Metal hollow fiber membrane with internal and external double-opening structure and preparation method of metal hollow fiber membrane

By constructing an inner and outer double-porous structure in the hollow fiber membrane, using the combination of the outer porous layer, dense separation layer and inner porous layer, the problem of small surface area of ​​the existing membrane is solved, and the hydrogen flux and hydrogen permeability rate is improved, which promotes the promotion of The hydrogen surface reaction.

CN119056271APending Publication Date: 2024-12-03CANGZHOU INSTITUTE OF TIANGONG UNIVERSITY +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411476309.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing hollow fiber membrane has a small surface area on both sides, which limits the hydrogen permeability rate of hydrogen and makes it difficult to increase the surface area on both sides at the same time.

Method used

A metal hollow fiber membrane with an inner and outer double-porous structure is adopted to form finger-like pores through the structure of an outer porous layer, a dense separation layer and an inner porous layer, thereby enhancing the specific surface area and reaction rate of the membrane.

Benefits of technology

It significantly improves the hydrogen flux and hydrogen permeability rate, provides a larger membrane surface area, promotes hydrogen surface reaction, and improves the filling density and catalytic efficiency of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056271A_ABST
    Figure CN119056271A_ABST
Patent Text Reader

Abstract

The invention relates to a metal hollow fiber membrane with an internal and external double-opening structure and a preparation method thereof. A microstructure of a membrane wall of the metal hollow fiber membrane with the inner and outer double-opening structure is sequentially provided with an outer porous layer, a compact separation layer and an inner porous layer from outside to inside, finger-shaped pore channels are formed in the outer porous layer and the inner porous layer, and a hollow inner cavity is formed in the inner porous layer. According to the metal hollow fiber membrane with the internal and external double-opening structure, the opening layers are arranged on the two sides, and the compact separation layer is arranged in the middle, so that a larger membrane specific surface area can be provided, a surface reaction is promoted, and the hydrogen flux is improved. The separation / catalysis area is large, and the filling density of the catalyst is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of membrane separation, and in particular relates to a metal hollow fiber membrane with inner and outer double opening structures and a membrane reactor. Background Art

[0002] As a clean and efficient energy source, hydrogen is of great significance in environmental protection, energy storage, green transportation and industrial applications. However, the extraction of hydrogen currently relies mainly on fossil fuels, which not only consumes a lot of energy, but also produces a lot of pollutants and aggravates global warming. In order to take into account both economic benefits and environmental protection, the production of hydrogen using industrial by-products such as coke oven gas, tar, crude glycerol, etc. is a feasible method.

[0003] Hydrogen has a dissolution diffusion mechanism for dense alloy membranes such as palladium, nickel, iron, vanadium, niobium, and tantalum, so metal membranes have 100% selectivity for hydrogen. Compared with traditional cryogenic distillation or pressure swing adsorption technology, the use of metal membranes for hydrogen separation has the advantages of high purity and low energy consumption, and the configuration of hollow fiber membranes can provide a greater packing density, so that the membrane assembly per unit volume provides a larger membrane area and reduces the floor space.

[0004] Hydrogen separation using dense metal membranes mainly undergoes two surface reactions and one bulk diffusion, specifically including the steps of hydrogen dissociating into hydrogen atoms by reaction on the membrane surface on the high-pressure side, the diffusion of hydrogen atoms in the membrane bulk, and the recombining of hydrogen atoms into hydrogen after permeation from the low-pressure side and surface reaction.

[0005] Patent document CN117899800A reports a metal hollow fiber membrane. Judging from the microstructure of its membrane wall, it has a structure in which one side of the membrane wall is a porous layer and the other side is a smooth and dense separation layer. Therefore, the hollow fiber membrane disclosed in this document can only obtain a large surface reaction rate on one side of the porous layer, while the smooth and dense layer on the other side is still limited.

[0006] Therefore, how to construct the structure of the hollow fiber membrane to simultaneously increase the surface area on both the inner and outer sides thereof, thereby providing a greater hydrogen permeation rate, is one of the problems to be solved urgently in the art. Summary of the invention

[0007] After research, the inventors found that by adopting the metal hollow fiber membrane with internal and external double opening structures of the present application, both sides of the membrane have a large specific surface area, which can increase the reaction rate on the membrane surface, ultimately increase the hydrogen flux, and provide a greater hydrogen permeation rate.

[0008] In order to achieve the above objectives, the present application provides the following technical solutions.

[0009] [1]. A metal hollow fiber membrane with double-opening structure inside and outside, which comprises an outer porous layer, a dense separation layer and an inner porous layer from the outside to the inside, wherein the outer porous layer and the inner porous layer have finger-like channels, and the inner porous layer forms a hollow inner cavity.

[0010] [2] A method for preparing a metal hollow fiber membrane with an inner and outer double-opening structure as described in [1], the method comprising the following steps:

[0011] Metal powder casting liquid preparation step: dissolving a first organic polymer in a first organic solvent, adding metal powder, and stirring to obtain a metal powder casting liquid;

[0012] Temporary outer skin layer casting liquid preparation step: dissolving the second organic polymer in the second organic solvent, and then adding the outer skin layer regulator to obtain the temporary outer skin layer casting liquid;

[0013] A temporary inner skin layer casting liquid preparation step: dissolving a third organic polymer in a third organic solvent, and then adding an inner skin layer regulator to obtain a temporary inner skin layer casting liquid;

[0014] Precursor preparation process: after vacuum degassing the metal powder casting liquid, the temporary outer skin layer casting liquid, and the temporary inner skin layer casting liquid, the temporary outer skin layer casting liquid, the metal powder casting liquid, the temporary inner skin layer casting liquid, and the inner solidification liquid are extruded from the outside to the inside into the outer solidification liquid through a three-layer spinneret, and under the action of the inner solidification liquid and the outer solidification liquid, the temporary outer skin layer casting liquid, the metal powder casting liquid, and the temporary inner skin layer casting liquid are solidified to form a temporary outer skin layer, a metal powder layer, and a temporary inner skin layer, respectively, and the temporary inner skin layer is formed into a structure with a hollow inner cavity, the metal powder layer is coated on the outside of the temporary inner skin layer, and the temporary outer skin layer is coated on the surface of the metal powder layer, and then dried to obtain a precursor;

[0015] Calcination process: calcining the precursor in an oxidizing atmosphere to remove the temporary outer skin layer and the temporary inner skin layer, forming an outer porous layer and an inner porous layer having finger-like pores, and part of the metal in the outer porous layer and the inner porous layer is oxidized, and part of the organic matter in the metal powder layer adjacent to the surface of the temporary outer skin layer and the temporary inner skin layer is removed, and then calcining in a reducing atmosphere to reduce the oxidized metal to obtain a metal hollow fiber membrane with inner and outer double-opening structures.

[0016] [3] According to the method for preparing a metal hollow fiber membrane with inner and outer double-opening structure described in [2], in the step of preparing the metal powder casting liquid,

[0017] The first organic polymer is at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide;

[0018] The first organic solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide;

[0019] The metal powder is at least one selected from iron powder, nickel powder, and iron-nickel alloy powder;

[0020] In the metal powder casting solution, the weight percentage of the first organic polymer is 5-10%, the weight percentage of the first organic solvent is 10-45%, and the weight percentage of the metal powder is 50-80%.

[0021] [4] According to the method for preparing the metal hollow fiber membrane with inner and outer double opening structures described in [2],

[0022] In the temporary outer skin layer casting liquid preparation step,

[0023] The second organic polymer is at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide;

[0024] The second organic solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide;

[0025] The outer epidermis layer regulating agent is at least one selected from water, ethanol, polyvinyl pyrrolidone, ammonium polymethacrylate, polymethyl methacrylate and phosphate;

[0026] In the temporary outer skin layer casting solution, the weight percentage of the second organic polymer is 5-10%, the weight percentage of the second organic solvent is 50-90%, and the weight percentage of the outer skin layer regulator is 2%-40%.

[0027] [5] According to the method for preparing the metal hollow fiber membrane with inner and outer double opening structures described in [2],

[0028] In the temporary inner skin layer casting solution preparation step,

[0029] The third organic polymer is at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide;

[0030] The third organic solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide;

[0031] The inner epidermis layer regulating agent is at least one selected from water, ethanol, polyvinyl pyrrolidone, ammonium polymethacrylate, polymethyl methacrylate and phosphate;

[0032] In the temporary inner skin layer casting solution, the weight percentage of the third organic polymer is 5-10%, the weight percentage of the third organic solvent is 50-90%, and the weight percentage of the inner skin layer regulating agent is 2%-40%.

[0033] [6] According to the method for preparing the metal hollow fiber membrane with inner and outer double opening structures described in [2],

[0034] In the precursor preparation process,

[0035] The internal coagulation liquid is a mixture of a solvent and a non-solvent, the solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and the non-solvent is at least one selected from water, ethanol, propanol, and ethylene glycol;

[0036] The mass percentage of the non-solvent in the internal coagulation liquid is 20-60%.

[0037] [7]. According to the method for preparing a metal hollow fiber membrane with an inner and outer double-opening structure described in [2], in the precursor preparation step,

[0038] The external coagulation liquid is a mixture of a solvent and a non-solvent, the solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and the non-solvent is at least one selected from water, ethanol, propanol, and ethylene glycol;

[0039] The mass percentage of the non-solvent in the external coagulation liquid is 20 to 90%.

[0040] [8]. According to the method for preparing a metal hollow fiber membrane with an inner and outer double-opening structure described in [2], in the calcination process, the oxidizing atmosphere is air or an air-N2 mixture; the reducing atmosphere is an H2-Ar mixture or an H2-N2 mixture; the calcination temperature under the oxidizing atmosphere is 300 to 800°C; the calcination temperature under the reducing atmosphere is 1100 to 1400°C.

[0041] Effects of the Invention

[0042] The metal hollow fiber membrane with inner and outer double opening structures of the present invention can provide a larger membrane specific surface area, promote surface reaction, and increase hydrogen flux by adopting a structure with opening layers on both sides and a dense separation layer in the middle. The metal hollow fiber membrane with inner and outer double opening structures prepared by the preparation method of the metal hollow fiber membrane with inner and outer double opening structures of the present invention has a large specific surface area on both sides, which can increase the reaction rate of the membrane surface, ultimately increase the hydrogen flux, and provide a larger hydrogen permeation rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a schematic diagram of the structure of a metal nickel hollow fiber membrane with inner and outer double opening structures according to an embodiment.

[0044] Figure 2 It is a schematic diagram of the structure of a precursor obtained through a precursor preparation step in a preparation method according to one embodiment.

[0045] Figure 3 The following is a scanning electron microscope photo of the precursor and the metal nickel hollow fiber membrane with double internal and external openings prepared in Example 1. Figure 3 A is a cross-sectional photograph of the precursor; Figure 3 B is the cross section of the metal nickel hollow fiber membrane with double openings inside and outside; Figure 3 C is the outer surface of the metal nickel hollow fiber membrane with inner and outer double-opening structure; Figure 3 D is an enlarged view of the outer surface of the metal nickel hollow fiber membrane with inner and outer double-opening structure; Figure 3 E is the inner surface of the metal nickel hollow fiber membrane with inner and outer double-opening structure; Figure 3 F is an enlarged view of the inner surface of the metal nickel hollow fiber membrane with inner and outer double-opening structures.

[0046] Figure 4 The following is a scanning electron microscope photo of the precursor prepared in Comparative Example 1 and the metal nickel hollow fiber membrane with holes on the outside. Figure 4 A is a cross-sectional photograph of the precursor; Figure 4 B is a cross-sectional photograph of a metal nickel hollow fiber membrane with holes opened on the outside; Figure 4 C is a photograph of the outer surface of a metal nickel hollow fiber membrane with holes opened on the outside; Figure 4 D is a photograph of the inner surface of a metal nickel hollow fiber membrane with holes opened on the outside.

[0047] Figure 5 The hydrogen permeation curves of the hollow fiber membranes prepared in Example 1 and Comparative Example 1 at different temperatures. DETAILED DESCRIPTION

[0048] In order to better understand the present invention, the present invention is further described in detail below in conjunction with the embodiments, but the scope of protection claimed in the present invention is not limited to the scope represented by the embodiments. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present disclosure.

[0049] In this specification, unless otherwise specified, percentages are by mass and temperatures are in degrees Celsius (°C).

[0050] The metal hollow fiber membrane with inner and outer double opening structures of the present invention has an outer porous layer, a dense separation layer and an inner porous layer from the outside to the inside, the outer porous layer and the inner porous layer have finger-like channels, and the inner porous layer forms a hollow inner cavity.

[0051] Figure 1 FIG. 1 is a schematic diagram of a cross-section of a metal hollow fiber membrane having an inner and outer double-opening structure according to an embodiment. Figure 1 As shown, the cross section of the metal nickel hollow fiber membrane with inner and outer double-opening structure has an outer porous layer 1, a dense separation layer 2 and an inner porous layer 3. Among them, the inner porous layer 3 has a first finger-shaped channel 4, the outer porous layer 1 has a second finger-shaped channel 5, and the inner porous layer 3 surrounds a hollow inner cavity 6. The metal hollow fiber membrane has two layer structures of the outer porous layer 1 and the inner porous layer 3 on the outer side and the inner side of the dense separation layer 2, respectively, and the inner porous layer 3 and the outer porous layer 1 contain the first finger-shaped channel 4 and the second finger-shaped channel 5, respectively, so that a large surface area can be obtained.

[0052] In the metal hollow fiber membrane with inner and outer double pore structure of one embodiment, the thickness of the outer porous layer can be, for example, in the range of 50 to 150 μm. In addition, in the outer porous layer, the length of the finger-like channels in the thickness direction of the outer porous layer is substantially the same as the thickness of the outer porous layer. In addition, the diameter of the cross section of the finger-like channels in the outer porous layer can be, for example, in the range of 5 to 50 μm.

[0053] In the metal hollow fiber membrane with inner and outer double pore structure of one embodiment, the thickness of the inner porous layer can be, for example, in the range of 5 to 150 μm. In addition, in the outer porous layer, the length of the finger-like channels in the thickness direction of the inner porous layer is substantially the same as the thickness of the inner porous layer. In addition, the diameter of the cross section of the finger-like channels in the inner porous layer can be, for example, in the range of 5 to 50 μm.

[0054] In the metal hollow fiber membrane with inner and outer double opening structures according to one embodiment, the thickness of the dense separation layer may be, for example, in the range of 1 to 25 μm.

[0055] In addition, when using the metal hollow fiber membrane with inner and outer double opening structure of the present invention for catalytic reaction, by containing the aforementioned metal hollow fiber membrane with inner and outer double opening structure, there are two reaction areas, namely the first reaction zone and the second reaction zone, thereby achieving a large catalyst packing density and improving the catalytic efficiency.

[0056] In addition, the metal hollow fiber membrane with inner and outer double opening structures of the present invention can be assembled into a metal hollow fiber membrane module with inner and outer double opening structures. In this case, the hollow fiber membrane can also have a shell, and the shell can be, for example, metal, quartz, ceramic, etc., without special restrictions, preferably a metal material, such as stainless steel.

[0057] The preparation method of the aforementioned metal hollow fiber membrane with inner and outer double opening structures comprises the following steps:

[0058] Metal powder casting liquid preparation step: dissolving a first organic polymer in a first organic solvent, adding metal powder, and stirring to obtain a metal powder casting liquid;

[0059] Temporary outer skin layer casting liquid preparation step: dissolving the second organic polymer in the second organic solvent, and then adding the outer skin layer regulator to obtain a temporary outer skin layer casting liquid;

[0060] A temporary inner skin layer casting liquid preparation step: dissolving a third organic polymer in a third organic solvent, and then adding an inner skin layer regulator to obtain a temporary inner skin layer casting liquid;

[0061] Precursor preparation process: after vacuum degassing the metal powder casting liquid, the temporary outer skin layer casting liquid, and the temporary inner skin layer casting liquid, the temporary outer skin layer casting liquid, the metal powder casting liquid, the temporary inner skin layer casting liquid, and the inner solidification liquid are extruded from the outside to the inside into the outer solidification liquid through a three-layer spinneret, and under the action of the inner solidification liquid and the outer solidification liquid, the temporary outer skin layer casting liquid, the metal powder casting liquid, and the temporary inner skin layer casting liquid are solidified to form a temporary outer skin layer, a metal powder layer, and a temporary inner skin layer, respectively, and the temporary inner skin layer is formed into a structure with a hollow inner cavity, the metal powder layer is coated on the outside of the temporary inner skin layer, and the temporary outer skin layer is coated on the surface of the metal powder layer, and then dried to obtain a precursor;

[0062] Calcination process: calcining the precursor in an oxidizing atmosphere to remove the temporary outer skin layer and the temporary inner skin layer, forming an outer porous layer and an inner porous layer having finger-like pores, and part of the metal in the outer porous layer and the inner porous layer is oxidized, and part of the organic matter in the metal powder layer adjacent to the surface of the temporary outer skin layer and the temporary inner skin layer is removed, and then calcining in a reducing atmosphere to reduce the oxidized metal to obtain a metal hollow fiber membrane with inner and outer double-opening structures.

[0063] Figure 2 The schematic diagram of the structure of the precursor obtained by the precursor preparation process in the preparation method of the metal hollow fiber membrane with inner and outer double opening structures in one embodiment is shown. Figure 2 As shown, in Figure 1 The structure of the metal nickel hollow fiber membrane with inner and outer double opening structures is further provided with a temporary outer skin layer 7 and a temporary inner skin layer 8. The temporary outer skin layer 7 and the temporary inner skin layer 8 are removed by a subsequent calcination process.

[0064] Hereinafter, each of the aforementioned steps will be described in sequence.

[0065] In the aforementioned step of preparing the metal powder casting solution, the first organic polymer may be, for example, at least one selected from the group consisting of polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide.

[0066] In the aforementioned step of preparing the metal powder casting solution, the first organic solvent may be, for example, at least one selected from the group consisting of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

[0067] In the aforementioned step of preparing the metal powder casting solution, the metal powder may be at least one selected from iron powder, nickel powder, and iron-nickel alloy powder.

[0068] The components of the metal powder casting liquid formed by the metal powder casting liquid modulation process can be the following composition, for example, the weight percentage of the first organic polymer is 5-10%, the weight percentage of the first organic solvent is 10-45%, and the weight percentage of the metal powder is 50-80%.

[0069] During the metal powder casting solution preparation process, the metal powder can be added in batches to facilitate uniform dispersion of the metal powder.

[0070] In the temporary outer skin layer casting solution preparation step, the second organic polymer may be at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide. The second organic polymer may be the same as or different from the first organic polymer, preferably the same.

[0071] In the temporary outer skin layer casting solution preparation step, the second organic solvent can be, for example, at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide. The second organic solvent can be the same as or different from the first organic solvent, preferably the same.

[0072] In the aforementioned temporary outer skin layer casting solution preparation step, the outer skin layer control agent may be at least one selected from water, ethanol, polyvinyl pyrrolidone, ammonium polymethacrylate, polymethyl methacrylate and phosphate ester.

[0073] In the aforementioned temporary outer skin layer casting liquid preparation process, the purpose of adding the outer skin layer regulator is to adjust the viscosity of the temporary outer skin layer casting liquid to the same or similar viscosity as the aforementioned metal powder casting liquid, thereby obtaining the same or similar fluidity as the metal powder casting liquid, so as to facilitate the formation of the precursor.

[0074] The temporary outer skin layer casting liquid prepared in the aforementioned temporary outer skin layer casting liquid preparation step can be, for example, of the following composition: for example, the weight percentage of the second organic polymer is 5-10%, the weight percentage of the second organic solvent is 50-90%, and the weight percentage of the outer skin layer regulator is 2%-40%.

[0075] In the aforementioned temporary inner skin layer casting solution preparation step, the third organic polymer may be at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide. The aforementioned third organic polymer may be the same as or different from the second organic polymer and the first organic polymer, and is preferably the same as at least one of the second organic polymer and the first organic polymer. Most preferably, the third organic polymer is the same as both the second organic polymer and the first organic polymer.

[0076] In the temporary inner skin layer casting solution preparation step, the third organic solvent may be, for example, at least one selected from N-methylpyrrolidone, N,N-dimethylamide, N,N-dimethylacetamide and dimethyl sulfoxide. The third organic solvent may be the same as or different from the second organic solvent and the first organic solvent, and is preferably the same as at least one of the second organic solvent and the first organic solvent. Most preferably, the third organic solvent is the same as the second organic solvent and the first organic solvent.

[0077] In the aforementioned temporary inner skin layer casting solution preparation step, the inner skin layer control agent may be at least one selected from water, ethanol, polyvinyl pyrrolidone, ammonium polymethacrylate, polymethyl methacrylate and phosphate ester.

[0078] The temporary inner skin layer casting liquid prepared in the aforementioned temporary inner skin layer casting liquid preparation step can be, for example, of the following composition: for example, the weight percentage of the third organic polymer is 5 to 10%, the weight percentage of the third organic solvent is 5 to 90%, and the weight percentage of the inner skin layer regulator is 2% to 40%.

[0079] In the aforementioned precursor preparation process, the internal coagulation liquid can be, for example, a mixture of a solvent and a non-solvent, and the aforementioned solvent can be, for example, at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. The aforementioned non-solvent can be, for example, at least one selected from water, ethanol, propanol, and ethylene glycol. In the aforementioned internal coagulation liquid, the mass percentage of the non-solvent can be, for example, 20 to 60%.

[0080] In the aforementioned precursor preparation process, the external coagulation liquid can be a mixture of a solvent and a non-solvent, the aforementioned solvent can be at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide, and the aforementioned non-solvent can be at least one selected from water, ethanol, propanol, and ethylene glycol. The mass percentage of the non-solvent in the aforementioned external coagulation liquid can be, for example, 20 to 90%.

[0081] In the aforementioned precursor preparation process, vacuum degassing can be performed under the condition of an ambient pressure of 0.01 to 0.1 MPa.

[0082] In the aforementioned precursor preparation step, the extrusion rate through the three-layer spinneret can be, for example, in the range of 1 to 15 mL / min.

[0083] In the aforementioned precursor preparation process, the aforementioned three-layer spinneret has a four-layer structure from the outside to the inside, wherein the diameter of the outermost layer can be, for example, 3 to 4 mm, the diameter of the second layer can be, for example, 2 to 3 mm, the diameter of the third layer can be, for example, 1 to 2 mm, and the diameter of the innermost layer can be, for example, in the range of 0.4 to 1 mm.

[0084] In the aforementioned precursor preparation step, the flow rate of the internal coagulation liquid may be, for example, in the range of 1 to 20 mL / min.

[0085] In one embodiment of the method for preparing a metal hollow fiber membrane with an inner and outer double-opening structure, the aforementioned calcination process can be carried out as follows: for example, the precursor obtained in the precursor preparation process is placed in an oxidizing atmosphere, and then heated at a certain heating rate to perform oxidative calcination to remove organic matter, and then heated at a certain heating rate in a reducing atmosphere to perform reduction calcination.

[0086] In the aforementioned calcining step, the oxidizing atmosphere can be, for example, air or an air-N2 mixed gas.

[0087] In the aforementioned calcination process, the reducing atmosphere may be, for example, a H2-Ar mixed gas or a H2-N2 mixed gas.

[0088] In the calcination step, the calcination temperature in the oxidizing atmosphere may be, for example, 300 to 800° C. The heating rate in the oxidizing atmosphere may be, for example, 1 to 20° C. / min. The calcination time in the oxidizing atmosphere may be, for example, 2 to 10 hours.

[0089] In the calcination step, the calcination temperature in the reducing atmosphere may be, for example, 1100 to 1400° C. The heating rate in the reducing atmosphere may be, for example, 1 to 20° C. / min. The calcination time in the reducing atmosphere may be, for example, 2 to 10 hours.

[0090] Example

[0091] Below, in order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its applications. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work belong to the scope of protection of the present application.

[0092] The materials used in the examples of this application can all be obtained commercially.

[0093] Example 1

[0094] Weigh 60 grams of N,N-dimethylacetamide solvent, then add 200 grams of nickel alloy powder with a particle size of 0.5 microns, and stir for 2 hours. During the stirring process, gradually add 16 grams of polysulfone and continue stirring for 72 hours to ensure that the polysulfone is completely dissolved, thereby obtaining a uniform and stable metal powder casting solution. The weight ratio of each component in the casting solution is metal powder: polymer: solvent = 1:0.08:0.3.

[0095] Weigh 60 grams of N,N-dimethylacetamide solvent, gradually add 16 grams of polysulfone while stirring and continue stirring for 72 hours to ensure that the polysulfone is completely dissolved, and then gradually add 4 grams of polyvinyl pyrrolidone as an outer skin layer regulator, stir evenly, so as to obtain a stable temporary outer skin layer casting solution. The weight ratio of each component in the temporary outer skin layer casting solution is outer skin layer regulator: polymer: solvent = 1:4:15.

[0096] 60 grams of N,N-dimethylacetamide solvent was weighed, 16 grams of polysulfone was gradually added while stirring, and the stirring was continued for 72 hours to ensure that the polysulfone was completely dissolved, and then 4 grams of polyvinyl pyrrolidone as an inner skin layer regulator was gradually added and stirred evenly to obtain a stable temporary inner skin layer casting solution. The weight ratio of each component in the temporary inner skin layer casting solution was inner skin layer regulator: polymer: solvent = 1:4:15.

[0097] Transfer the prepared metal powder casting liquid, temporary outer skin layer casting liquid, and temporary inner skin layer casting liquid to metal syringes respectively, and then place them in a vacuum box of 0.08Mpa for degassing for 1 hour. Use a high-pressure injection pump to inject the temporary outer skin layer casting liquid, metal powder casting liquid, temporary inner skin layer casting liquid and 50% NMP-50% H2O as an inner coagulation bath into four three-layer spinning heads with spinneret sizes of 4mm, 3.2mm, 1.8mm, and 1mm from outside to inside, respectively, at a speed of 3mL / min, 1.5mL / min, 1.5mL / min, and 10mL / min, and then extrude them into the outer coagulation bath to obtain a precursor. Among them, the outer coagulation bath is deionized water with a temperature of 25°C.

[0098] The precursor was cut into pieces of about 40 cm in length, straightened and dried naturally at room temperature for 24 hours. The precursor was then placed in an air atmosphere furnace for sintering. First, it was slowly heated to 600°C at a heating rate of 3°C per minute and continued for 2 hours to remove organic matter. Then a mixed gas containing 50% H2 and 50% N2 was introduced, and the temperature was raised to 1300°C at the same heating rate, and sintered at high temperature for 3 hours. Finally, the sample was naturally cooled to room temperature to obtain a metal hollow fiber membrane with double open-pore structures inside and outside. The cross-section and surface of the prepared hollow fiber membrane were scanned using a scanning electron microscope (PHENOMSCIENTIFIC Phenom Pro), and the scanning electron microscope photos obtained are shown in Figure 3 .

[0099] Figure 3 middle, Figure 3 A is a cross-sectional photograph of the prepared precursor. Figure 3 B is the cross section of the metal nickel hollow fiber membrane with double openings inside and outside. Figure 3 C is the outer surface of the metal nickel hollow fiber membrane with double openings inside and outside. Figure 3 D is an enlarged view of the outer surface of the metal nickel hollow fiber membrane with double inner and outer openings. Figure 3 E is the inner surface of the metal nickel hollow fiber membrane with double openings inside and outside. Figure 3 F is an enlarged view of the inner surface of the metal nickel hollow fiber membrane with double openings inside and outside. Figure 3It can be seen from B that in the metal nickel hollow fiber membrane with inner and outer double-opening structure prepared in Example 1, the thickness of the outer porous layer is about 50 μm, the thickness of the dense separation layer is about 10 μm, and the thickness of the inner porous layer is 40 μm.

[0100] Example 2

[0101] 60g of N,N-dimethylacetamide solvent, 200g of iron alloy powder with a particle size of 0.5 microns and 16g of polysulfone were prepared into a metal powder casting solution according to the method of Example 1. The same temporary outer skin layer casting solution and temporary inner skin layer casting solution as in Example 1 were also prepared.

[0102] The prepared metal powder casting liquid, temporary outer skin layer casting liquid, and temporary inner skin layer casting liquid are transferred to metal syringes respectively and spun in the manner of Example 1 to obtain a precursor. The above hollow fiber membrane precursor is cut into pieces of about 60 cm in length, straightened and dried naturally at room temperature for 15 hours, and then sintered in an atmosphere furnace. First, slowly heat to 800°C at a heating rate of 3°C per minute, and continue to treat for 1 hour to remove organic matter. Then introduce a mixed gas containing 50% H2 and 50% N2, and raise the temperature to 1400°C at the same heating rate, and sinter at high temperature for 3 hours. Finally, the sample is naturally cooled to room temperature to obtain an iron alloy hollow fiber membrane with double-opening structure inside and outside.

[0103] The hydrogen permeability of the iron alloy hollow fiber membrane with double internal and external openings prepared according to the method of Example 1 was measured. The hydrogen permeability was 35.7 mmol / m at 800°C. -2 s -1 , the hydrogen recovery rate is 29.2%.

[0104] Example 3

[0105] 60 grams of N, N-dimethylacetamide solvent, 200 grams of nickel alloy powder with a particle size of 0.5 microns and 20 grams of polyacrylonitrile are configured into a metal powder casting liquid according to the method of Example 1. The weight ratio of each component in the casting liquid is metal powder: polymer: solvent = 1: 0.1: 0.3. 60 grams of N, N-dimethylacetamide solvent, 20 grams of polyacrylonitrile and 5 grams of polyvinyl pyrrolidone as an outer skin layer regulator are configured into a temporary outer skin layer casting liquid according to the method of Example 1. The weight ratio of each component in the temporary outer skin layer casting liquid is outer skin layer regulator: polymer: solvent = 1: 4: 12. 60 grams of N, N-dimethylacetamide solvent, 20 grams of polyacrylonitrile and 5 grams of polyvinyl pyrrolidone as an inner skin layer regulator are configured into a temporary inner skin layer casting liquid according to the method of Example 1. The weight ratio of each component in the temporary inner skin layer casting liquid is outer skin layer regulator: polymer: solvent = 1: 4: 12.

[0106] The prepared metal powder casting liquid, temporary outer skin layer casting liquid, and temporary inner skin layer casting liquid are transferred to metal syringes respectively and spun in the manner of Example 1 to obtain a precursor. The above hollow fiber membrane precursor is cut into pieces of about 60 cm in length, straightened and naturally dried at room temperature for 15 hours, and then sintered in an atmosphere furnace. First, slowly heat to 600°C at a heating rate of 3°C per minute, and continue to treat for 2 hours to remove organic matter. Then introduce a mixed gas containing 50% H2 and 50% N2, and raise the temperature to 1300°C at the same heating rate, and sinter at high temperature for 3 hours. Finally, the sample is naturally cooled to room temperature to obtain a nickel alloy hollow fiber membrane with double-opening structure inside and outside.

[0107] The hydrogen permeability of the nickel alloy hollow fiber membrane with double internal and external openings prepared above was measured according to the method of Example 1. The hydrogen permeability was 49.5 mmol / m at 900°C. -2 s -1 , the hydrogen recovery rate is 44.8%.

[0108] Comparative Example 1

[0109] Weigh 60 grams of N,N-dimethylacetamide solvent, then add 200 grams of nickel alloy powder with a particle size of 0.5 microns, and stir for 2 hours. During the stirring process, gradually add 16 grams of polysulfone and continue stirring for 72 hours to ensure that the polysulfone is completely dissolved, thereby obtaining a uniform and stable metal powder casting solution. The weight ratio of each component in the casting solution is metal powder: polymer: solvent = 1:0.08:0.3.

[0110] Weigh 60 grams of N,N-dimethylacetamide solvent, gradually add 16 grams of polysulfone while stirring and continue stirring for 72 hours to ensure that the polysulfone is completely dissolved, and then gradually add 4 grams of polyvinyl pyrrolidone as an outer skin layer regulator, stir evenly, so as to obtain a stable temporary outer skin layer casting solution. The weight ratio of each component in the temporary outer skin layer casting solution is outer skin layer regulator: polymer: solvent = 1:4:15.

[0111] The prepared metal powder casting liquid and temporary outer skin layer casting liquid were transferred to metal syringes respectively, and then they were placed in a vacuum box of 0.08Mpa for degassing for 1 hour. Using a high-pressure injection pump, the temporary outer skin layer casting liquid, the metal powder casting liquid and 30% NMP-50% H2O as an inner coagulation bath were injected into three double-layer spinning heads with spinneret sizes of 4mm, 3.2mm and 1mm from the outside to the inside respectively at a speed of 3mL / min, 1.5mL / min and 10mL / min, and then extruded into deionized water at a temperature of 25°C as an outer coagulation bath to obtain a precursor.

[0112] The precursor was cut into pieces of about 40 cm in length, straightened and dried naturally at room temperature for 24 hours. The precursor was then placed in an air atmosphere furnace for sintering. First, it was slowly heated to 600°C at a heating rate of 3°C per minute for 2 hours to remove organic matter. Then a mixed gas containing 50% H2 and 50% N2 was introduced, and the temperature was raised to 1300°C at the same heating rate, and sintered at high temperature for 3 hours. Finally, the sample was naturally cooled to room temperature to obtain a metal hollow fiber membrane with holes on the outside.

[0113] The cross section and surface of the hollow fiber membrane were scanned using a scanning electron microscope (PHENOM SCIENTIFIC, Phenom Pro). The obtained scanning electron microscope photos are shown in Figure 4 .from Figure 4 It can be seen that the metal hollow fiber membrane with outer openings prepared in Comparative Example 1 does not have an inner porous layer.

[0114] The metal hollow fiber membrane with double openings inside and outside prepared in Example 1 and the metal hollow fiber membrane with openings outside prepared in Comparative Example 1 were subjected to the following gas permeability tests: a H2-He mixed gas containing 50% hydrogen was introduced outside the hollow fiber membrane, N2 was used as a purge gas, the H2 content in the purge gas was measured by gas chromatography, and the hydrogen permeation and hydrogen recovery rate at different temperatures were calculated. The results are shown in Figure 5 .from Figure 5 It can be seen that compared with Comparative Example 1, the hydrogen permeability of the metal hollow fiber membrane with inner and outer double-opening structure prepared in Example 1 is increased by 85% to 90% in almost all temperature ranges.

[0115] The above embodiments illustrate that the metal hollow fiber membrane with double inner and outer opening structures provided by the present invention has a much larger specific surface area than the metal hollow fiber membrane with single-side opening structures, and can effectively promote the dissociation and analysis process of hydrogen on the membrane surface, and can obtain a higher hydrogen permeability when the thickness of the separation layer is the same.

[0116] Obviously, the above embodiments of the present disclosure are merely examples for clearly illustrating the present disclosure, and are not limitations on the implementation methods of the present disclosure. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present disclosure are still within the protection scope of the present disclosure.

Claims

1. A metal hollow fiber membrane with double openings inside and outside. It is characterized in that It comprises an outer porous layer, a dense separation layer and an inner porous layer in sequence from the outside to the inside. The outer porous layer and the inner porous layer have finger-like channels, and the inner porous layer forms a hollow inner cavity.

2. A method for preparing the metal hollow fiber membrane with inner and outer double opening structures as claimed in claim 1, It is characterized in that The preparation method comprises the following steps: Metal powder casting liquid preparation step: dissolving a first organic polymer in a first organic solvent, adding metal powder, and stirring to obtain a metal powder casting liquid; Temporary outer skin layer casting liquid preparation step: dissolving the second organic polymer in the second organic solvent, and then adding the outer skin layer regulator to obtain the temporary outer skin layer casting liquid; A temporary inner skin layer casting liquid preparation step: dissolving a third organic polymer in a third organic solvent, and then adding an inner skin layer regulator to obtain a temporary inner skin layer casting liquid; Precursor preparation process: after vacuum degassing the metal powder casting liquid, the temporary outer skin layer casting liquid, and the temporary inner skin layer casting liquid, the temporary outer skin layer casting liquid, the metal powder casting liquid, the temporary inner skin layer casting liquid, and the inner solidification liquid are extruded from the outside to the inside into the outer solidification liquid through a three-layer spinneret, and under the action of the inner solidification liquid and the outer solidification liquid, the temporary outer skin layer casting liquid, the metal powder casting liquid, and the temporary inner skin layer casting liquid are solidified to form a temporary outer skin layer, a metal powder layer, and a temporary inner skin layer, respectively, and the temporary inner skin layer is formed into a hollow inner cavity structure, the metal powder layer is coated on the outside of the temporary inner skin layer, and the temporary outer skin layer is coated on the surface of the metal powder layer, and then dried to obtain a precursor; Calcination process: calcining the precursor in an oxidizing atmosphere to remove the temporary outer skin layer and the temporary inner skin layer, forming an outer porous layer and an inner porous layer having finger-like pores, and part of the metal in the outer porous layer and the inner porous layer is oxidized, and part of the organic matter in the metal powder layer adjacent to the surface of the temporary outer skin layer and the temporary inner skin layer is removed, and then calcining in a reducing atmosphere to reduce the oxidized metal to obtain a metal hollow fiber membrane with inner and outer double-opening structures.

3. The method for preparing the metal hollow fiber membrane with inner and outer double opening structures according to claim 2, in, In the metal powder casting solution preparation step, The first organic polymer is at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide; The first organic solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide; The metal powder is at least one selected from iron powder, nickel powder, and iron-nickel alloy powder; In the metal powder casting solution, the weight percentage of the first organic polymer is 5-10%, the weight percentage of the first organic solvent is 10-45%, and the weight percentage of the metal powder is 50-80%.

4. The method for preparing the metal hollow fiber membrane with inner and outer double opening structures according to claim 2, in, In the temporary outer skin layer casting liquid preparation step, The second organic polymer is at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide; The second organic solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide; The outer epidermis layer regulating agent is at least one selected from water, ethanol, polyvinyl pyrrolidone, ammonium polymethacrylate, polymethyl methacrylate and phosphate; In the temporary outer skin layer casting solution, the weight percentage of the second organic polymer is 5-10%, the weight percentage of the second organic solvent is 50-90%, and the weight percentage of the outer skin layer regulator is 2%-40%.

5. The method for preparing the metal hollow fiber membrane with inner and outer double opening structures according to claim 2, in, In the temporary inner skin layer casting solution preparation step, The third organic polymer is at least one selected from polysulfone, polyethersulfone, polyacrylonitrile and polyetherimide; The third organic solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide; The inner epidermis layer regulating agent is at least one selected from water, ethanol, polyvinyl pyrrolidone, ammonium polymethacrylate, polymethyl methacrylate and phosphate; In the temporary inner skin layer casting solution, the weight percentage of the third organic polymer is 5-10%, the weight percentage of the third organic solvent is 50-90%, and the weight percentage of the inner skin layer regulating agent is 2%-40%.

6. The method for preparing the metal hollow fiber membrane with inner and outer double opening structures according to claim 2, It is characterized in that In the precursor preparation process, the internal coagulation liquid is a mixture of a solvent and a non-solvent, the solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide, and the non-solvent is at least one selected from water, ethanol, propanol, and ethylene glycol; The mass percentage of the non-solvent in the internal coagulation liquid is 20-60%.

7. The method for preparing the metal hollow fiber membrane with inner and outer double opening structures according to claim 2, in, In the precursor preparation process, the external coagulation liquid is a mixture of a solvent and a non-solvent, the solvent is at least one selected from N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide, and the non-solvent is at least one selected from water, ethanol, propanol, and ethylene glycol; The mass percentage of the non-solvent in the external coagulation liquid is 20 to 90%.

8. The method for preparing the metal hollow fiber membrane with inner and outer double opening structures according to claim 2, It is characterized in that In the calcination process, the oxidizing atmosphere is air or air-N 2 Mixed gas; the reducing atmosphere is H 2 -Ar mixed gas or H 2 -N 2 mixed gas; the calcination temperature under the oxidizing atmosphere is 300 to 800°C; the calcination temperature under the reducing atmosphere is 1100 to 1400°C.

Citation Information

Patent Citations

  • Hollow fiber ceramic oxygen permeation membrane with dual composite asymmetric structure and preparation method thereof

    CN102895886A

  • High-flux polyvinylidene fluoride hollow fiber membrane

    CN103111189A

  • Nickel alloy hollow fiber membrane and preparation method and application thereof

    CN105195030A

  • Gradient porous self-supporting symmetrical ceramic membrane as well as preparation method and application thereof

    CN111085112A

  • Preparation method of metal hollow fiber catalytic membrane reactor, reactor and application thereof

    CN117899800A