Plasma enhanced silver nanoparticles / 4, 5-dibromofluorescein composite photocatalyst, preparation method and application
By growing silver nanoparticles on the surface of 4,5-dibromofluorescein nanosheets to form a composite photocatalyst, the problems of narrow photoresponse range and low carrier separation efficiency of traditional photocatalytic materials are solved, and high efficiency under visible light is achieved Photocatalytic decomposition of aquatic hydrogen and long-term stability.
Patent Information
- Application Number
- CN202411385784.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
The intrinsic band gap of traditional inorganic photocatalytic materials is wide and can only absorb ultraviolet light and part of visible light, which limits its light response range. The 4,5-dibromofluorescein has low solubility in aqueous media and photogenerated carrier separation Poor efficiency leads to low photocatalytic activity, limiting its application in the field of photolysis aquatic hydrogen.
Silver nanoparticles are grown on the surface of 4,5-dibromofluorescein nanosheets by in-situ photodeposition, and surface plasmon resonance effect is introduced to form silver nanoparticles/4,5-dibromofluorescein composite photocatalyst to enhance light absorption performance and charge migration efficiency.
The photocatalytic activity and visible light response capability are improved, and the high-efficiency photocatalytic decomposition of aquatic hydrogen under visible light is achieved, and it has long-term stability, which significantly improves the performance of the photocatalyst.
Smart Images

Figure HDA0005070960900000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photocatalytic functional materials, and specifically relates to a novel silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst and a preparation technology thereof. Background Art
[0002] Photocatalytic hydrogen production technology plays an increasingly important role in the development of zero-carbon energy and is a key technology in line with the sustainable development strategy. However, traditional inorganic photocatalytic materials have a wide intrinsic band gap and can only absorb ultraviolet light with higher frequencies and part of visible light, and have a narrow light response range. Therefore, the development of new semiconductor photocatalytic materials that can capture a wider solar spectrum is the key to achieving efficient photocatalysis. Compared with inorganic photocatalytic materials, organic photocatalytic materials are highly respected for their excellent light capture ability, highly delocalized π electron structure, and easily adjustable molecular structure.
[0003] 4,5-dibromofluorescein is a member of the organic semiconductors with a large absorption cross section, high quantum efficiency and a wide range of light absorption. However, pure 4,5-dibromofluorescein has two disadvantages as a photocatalyst. First, 4,5-dibromofluorescein has a low solubility in aqueous media, resulting in a low density of surface active sites; second, the separation efficiency of photogenerated carriers is poor, resulting in low photocatalytic activity. The above disadvantages limit its application in the field of photolysis of water to produce hydrogen. Therefore, it is necessary to find a suitable modification method to improve its photocatalytic activity. Summary of the invention
[0004] The present invention aims to enrich the types and sources of existing photocatalytic materials, provides a new type of silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst and its preparation technology, and applies it to the field of photocatalytic hydrogen production.
[0005] The inventive concept of the present invention is that the surface plasmon resonance effect presented by introducing silver nanoparticles on semiconductor photocatalysts is expected to overcome the limitations of low visible light absorption capacity and high carrier recombination rate of semiconductor photocatalysts. Inspired by this, the present invention has developed a visible light responsive silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst and its preparation method.
[0006] The silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst prepared by the invention has the advantages of high photocatalytic activity and visible light response, and can be applied to photocatalytic water decomposition to produce hydrogen.
[0007] The above object of the present invention is achieved through the following technical solutions:
[0008] The present invention firstly requests to protect a silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst. The catalyst uses 4,5-dibromofluorescein nanosheets as carriers and grows silver nanoparticles on the surface of 4,5-dibromofluorescein nanosheets by an in-situ photodeposition method.
[0009] The present invention also claims a method for preparing the composite catalyst, which comprises the following specific steps:
[0010] First, weigh 94-100 mg of 4,5-dibromofluorescein, add 30-35 ml of deionized water, and ultrasonically disperse for 5-10 minutes to obtain a uniformly dispersed suspension A; then, add 0-800 μl of silver nitrate solution (0.0926 mol / L) to the suspension A under dark conditions, stir thoroughly, and continue ultrasonicating for 5-10 minutes to obtain a solution B.
[0011] Solution B is transferred to a quartz reactor and placed under a xenon lamp, connected to a circulating water system to maintain the temperature of the reaction solution at 30-35°C, and irradiated under the full spectrum for 30-35 minutes, and the whole process is carried out under magnetic stirring. After the reaction is completed, the product is collected by centrifugation, and washed with deionized water for 3-5 times, and finally the product collected by centrifugation is placed in an oven for drying for 10-12 hours, and finally x wt% silver nanoparticles / 4,5-dibromofluorescein composite photocatalyst is obtained, wherein x represents the mass percentage of theoretical silver nanoparticles in the product, and x=4-8.
[0012] As a preferred embodiment of the present invention, the preparation method of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst is as follows: first, weigh 92-96 mg of 4,5-dibromofluorescein with a total mass into a beaker, add 30 ml of deionized water, and ultrasonically disperse for 5 minutes to obtain a uniformly dispersed suspension A. Then, add 400-800 microliters of silver nitrate solution (0.0926 mol / L) to the suspension A under dark conditions, stir well, and continue ultrasonication for 10 minutes to obtain solution B. Solution B is transferred to a quartz reactor and placed under a xenon lamp, connected to a circulating water system to keep the reaction liquid temperature at 35°C, irradiated under full spectrum for 30 minutes, and the whole process is carried out under magnetic stirring. After the reaction is completed, the product is collected by centrifugation and washed with deionized water 3 times. Finally, the product collected by centrifugation is placed in an oven and dried for 12 hours to finally obtain a silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst.
[0013] The present invention seeks to protect the application of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst, namely, the application of photocatalytic decomposition of water to produce hydrogen under visible light.
[0014] Compared with the prior art, the present invention has the following advantages:
[0015] (1) The present invention adopts an in-situ photodeposition method to prepare the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst, which does not require high temperature and high pressure, has the advantages of simple and easy operation, easy availability of raw materials, low cost and no pollution.
[0016] (2) The excellent performance of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst prepared by the present invention mainly comes from two aspects: on the one hand, the surface plasmon resonance effect induced by silver nanoparticles can improve light utilization efficiency and energy conversion by enhancing local field strength, resonant energy transfer, hot electron injection and other mechanisms, thereby improving light absorption performance; on the other hand, the Schottky junction formed between the silver nanoparticles and the 4,5-dibromofluorescein nanosheets can realize the directional migration of charges, effectively inhibiting the recombination of photogenerated electrons and holes.
[0017] (3) The composite photocatalyst prepared by the present invention can efficiently photocatalytically decompose water to produce hydrogen under visible light and has long-term stability in the photocatalytic hydrogen production process, which further verifies the superiority of the photocatalyst. The present invention has a positive effect on enriching the types and sources of photocatalytic materials.
[0018] The present invention provides a new approach for researching and developing novel semiconductor photocatalytic materials that respond to visible light. This technology is of great significance for solving the increasingly serious energy problem and has potential broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A is a scanning electron microscope image of 4,5-dibromofluorescein;
[0020] Figure 1 B is a transmission electron micrograph of the prepared silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst.
[0021] Figure 1 C is a comparison chart of the rates of hydrogen production from water decomposition by the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst and pure 4,5-dibromofluorescein under visible light irradiation.
[0022] Figure 1 D is the cyclic stability diagram of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst for decomposing water to produce hydrogen under visible light irradiation. DETAILED DESCRIPTION
[0023] In order to more clearly illustrate the purpose, technical solutions and advantages of the present invention, the embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. It should be understood that the following description of the embodiments is intended to explain and illustrate the overall concept of the present invention, and should not be construed as limiting the present invention. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial sources.
[0024] Example 1
[0025] Weigh 96 mg of 4,5-dibromofluorescein in a beaker, add 30 ml of deionized water, and ultrasonically disperse for 5 minutes to obtain a uniformly dispersed suspension A. Then, add 400 microliters of silver nitrate solution (0.0926 mol / L) to suspension A under dark conditions, stir well, and continue ultrasonication for 10 minutes to obtain solution B. Solution B is transferred to a quartz reactor and placed under a xenon lamp, connected to a circulating water system to keep the reaction liquid temperature at 35°C, irradiated for 30 minutes under the full spectrum, and the whole process is carried out under magnetic stirring. After the reaction is completed, the product is collected by centrifugation and washed 3 times with deionized water. Finally, the product collected by centrifugation is placed in an oven and dried for 12 hours, and finally a silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst with a catalyst x=4.0 is obtained.
[0026] Example 2
[0027] The difference between this embodiment and embodiment 1 is that the mass of 4,5-dibromofluorescein added in step (1) is adjusted to 94 mg, and the volume of the added silver nitrate solution is adjusted to 600 μL, and finally a silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst with a catalyst x=6.0 is obtained.
[0028] Example 3
[0029] The difference between this embodiment and embodiment 1 is that the mass of 4,5-dibromofluorescein added in step (1) is adjusted to 92 mg, and the volume of the added silver nitrate solution is adjusted to 800 μL, and finally a silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst with a catalyst of x=8.0 is obtained.
[0030] Comparative Example 1
[0031] The difference between this embodiment and embodiment 1 is that the mass of 4,5-dibromofluorescein added in step (1) is adjusted to 100 mg, the volume of the added silver nitrate solution is adjusted to 0 μl, and the catalyst finally obtained is pure 4,5-dibromofluorescein.
[0032] like Figure 1 (A) is a scanning electron microscope image of 4,5-dibromofluorescein. From the image, it can be seen that 4,5-dibromofluorescein is a two-dimensional nanosheet with a smooth surface. Figure 1 (B) shows a transmission electron micrograph of the prepared silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst. It can be clearly observed from the figure that a large number of silver nanoparticles are uniformly dispersed on the surface of 4,5-dibromofluorescein nanosheets, and the average particle size of the silver nanoparticles is 10±3 nanometers.
[0033] Application Example 1
[0034] The silver nanoparticles / 4,5-dibromofluorescein composite photocatalyst prepared in Example 2 is used for photocatalytic water decomposition and hydrogen production, and the 4,5-dibromofluorescein prepared in Comparative Example 1 is used as a control sample. The reaction of photocatalytic water decomposition and hydrogen production is carried out in a sealed circulation system, the reactor volume is 100 ml, and a 300-watt xenon lamp equipped with a 420-nanometer filter is used as a light source. 50 mg of silver nanoparticles / 4,5-dibromofluorescein composite photocatalyst is placed in a reactor, and then 50 ml of a mixed solution prepared by 40 ml of deionized water and 10 ml of triethanolamine is added. The photocatalytic reaction is reacted under magnetic stirring, and the reaction system is evacuated to vacuum. Subsequently, the light source and the gas circulation pump are turned on, and the sample is automatically injected once per hour during the reaction process. Finally, the product is measured and analyzed by a gas chromatograph to obtain the photocatalytic water decomposition and hydrogen production results of the silver nanoparticles / 4,5-dibromofluorescein composite photocatalyst.
[0035] Figure 1 (C) is a comparison of the rates of hydrogen production from water decomposition by the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst and pure 4,5-dibromofluorescein under visible light irradiation. The experimental results show that the hydrogen production rate of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst is as high as 1265.22 μmol g -1 ·h -1 This value is higher than that of pure 4,5-dibromofluorescein (11.39 μmol g -1 ·h -1 ) The hydrogen production rate was 111 times higher than that of the conventional photocatalyst, which fully demonstrated the superiority of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst in the field of photocatalytic water decomposition and hydrogen production. In addition, no obvious attenuation of hydrogen production activity was observed during continuous irradiation under visible light for 20 hours. This result strongly proves that the photocatalytic material of the present invention has long-term stability in the process of photocatalytic hydrogen production, further verifying the superiority of the prepared photocatalyst.
[0036] Figure 1 D is a cyclic stability diagram of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst decomposing water to produce hydrogen under visible light irradiation. It can be observed from the figure that no obvious attenuation of hydrogen production activity was observed during the continuous irradiation of visible light for 20 hours. This result strongly proves that the photocatalytic material of the present invention has long-term stability in the process of photocatalytic hydrogen production, further verifying the superiority of the prepared photocatalyst.
[0037] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0038] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. Plasma-enhanced silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst, which uses 4,5-dibromofluorescein nanosheets as carriers and grows silver nanoparticles on the surface of 4,5-dibromofluorescein nanosheets by in-situ photodeposition.
2. The method for preparing the composite catalyst according to claim 1, comprising the steps of: First, 94-100 mg of 4,5-dibromofluorescein was weighed, 30-35 ml of deionized water was added, and ultrasonic dispersion was performed for 5-10 minutes to obtain a uniformly dispersed suspension A; then, 0-800 μl of silver nitrate solution was added to the suspension A under dark conditions, and after sufficient stirring, ultrasonic dispersion was continued for 5-10 minutes to obtain a solution B; Solution B is transferred to a quartz reactor and placed under a xenon lamp, connected to a circulating water system to maintain the temperature of the reaction solution at 30-35°C, and irradiated under the full spectrum for 30-35 minutes, and the whole process is carried out under magnetic stirring. After the reaction is completed, the product is collected by centrifugation, and washed with deionized water for 3-5 times, and finally the product collected by centrifugation is placed in an oven for drying for 10-12 hours, and finally x wt% silver nanoparticles / 4,5-dibromofluorescein composite photocatalyst is obtained, wherein x represents the mass percentage of theoretical silver nanoparticles in the product, and x=4-8.
3. The preparation method according to claim 2, characterized in that: The concentration of silver nitrate solution is 0.09~0.1mol / L.
4. The preparation method according to claim 3, characterized in that: The concentration of silver nitrate solution is 0.0926 mol / L.
5. The preparation method according to claim 2, characterized in that: First, weigh 92 to 96 mg of 4,5-dibromofluorescein in a total mass and put it into a beaker, add 30 ml of deionized water, and ultrasonically disperse it for 5 minutes to obtain a uniformly dispersed suspension A; then, add 400 to 800 microliters of 0.0926 mol / L silver nitrate solution to the suspension A under dark conditions, stir it thoroughly, and continue ultrasonicating for 10 minutes to obtain a solution B; transfer the solution B to a quartz reactor, place it under a xenon lamp, connect a circulating water system to keep the reaction liquid temperature at 35°C, irradiate it under the full spectrum for 30 minutes, and the whole process is carried out under magnetic stirring; after the reaction is completed, collect the product by centrifugation, wash it with deionized water 3 times, and finally place the product collected by centrifugation in an oven to dry for 12 hours, and finally obtain a silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst.
6. The use of the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst according to claim 1, characterized in that: Application of photocatalytic water decomposition to produce hydrogen under visible light.
7. The use according to claim 6, characterized in that: The experiment was carried out in a sealed circulation system, with a 300-watt xenon lamp equipped with a 420-nanometer filter as the light source; the silver nanoparticle / 4,5-dibromofluorescein composite photocatalyst was placed in a reactor, and then a mixed solution prepared with deionized water and triethanolamine was added; the photocatalytic reaction was carried out under magnetic stirring, and the reaction system was evacuated to a vacuum; then the light source and the gas circulation pump were turned on, and the sample was automatically injected once every hour during the reaction.