-type solid electrolyte tantalum capacitors of the same specifications, the higher the formation voltage, the better the withstand voltage. However, with the miniaturization and lightweighting of chip tantalum capacitors, product design has become increasingly extreme. The formation voltage of some tantalum capacitors is only 2 to 3 times the rated voltage, resulting in insufficient withstand voltage. Therefore, a method for improving the withstand voltage of capacitors is needed.

[0003] Patent document No. CN117711825A discloses an ultra-high voltage and high reliability chip tantalum capacitor, comprising an anode tantalum core, a tantalum wire, a cathode connector, an insulating layer, a lead frame cathode bonding surface, a lead frame positive support, and an epoxy resin encapsulated in the outer layer of the ultra-high voltage and high reliability chip tantalum capacitor; its manufacturing method is as follows: according to the working state involving the anode, tantalum powder is formed and pressed and then sintered at high temperature to obtain a tantalum block; the tantalum block is electrochemically increased to form a tantalum pentoxide dielectric oxide film; the formed tantalum block is immersed in a manganese nitrate solution and decomposed at high temperature, and a manganese dioxide layer is filled inside and coated on the surface, and then an auxiliary material is coated on the surface to achieve cathode lead-out. However, the electrolyte additives of this application are different from those of the invention, and the processing method is also different from that of this application. Summary of the Invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a voltage-resistant tantalum capacitor and a voltage-resistant dielectric layer thereof.

[0005] The present invention is achieved through the following technical solutions.

[0006] The present invention provides a method for preparing a pressure-resistant dielectric layer, which includes placing a tantalum core used for capacitor preparation under corresponding voltage and current density to form the pressure-resistant dielectric layer.

[0007] The process of placing the tantalum core under corresponding voltage and current density to form a pressure-resistant dielectric layer includes the following steps:

[0008] 1) Place the tantalum core into a forming tank with an electrolyte and apply the corresponding voltage and current density;

[0009] 2) spraying and boiling the tantalum core after step 1);

[0010] 3) The tantalum core after boiling and washing is cooled, and then repaired according to the original forming process. After the repair is completed, spray and boil and wash according to step 2).

[0011] Preferably, the tantalum core in step 1) includes a tantalum core before, during or after normal formation, the electrolyte includes deionized water, boric acid and sodium tetraborate, and the preparation and use steps of the electrolyte include: adding boric acid and sodium tetraborate into deionized water and completely dissolving them to obtain an electrolyte.

[0012] Preferably, in step 1), the tantalum core is placed in the electrolyte when the electrolyte temperature reaches T and the conductivity is D.

[0013] Preferably, the tantalum core is placed in the electrolyte when the ionic water conductivity is less than 0.8 μS / cm, the electrolyte temperature is 10-75° C., and the conductivity is 1000-2000 μS / cm.

[0014] Preferably, in step 1), after the tantalum core is placed in the electrolyte, the power supply is turned on to boost the voltage, and the voltage is set to U and the current density is I d After that, keep constant voltage for time t1, then turn off the power and take out the tantalum core.

[0015] Preferably, the voltage is 2 to 3 times the forming voltage, the current density is 500 to 1000 mA / g, and the constant voltage is maintained for 2 to 5 minutes.

[0016] Preferably, the spraying time in step 2) is 5 to 8 minutes, and then the product is placed in a boiling and washing tank for boiling and washing, the boiling and washing tank temperature is 80 to 90° C., and the boiling and washing time is 60 to 70 minutes.

[0017] Preferably, after the boiling and washing in step 3) is completed, the tantalum core is placed in the air for natural cooling, and the cooling time is ≥10 minutes.

[0018] A tantalum capacitor prepared by the method.

[0019] The beneficial effects of the present invention are:

[0020] The method of the present invention can generate a pressure-resistant dielectric layer on the surface of a tantalum core. This dielectric layer is an oxide film. The dielectric oxide film preparation method forms a highly pressure-resistant protective layer on the surface of the tantalum anode block. This method uses high voltage and high current density to rapidly form the dielectric oxide film on the surface of the tantalum anode block. The high voltage used is 1.5 to 3 times higher than the formation voltage of the capacitor tantalum core itself.

[0021] By forming this dielectric oxide film, the capacitor's withstand voltage is significantly improved. The dielectric oxide film preparation method of the present invention can improve the withstand voltage of chip-type solid electrolyte tantalum capacitors, particularly those with a formed voltage less than three times the rated voltage. This method can be used to manufacture chip-type solid electrolyte tantalum capacitors with strong withstand voltage and high reliability, thus expanding the application range of chip-type solid electrolyte tantalum capacitors. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.

[0023] Example 1:

[0024] A method for preparing a pressure-resistant dielectric layer, wherein a tantalum core is placed under corresponding voltage and current density to form the pressure-resistant dielectric layer, comprises the following steps:

[0025] 1) Place the tantalum core into a forming tank with an electrolyte and apply the corresponding voltage and current density;

[0026] 2) spraying and boiling the tantalum core after step 1);

[0027] 3) The tantalum core after boiling and washing is cooled, and then repaired according to the original forming process. After the repair is completed, spray and boil and wash according to step 2).

[0028] The tantalum core in step 1) is a tantalum core after formation, the electrolyte is deionized water, boric acid and sodium tetraborate, and the preparation and use steps of the electrolyte include: adding boric acid and sodium tetraborate into deionized water and completely dissolving them to obtain the electrolyte.

[0029] The tantalum core is placed in the electrolyte when the ion water conductivity is less than 0.8 μS / cm, the electrolyte temperature is 10-75° C., and the conductivity is 1000-2000 μS / cm.

[0030] In the step 1), after placing the tantalum core in the electrolyte, the power supply is turned on to boost the voltage, and the voltage is set to 2 times the formation voltage, the current = (number of cores × current density), and after the current density reaches 500mA / g, the constant voltage is maintained for 2 minutes, and then the power supply is turned off and the tantalum core is taken out.

[0031] The spraying time in step 2) is 5 minutes, and then the product is placed in a boiling and washing tank for boiling and washing. The boiling and washing tank temperature is 80° C. and the boiling and washing time is 60 minutes.

[0032] After the boiling and washing in step 3) is completed, the tantalum core is placed in the air for natural cooling, and the cooling time is 15 minutes.

[0033] Example 2:

[0034] A method for preparing a pressure-resistant dielectric layer, wherein a tantalum core is placed under corresponding voltage and current density to form the pressure-resistant dielectric layer, comprises the following steps:

[0035] 1) Place the tantalum core into a forming tank with an electrolyte and apply the corresponding voltage and current density;

[0036] 2) spraying and boiling the tantalum core after step 1);

[0037] 3) The tantalum core after boiling and washing is cooled, and then repaired according to the original forming process. After the repair is completed, spray and boil and wash according to step 2).

[0038] The tantalum core in step 1) is a tantalum core after formation, the electrolyte is deionized water, boric acid and sodium tetraborate, and the preparation and use steps of the electrolyte include: adding boric acid and sodium tetraborate into deionized water and completely dissolving them to obtain the electrolyte.

[0039] The tantalum core is placed in the electrolyte when the ion water conductivity is less than 0.8 μS / cm, the electrolyte temperature is 75° C., and the conductivity is 1000-2000 μS / cm.

[0040] In the step 1), after placing the tantalum core in the electrolyte, the power supply is turned on to boost the voltage, and the voltage is set to 3 times the formation voltage, the current = (number of cores × current density), and after the current density reaches 1000mA / g, the constant voltage is maintained for 5 minutes, and then the power supply is turned off and the tantalum core is taken out.

[0041] The spraying time in step 2) is 8 minutes, and then the product is placed in a boiling and washing tank for boiling and washing. The boiling and washing tank temperature is 90° C. and the boiling and washing time is 70 minutes.

[0042] After the boiling and washing in step 3) is completed, the tantalum core is placed in the air for natural cooling, and the cooling time is 20 minutes.

[0043] Example 3:

[0044] A method for preparing a pressure-resistant dielectric layer, wherein a tantalum core is placed under corresponding voltage and current density to form the pressure-resistant dielectric layer, comprises the following steps:

[0045] 1) Place the tantalum core into a forming tank with an electrolyte and apply the corresponding voltage and current density;

[0046] 2) spraying and boiling the tantalum core after step 1);

[0047] 3) The tantalum core after boiling and washing is cooled, and then repaired according to the original forming process. After the repair is completed, spray and boil and wash according to step 2).

[0048] The tantalum core in step 1) is a tantalum core after formation, the electrolyte is deionized water, boric acid and sodium tetraborate, and the preparation and use steps of the electrolyte include: adding boric acid and sodium tetraborate into deionized water and completely dissolving them to obtain the electrolyte.

[0049] The tantalum core is placed in the electrolyte when the ion water conductivity is less than 0.8 μS / cm, the electrolyte temperature is 50° C., and the conductivity is 1500 μS / cm.

[0050] In the step 1), after placing the tantalum core in the electrolyte, the power supply is turned on to boost the voltage, and the voltage is set to 2 times the formation voltage, the current = (number of cores × current density), and after the current density reaches 800mA / g, the constant voltage is maintained for 3 minutes, and then the power supply is turned off and the tantalum core is taken out.

[0051] The spraying time in step 2) is 7 minutes, and then the product is placed in a boiling and washing tank for boiling and washing. The boiling and washing tank temperature is 87° C. and the boiling and washing time is 66 minutes.

[0052] After the boiling and washing in step 3) is completed, the tantalum core is placed in the air for natural cooling, and the cooling time is 15 minutes.

[0053] Comparative Example 1:

[0054] A 6.3V 100μF-B chip-type solid electrolyte tantalum capacitor processed by existing technology.

[0055] Comparative Example 2:

[0056] A 16V 330μF-H chip-type solid electrolyte tantalum capacitor processed by existing technology.

[0057] Examples 1-3 were fabricated using a 6.3V 100μF-B tantalum core and a 16V 330μF-H tantalum core, respectively, for chip-type solid electrolyte tantalum capacitors. After fabrication, the capacitors were processed according to the normal production process for chip-type solid electrolyte tantalum capacitors. The resulting capacitors were compared with those obtained in Comparative Examples 1 and 2. Ten randomly selected capacitor samples were subjected to static breakdown voltage testing. The test results are shown in Tables 1 and 2. The production process yields of the capacitors fabricated in Examples 1-3 and those obtained in Comparative Examples 1 and 2 were compared, as shown in Tables 3 and 4.

[0058] Table 1 6.3V100μF-B static breakdown voltage test results

[0059]

[0060] As can be seen from Table 1, Example 3 is the best example. Compared with the 6.3V 100μF-B chip solid electrolyte tantalum capacitor processed by the normal process, the 6.3V 100μF-B chip solid capacitor processed by the method of Example 3 has an average breakdown voltage increased by 2.8V.

[0061]

[0062]

[0063] Table 2 16V330μF-H static breakdown voltage test results

[0064] As can be seen from Table 2, Example 3 is the best example. Compared with the 16V330μF-H chip solid electrolyte tantalum capacitor processed by the normal process, the breakdown voltage of the 16V330μF-H chip solid capacitor processed by the method of Example 3 is increased by an average of 3.2V.

[0065] Table 3 6.3V100μF-B pass rate and input-output ratio

[0066]

[0067] It can be seen from Table 3 that Example 2 is the best example. Compared with the 6.3V 100μF-B chip solid electrolyte tantalum capacitor processed by the normal process, the 6.3V 100μF-B chip solid capacitor processed by the method of Example 2 has an input-output ratio increased by 5.02%.

[0068] Table 4 16V330μF-H qualified rate and input-output ratio

[0069]

[0070]

[0071] It can be seen from Table 4 that Example 3 is the best example. Compared with the 16V330μF-H chip solid electrolyte tantalum capacitor processed by the normal process, the input-output ratio of the 16V330μF-H chip solid electrolyte tantalum capacitor processed by the method of Example 3 is increased by 3.46%.

Claims

1. A method for preparing a pressure-resistant dielectric layer, characterized in that: The invention comprises the process of placing the tantalum core used for capacitor preparation under corresponding voltage and current density to form a pressure-resistant dielectric layer.

2. The method for preparing a pressure-resistant dielectric layer according to claim 1, characterized in that: The process of placing the tantalum core under corresponding voltage and current density to form a pressure-resistant dielectric layer includes the following steps: 1) Place the tantalum core into a forming tank with an electrolyte and apply a corresponding voltage and current density; 2) spraying and boiling the tantalum core after step 1); 3) The tantalum core after boiling and washing is cooled, and then supplementary forming is performed according to the original forming process flow. After the supplementary forming is completed, spraying and boiling and washing are performed according to step 2).

3. The method for preparing a pressure-resistant dielectric layer according to claim 2, characterized in that: The tantalum core in step 1) includes a tantalum core before, during or after normal formation, the electrolyte includes deionized water, boric acid and sodium tetraborate, and the preparation and use steps of the electrolyte include: adding boric acid and sodium tetraborate into deionized water and completely dissolving them to obtain an electrolyte.

4. The method for preparing a pressure-resistant dielectric layer according to claim 2, characterized in that: In the step 1), when the electrolyte temperature reaches T and the conductivity is D, the tantalum core is placed in the electrolyte.

5. The method for preparing a pressure-resistant dielectric layer according to claim 4, characterized in that: The ion water conductivity is less than 0.8 μS / cm, the electrolyte temperature is 10-75° C., and the conductivity is 1000-2000 μS / cm, and the tantalum core is placed in the electrolyte.

6. The method for preparing a pressure-resistant dielectric layer according to claim 2, characterized in that: In the step 1), the tantalum core is placed in the electrolyte and the power supply is turned on to boost the voltage, and the voltage is set to U and the current density is I d After that, keep constant voltage for time t1, then turn off the power and take out the tantalum core.

7. The method for preparing a pressure-resistant dielectric layer according to claim 6, characterized in that: The voltage is 2 to 3 times the forming voltage, the current density is 500 to 1000 mA / g, and the constant voltage is maintained for 2 to 5 minutes.

8. The method for preparing a pressure-resistant dielectric layer according to claim 1, characterized in that: The spraying time in step 2) is 5 to 8 minutes, and then the mixture is placed in a boiling and washing tank for boiling and washing. The temperature of the boiling and washing tank is 80 to 90° C. and the boiling and washing time is 60 to 70 minutes.

9. The method for preparing a pressure-resistant dielectric layer according to claim 1, characterized in that: After the boiling and washing in step 3) is completed, the tantalum core is placed in the air for natural cooling, and the cooling time is ≥ 10 minutes.

10. A tantalum capacitor prepared by the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Capacitor for reducing tantalum capacitance attenuation and preparation method thereof