Chromium-free passivator for nickel-plated plate and preparation process of chromium-free passivator
By using chromium-free passivating agents composed of silane coupling agents and their preparation technology, the toxicity problem of hexavalent chromium in the passivation treatment of traditional nickel plates is solved, providing an environmentally friendly, safe and efficient passivation effect, replacing the traditional Passivating agent to avoid environmental pollution and maintain corrosion resistance.
Patent Information
- Application Number
- CN202411159084.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
The hexavalent chromium-containing passivating agent used in the passivation treatment of traditional nickel plates has serious toxicity and carcinogenicity, causing environmental and human health hazards. It is urgent to design a chromium-free passivating agent and its preparation process.
A chromium-free passivator consisting of silane coupling agent, titanate, zirconium salt, stabilizer, organic acid, oxidizing agent, rare earth element compounds, complexing agent, wetting agent and deionized water is used, and the specific combination is The ratio and process steps are prepared, including stirring, heating and filtration, to form a chromium-free passivator.
It provides an environmentally friendly, safe and efficient alternative, avoids environmental pollution of hexavalent chromium, has corrosion resistance similar to traditional passivating agents, and is simple in process and low in cost.
Smart Images

Figure CN119040867A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of passivators, and in particular to a chromium-free passivator for nickel-plated plates and a preparation process thereof. Background Art
[0002] Passivation agents can form a passivation protective film on the metal surface to protect the metal from corrosion and extend the service life of the metal. The passivation protective film is dense and has good gloss, which can protect the metal from corrosion, improve the performance of the metal material, and give the metal material surface various colors;
[0003] The Chinese patent with the publication (announcement) number CN106350803A discloses a metal plate passivator, which is composed of the following components by weight: 1-2 parts of phosphoric acid, 7.8 parts of phosphoric acid, 0.7 parts of yam residue extract, 1.1 parts of sodium dodecyl sulfonate, 2.3 parts of vinyl trimethoxysilane, 0.9 parts of dodecyl trimethyl ammonium bromide, 8.4 parts of hydroxyethylidene diphosphonic acid, 1.2 parts of sodium alkyl succinate sulfonate, 0.7 parts of sodium aluminate, and 36 parts of deionized water. The metal plate passivator of the present invention can be used for passivation treatment of metals to form a uniform passivation protective film on the metal surface. The protective film has excellent rust resistance, abrasion resistance, corrosion resistance, heat resistance, cold resistance, and weather resistance, and has good surface finish.
[0004] The traditional passivation treatment of nickel-plated plates usually uses a passivating agent containing hexavalent chromium. Although the passivation effect is good, hexavalent chromium is highly toxic and carcinogenic, causing serious harm to the environment and human health. Therefore, it is urgent to design a chromium-free passivating agent for nickel-plated plates and its preparation process to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a chromium-free passivating agent for nickel-plated plates and a preparation process thereof, so as to solve the above-mentioned deficiencies in the prior art.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A chromium-free passivator for a nickel-plated plate includes a chromium-free passivator, wherein the chromium-free passivator is composed of a silane coupling agent, a titanate, a zirconium salt, a stabilizer, an organic acid, an oxidant, a rare earth element compound, a complexing agent, a wetting agent and deionized water, and is composed of the following components in percentage by weight:
[0008] Silane coupling agent 1-10%;
[0009] Titanate 0.1-5%;
[0010] Zirconium salt 1-10%;
[0011] Stabilizer 0.1-2%;
[0012] Organic acid 1-5%;
[0013] Oxidant: 0.1-1%;
[0014] Rare earth element compounds: 0.5-3%;
[0015] Complexing agent: 0.1-2%;
[0016] Wetting agent: 0.01-0.1%;
[0017] Deionized water: balance.
[0018] Preferably, the rare earth element compound is a mixture of one or more of yttrium nitrate or cerium nitrate, and the organic acid is a mixture of one or more of citric acid or acetic acid.
[0019] Preferably, the oxidant is a mixture of one or more of hydrogen peroxide, peracetic acid and sodium dichromate, and the complexing agent is a mixture of one or more of ethylenediaminetetraacetic acid, sodium triacetate and diethylenetriamine pentacarboxylate.
[0020] Preferably, the wetting agent is one of distilled water, anionic surfactant and nonionic surfactant.
[0021] Preferably, the silane coupling agent is γ-aminopropyltriethoxysilane, and the titanate can be isopropyltri(acetylacetonate)titanium.
[0022] Preferably, the zirconium salt is a mixture of one or more of fluorozirconic acid, ammonium fluorozirconate and ammonium zirconate, and the stabilizer can be a mixture of one or more of potassium sodium tartrate, tribasic lead salt and phosphite.
[0023] Preferably, the anionic surfactant is a mixture of one or more of alkyl sulfates, sulfonates, fatty acids or fatty acid ester sulfates, and the nonionic surfactant is a mixture of one or more of polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers and polyoxyethylene polyoxypropylene block copolymers.
[0024] In addition, a preparation process of a chromium-free passivating agent for a nickel-plated plate is provided, which is used to prepare the chromium-free passivating agent for a nickel-plated plate, and the preparation process comprises the following steps:
[0025] S1. Weigh the silane coupling agent, the titanate, the zirconium salt, the stabilizer, the organic acid, the oxidant, the rare earth element compound, the complexing agent, the wetting agent and the deionized water according to the proportion;
[0026] S2, dissolving the silane coupling agent, the titanate, the zirconium salt, the rare earth element compound, the organic acid, the oxidant, the complexing agent and the wetting agent in deionized water, and stirring them evenly using a stirring device to obtain a mixed solution;
[0027] S3, adding the mixed solution into a heating device, heating the mixed solution using the heating device, and stirring the mixed solution using a stirring device at the same time, and gradually adding the stabilizer while stirring the mixed solution;
[0028] S4, after the mixed solution is heated and stirred by the heating device and the stirring device, the mixed solution after heating and stirring is taken out and placed in a container, and then the mixed solution is cooled to room temperature;
[0029] S5. After the mixed solution is cooled to room temperature, the mixed solution is poured into a filtering device, and the mixed solution is filtered using the filtering device to obtain a chromium-free passivating agent, and then the obtained chromium-free passivating agent is stored using a storage tool for standby use.
[0030] The heating temperature of the mixed solution by the heating device is 60-80°C.
[0031] The stirring time of the mixed solution by the stirring device is 30-60 minutes.
[0032] In the above technical scheme, the present invention provides a chromium-free passivating agent for nickel-plated plates and a preparation process thereof, and the beneficial effects are:
[0033] (1) The chromium-free passivating agent for nickel-plated plates provided by the present invention has the advantages of being environmentally friendly, safe, and highly efficient, and can effectively replace traditional chromium-containing passivating agents, has a wide range of application prospects, and does not contain hexavalent chromium, thus avoiding the environmental pollution problem of hexavalent chromium.
[0034] (2) The chromium-free passivator for nickel-plated plates provided by the present invention has corrosion resistance close to that of a hexavalent chromium passivator and has an excellent passivation effect, thereby being able to effectively improve the corrosion resistance of the nickel-plated plates.
[0035] (3) The chromium-free passivating agent for nickel-plated plates provided by the present invention does not pollute the environment, can prevent volatile acids from causing harm to workers, and has a simple preparation process and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.
[0037] Figure 1 A schematic structural diagram of the steps of a preparation method provided in an embodiment of a chromium-free passivating agent for nickel-plated plates and a preparation process thereof is provided in the present invention.
[0038] Figure 2 A schematic structural diagram of specific preparation method steps provided for a chromium-free passivating agent for nickel-plated plates and a preparation process embodiment thereof according to the present invention. DETAILED DESCRIPTION
[0039] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.
[0040] like Figure 1-2 As shown, a chromium-free passivator for a nickel-plated plate provided in an embodiment of the present invention includes a chromium-free passivator, which is composed of a silane coupling agent, a titanate, a zirconium salt, a stabilizer, an organic acid, an oxidant, a rare earth element compound, a complexing agent, a wetting agent and deionized water, and is composed of the following components in weight percentage:
[0041] Silane coupling agent 1-10%;
[0042] Titanate 0.1-5%;
[0043] Zirconium salt 1-10%;
[0044] Stabilizer 0.1-2%;
[0045] Organic acid 1-5%;
[0046] Oxidant: 0.1-1%;
[0047] Rare earth element compounds: 0.5-3%;
[0048] Complexing agent: 0.1-2%;
[0049] Wetting agent: 0.01-0.1%;
[0050] Deionized water: balance.
[0051] Among them, the rare earth element compound is a mixture of one or more of yttrium nitrate or cerium nitrate, and the organic acid is a mixture of one or more of citric acid or acetic acid. The rare earth element compound is used to enhance the density and stability of the passivation film and improve the corrosion resistance. The organic acid adjusts the pH value of the passivator and promotes the passivation reaction.
[0052] The oxidant is a mixture of one or more of hydrogen peroxide, peracetic acid and sodium dichromate, and the complexing agent is a mixture of one or more of ethylenediaminetetraacetic acid, sodium triacetate and diethylenetriamine pentacarboxylate. The oxidant is used to provide the necessary oxidizing environment during the passivation process, and the complexing agent is used to effectively control the release rate of metal ions to form a uniform and dense passivation film.
[0053] The wetting agent is one of distilled water, anionic surfactant and nonionic surfactant. The wetting agent is used to improve the wettability of the passivation solution on the surface of the nickel plate and ensure the uniformity of the passivation film.
[0054] The silane coupling agent is γ-aminopropyltriethoxysilane, and the titanate can be selected from isopropyl tri(acetylacetonate)titanium. The silane coupling agent is used to improve the adhesion and durability between the passivator and the nickel-plated plate.
[0055] The zirconium salt is a mixture of one or more of fluorozirconic acid, ammonium fluorozirconate and ammonium zirconate. The stabilizer can be a mixture of one or more of potassium sodium tartrate, tribasic lead salt and phosphite. The zirconium salt is used to improve the corrosion resistance of the nickel-plated plate.
[0056] The anionic surfactant is a mixture of one or more of alkyl sulfates, sulfonates, fatty acids or fatty acid ester sulfates, and the nonionic surfactant is a mixture of one or more of polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers and polyoxyethylene polyoxypropylene block copolymers.
[0057] In addition, a preparation process of a chromium-free passivating agent for a nickel-plated plate is provided, which is used to prepare the above-mentioned chromium-free passivating agent for a nickel-plated plate, and the preparation process comprises the following steps:
[0058] S1. Weigh the components of silane coupling agent, titanate, zirconium salt, stabilizer, organic acid, oxidant, rare earth element compound, complexing agent, wetting agent and deionized water according to the proportion;
[0059] S2, dissolving the silane coupling agent, titanate, zirconium salt solution, rare earth element compound, organic acid, oxidant, complexing agent and wetting agent in deionized water, and stirring them evenly with a stirring device to obtain a mixed solution;
[0060] S3, adding the mixed solution into a heating device, heating the mixed solution using the heating device, and stirring the mixed solution using a stirring device at the same time, and gradually adding a stabilizer while stirring the mixed solution;
[0061] S4, after the mixed solution is heated and stirred using the heating device and the stirring device, the heated and stirred mixed solution is taken out and placed in a container, and then the mixed solution is cooled to room temperature;
[0062] S5. After the mixed solution is cooled to room temperature, the mixed solution is poured into a filtering device, and the mixed solution is filtered using the filtering device to obtain a chromium-free passivating agent, and then the obtained chromium-free passivating agent is stored using a storage tool for standby use.
[0063] The heating temperature of the mixed solution by the heating device is 60-80°C.
[0064] The stirring time of the mixed solution by the stirring device is 30-60 minutes.
[0065] Example 1
[0066] The preparation process is as follows:
[0067] S1. Weigh 3% of silane coupling agent, 1% of titanate, 5% of zirconium salt, 0.5% of stabilizer, 1.5% of organic acid, 0.25% of oxidant, 0.5% of rare earth element compound, 1% of complexing agent, 0.025% of wetting agent and the balance of deionized water;
[0068] S2, dissolving 3% of silane coupling agent, 1% of titanate, 5% of zirconium salt, 0.5% of stabilizer, 1.5% of organic acid, 0.25% of oxidant, 0.5% of rare earth element compound, 1% of complexing agent and 0.025% of wetting agent in deionized water, and stirring them evenly with a stirring device to obtain a mixed solution;
[0069] S3, adding the mixed solution into a heating device, heating the mixed solution with the heating device, the heating temperature is 70 ° C, and stirring the mixed solution with a stirring device at the same time, the stirring time is 45 minutes, and while stirring the mixed solution, gradually adding a stabilizer;
[0070] S4, after the mixed solution is heated and stirred using the heating device and the stirring device, the heated and stirred mixed solution is taken out and placed in a container, and then the mixed solution is cooled to room temperature;
[0071] S5. After the mixed solution is cooled to room temperature, the mixed solution is poured into a filtering device, and the mixed solution is filtered using the filtering device to obtain a chromium-free passivating agent, and then the obtained chromium-free passivating agent is stored using a storage tool for standby use.
[0072] Example 2
[0073] S1. Weigh 5% of silane coupling agent, 3% of titanate, 8% of zirconium salt, 1% of stabilizer, 3% of organic acid, 0.5% of oxidant, 2% of rare earth element compound, 1.5% of complexing agent, 0.5% of wetting agent and the balance of deionized water;
[0074] S2, dissolving 5% of silane coupling agent, 3% of titanate, 8% of zirconium salt, 1% of stabilizer, 3% of organic acid, 0.5% of oxidant, 2% of rare earth element compound, 1.5% of complexing agent and 0.5% of wetting agent in deionized water, and stirring them evenly with a stirring device to obtain a mixed solution;
[0075] S3, adding the mixed solution into a heating device, heating the mixed solution with the heating device, the heating temperature is 75 ° C, and simultaneously using a stirring device to keep stirring the mixed solution for 40 minutes, and gradually adding a stabilizer while stirring the mixed solution;
[0076] S4, after the mixed solution is heated and stirred using the heating device and the stirring device, the heated and stirred mixed solution is taken out and placed in a container, and then the mixed solution is cooled to room temperature;
[0077] S5. When the mixed solution is cooled to room temperature, pour the mixed solution into a filtering device, filter the mixed solution using the filtering device to obtain a chromium-free passivating agent, and then use a storage tool to store the obtained chromium-free passivating agent for standby use.
[0078] Example 3
[0079] S1. Weigh 7% of silane coupling agent, 4% of titanate, 9% of zirconium salt, 1.5% of stabilizer, 4% of organic acid, 1% of oxidant, 2.5% of rare earth element compound, 2% of complexing agent, 0.75% of wetting agent and the balance of deionized water;
[0080] S2, dissolving 7% of silane coupling agent, 4% of titanate, 9% of zirconium salt, 1.5% of stabilizer, 4% of organic acid, 1% of oxidant, 2.5% of rare earth element compound, 2% of complexing agent and 0.75% of wetting agent in deionized water, and stirring them evenly with a stirring device to obtain a mixed solution;
[0081] S3, adding the mixed solution into a heating device, heating the mixed solution with the heating device, the heating temperature is 80 ° C, and stirring the mixed solution with a stirring device at the same time, the stirring time is 50 minutes, and while stirring the mixed solution, gradually adding a stabilizer;
[0082] S4, after the mixed solution is heated and stirred using the heating device and the stirring device, the heated and stirred mixed solution is taken out and placed in a container, and then the mixed solution is cooled to room temperature;
[0083] S5. When the mixed solution is cooled to room temperature, pour the mixed solution into a filtering device, filter the mixed solution using the filtering device to obtain a chromium-free passivating agent, and then use a storage tool to store the obtained chromium-free passivating agent for standby use.
[0084] After testing the results of the stamping oils prepared in Example 1, Example 2 and Example 3, it was found that the stamping synthetic oil prepared in Example 2 had the best effect, could effectively meet the working requirements of the steel shell machine, and solve the problems of difficult-to-process heavy-load forming processes, difficult workpiece cleaning, and easy oxidation of oil products.
[0085] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.
Claims
1. A chromium-free passivator for nickel-plated plates, comprising a chromium-free passivator, characterized in that: The chromium-free passivating agent is composed of a silane coupling agent, a titanate, a zirconium salt, a stabilizer, an organic acid, an oxidant, a rare earth element compound, a complexing agent, a wetting agent and deionized water, and is composed of the following components in weight percentage: Silane coupling agent 1-10%; Titanate 0.1-5%; Zirconium salt 1-10%; Stabilizer 0.1-2%; Organic acid 1-5%; Oxidant: 0.1-1%; Rare earth element compounds: 0.5-3%; Complexing agent: 0.1-2%; Wetting agent: 0.01-0.1%; Deionized water: balance.
2. A chromium-free passivating agent for nickel-plated plates according to claim 1, characterized in that: The rare earth element compound is a mixture of one or more of yttrium nitrate or cerium nitrate, and the organic acid is a mixture of one or more of citric acid or acetic acid.
3. A chromium-free passivating agent for nickel-plated plates according to claim 1, characterized in that: The oxidant is a mixture of one or more of hydrogen peroxide, peracetic acid and sodium dichromate, and the complexing agent is a mixture of one or more of ethylenediaminetetraacetic acid, sodium triacetate and diethylenetriamine pentacarboxylate.
4. A chromium-free passivating agent for nickel-plated plates according to claim 1, characterized in that: The wetting agent is one of distilled water, anionic surfactant and nonionic surfactant.
5. A chromium-free passivating agent for nickel-plated plates according to claim 1, characterized in that: The silane coupling agent is γ-aminopropyltriethoxysilane, and the titanate can be selected from isopropyl tri(acetylacetonate)titanium.
6. A chromium-free passivating agent for nickel-plated plates according to claim 1, characterized in that: The zirconium salt is a mixture of one or more of fluorozirconic acid, ammonium fluorozirconate and ammonium zirconate, and the stabilizer can be a mixture of one or more of potassium sodium tartrate, tribasic lead salt and phosphite.
7. A chromium-free passivating agent for nickel-plated plates according to claim 4, characterized in that: The anionic surfactant is a mixture of one or more of alkyl sulfates, sulfonates, fatty acids or fatty acid ester sulfates, and the nonionic surfactant is a mixture of one or more of polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers and polyoxyethylene polyoxypropylene block copolymers.
8. A process for preparing a chromium-free passivating agent for nickel-plated plates, used for preparing a chromium-free passivating agent for nickel-plated plates as claimed in any one of claims 1 to 7, characterized in that: The preparation process comprises the following steps: S1. Weigh the silane coupling agent, the titanate, the zirconium salt, the stabilizer, the organic acid, the oxidant, the rare earth element compound, the complexing agent, the wetting agent and the deionized water according to the proportion; S2, dissolving the silane coupling agent, the titanate, the zirconium salt, the rare earth element compound, the organic acid, the oxidant, the complexing agent and the wetting agent in deionized water, and stirring them evenly using a stirring device to obtain a mixed solution; S3, adding the mixed solution into a heating device, heating the mixed solution using the heating device, and stirring the mixed solution using a stirring device at the same time, and gradually adding the stabilizer while stirring the mixed solution; S4, after the mixed solution is heated and stirred by the heating device and the stirring device, the mixed solution after heating and stirring is taken out and placed in a container, and then the mixed solution is cooled to room temperature; S5. After the mixed solution is cooled to room temperature, the mixed solution is poured into a filtering device, and the mixed solution is filtered using the filtering device to obtain a chromium-free passivating agent, and then the obtained chromium-free passivating agent is stored using a storage tool for standby use.
9. A process for preparing a chromium-free passivating agent for nickel-plated plates according to claim 8, characterized in that: The heating temperature of the mixed solution by the heating device is 60-80°C.
10. The process for preparing a chromium-free passivating agent for nickel-plated plates according to claim 8, characterized in that: The stirring time of the mixed solution by the stirring device is 30-60 minutes.