Preparation method of hydroxyl cobalt oxide with high specific surface area

By controlling the feed time and pH, combined with the use of cobalt source and chelating agent, the high specific surface area of ​​cobalt oxide is quickly prepared, which solves the problems of long reaction time and the use of toxic precipitants in the existing process, and achieves high efficiency and low cost production effect.

CN119059573APending Publication Date: 2024-12-03GEM JIANGSU COBALT IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411096348.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing cobalt hydroxyoxide preparation process has a long reaction time and the use of toxic odor precipitants increases production costs and environmental protection pressure, making it difficult to prepare products with high specific surface area.

Method used

By controlling the feeding time of solution A and the pH of the mixed solution, a rapid feeding method is used, combined with the combination of cobalt source and chelating agent, the reaction is carried out at a rotation speed of 300-750rpm and a temperature of 45-85℃ to prepare hydroxyl groups with a high specific surface area Cobalt oxide.

Benefits of technology

The reaction time is significantly shortened, energy consumption and production costs are reduced, and cobalt hydroxyoxide with a specific surface area of ​​up to 149m2/g has been successfully prepared. The process is simple and the control points are few, which reduces the water treatment cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059573A_ABST
    Figure CN119059573A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of hydroxyl cobalt oxide with high specific surface area, and the preparation method comprises the following steps: obtaining a solution A and a solution B. The solution A comprises a cobalt source and a chelating agent, and the solution B comprises a precipitating agent and an oxidizing agent; controlling the feeding time of the solution A and the pH value of the mixed solution after feeding is completed, adding the solution A into the stirred solution B for reaction, and collecting a product. According to the method, a rapid feeding method is adopted, and the feeding time of the cobalt source precursor solution and the pH value of a reaction system obtained after feeding are controlled, so that the reaction time is remarkably shortened, the reaction energy consumption is reduced, the production cost is reduced, and the hydroxyl cobalt oxide with the specific surface area as high as 149 m < 2 > / g is successfully prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cobalt compound preparation, and in particular to a method for preparing cobalt oxyhydroxide with high specific surface area. Background Art

[0002] Lithium cobalt oxide is one of the key materials for lithium batteries. With the development of battery technology, the requirements for battery cycle life, stability, safety and other performance are becoming higher and higher, so more stringent requirements are put forward for the performance of lithium cobalt oxide. In addition, as one of the raw materials for preparing lithium cobalt oxide, the morphology and performance of cobalt oxyhydroxide have a very important influence on the performance of the final lithium cobalt oxide.

[0003] At present, industrial production of cobalt hydroxide oxide is by adding an oxidant / oxidizing gas during the reaction process, or by first preparing cobalt hydroxide and then oxidizing it. There are also some methods that improve the preparation process to obtain cobalt hydroxide oxide with better performance. For example, CN116062800A discloses a preparation method of cobalt hydroxide oxide and its application, which mainly controls the specific surface area of ​​cobalt hydroxide oxide by adjusting the amount of hydrogen peroxide added. The specific surface area of ​​the prepared cobalt hydroxide oxide is 65-109m 2 / g. However, this method has a long reaction time, and the alkali solution uses ammonia water to produce toxic odor, and the wastewater needs to go through a deammoniation process, which increases the cost.

[0004] It is necessary to improve the existing cobalt oxyhydroxide preparation process to obtain cobalt oxyhydroxide with a high specific area while shortening the feed and reaction time. Summary of the invention

[0005] The invention aims to prepare cobalt oxyhydroxide with a high specific surface area by greatly shortening the feeding and reaction time without using a precipitant with an odor.

[0006] In order to achieve the above object, the present invention provides a method for preparing cobalt oxyhydroxide with high specific surface area, comprising: Obtaining solution A and solution B, wherein solution A comprises a cobalt source and a chelating agent, and solution B comprises a precipitant and an oxidant; The feeding time of solution A and the pH of the mixed solution when the feeding is completed are controlled, solution A is added to the stirred solution B for reaction, and the product is collected.

[0007] Further, the feeding time is 1-10min; The pH of the mixed solution is 8.0-9.0.

[0008] Further, after the feeding of solution A is completed, the mixed solution is allowed to react for 1-3 minutes.

[0009] Furthermore, the reaction is carried out at a rotation speed of 300-750 rpm and a temperature of 45-85°C.

[0010] Further, the concentration of the cobalt source in the solution A is 45-130 g / L; The mass of the chelating agent in the solution A is 0.01-0.05 times the mass of the cobalt source.

[0011] Further, the cobalt source includes at least one of cobalt chloride, cobalt sulfate, cobalt nitrate, and cobalt acetate; The chelating agent includes at least one of disodium ethylenediaminetetraacetate, ethylenediaminetetraacetic acid, and sodium nitrilotriacetate.

[0012] Furthermore, the solution B is obtained by mixing a precipitant solution with a mass concentration of 3%-8% and an oxidant solution with a mass concentration of 5%-10% in a volume ratio of 1:1-5.

[0013] Further, the precipitant includes at least one of sodium hydroxide, potassium hydroxide, and lithium hydroxide; The oxidant includes at least one of sodium hypochlorite, potassium hypochlorite and lithium hypochlorite.

[0014] The invention also provides cobalt oxyhydroxide with a high specific surface area, which is prepared by the above method.

[0015] The present invention also provides the use of the above-mentioned cobalt oxyhydroxide with high specific surface area in the preparation of lithium cobalt oxide.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention adopts a rapid feeding method, and by controlling the feeding time of the cobalt source precursor solution and the pH of the reaction system obtained after the feeding is completed, it not only significantly reduces the reaction time, reduces the reaction energy consumption, and reduces the production cost, but also successfully prepares a cobalt source precursor with a specific surface area of ​​up to 149m 2 / g of cobalt oxyhydroxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 The microscopic morphology of cobalt oxyhydroxide prepared in Example 1 of the present invention is shown; Figure 2 The microscopic morphology of cobalt oxyhydroxide prepared in Example 2 of the present invention is shown; Figure 3 The microscopic morphology of cobalt oxyhydroxide prepared in Example 3 of the present invention is shown; Figure 4 The microscopic morphology of cobalt oxyhydroxide prepared in Example 4 of the present invention is shown; Figure 5 The microscopic morphology of cobalt oxyhydroxide prepared in Example 5 of the present invention is shown; Figure 6 The microscopic morphology of cobalt oxyhydroxide prepared in Example 6 of the present invention is shown; Figure 7 The microscopic morphology of cobalt oxyhydroxide prepared in Example 7 of the present invention is shown; Figure 8 The microscopic morphology of cobalt oxyhydroxide prepared in Comparative Example 1 of the present invention is shown; Fig. 9 The microscopic morphology of cobalt oxyhydroxide prepared in Comparative Example 2 of the present invention is shown; Fig.10 The microscopic morphology of cobalt oxyhydroxide prepared in Comparative Example 3 of the present invention is shown; Fig.11 The microscopic morphology of cobalt oxyhydroxide prepared in Comparative Example 4 of the present invention is shown; Fig.12 The microscopic morphology of cobalt oxyhydroxide prepared in Comparative Example 5 of the present invention is shown; Fig.13 The microscopic morphology of cobalt oxyhydroxide of Comparative Example 6 of the present invention is shown. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0020] The following will be combined with the specific embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and disodium ethylenediaminetetraacetate (EDTA-2Na) in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare sodium hydroxide solution and sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:1 to obtain solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0022] Example 2 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare a sodium hydroxide solution and a sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:3 to obtain a solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0023] Example 3 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, dissolving sodium hydroxide and sodium hypochlorite in water to prepare sodium hydroxide solution and sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:5 to obtain solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0024] Example 4 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 60 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare a sodium hydroxide solution and a sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:3 to obtain a solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0025] Example 5 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt sulfate heptahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare a sodium hydroxide solution and a sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:3 to obtain a solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0026] Example 6 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare a sodium hydroxide solution and a sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:3 to obtain a solution B; Step 3, add solution B into the reactor, the amount added is 50% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 10 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0027] Example 7 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.01 times the mass of cobalt chloride hexahydrate; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare a sodium hydroxide solution and a sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:3 to obtain a solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0028] Comparative Example 1 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare a sodium hydroxide solution and a sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:3 to obtain a solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue the reaction for 10 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high specific surface area cobalt hydroxide oxide.

[0029] Comparative Example 2 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare sodium hydroxide solution and sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution at a volume ratio of 1:10 to obtain solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 3 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0030] Comparative Example 3 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate and EDTA-2Na in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L, and EDTA-2Na accounts for 0.05 times the mass of cobalt chloride hexahydrate; Step 2, dissolving sodium hydroxide and sodium hypochlorite in water to prepare sodium hydroxide solution and sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:5 to obtain solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 15 minutes, evenly and quickly introduce solution A into the reactor through the four feeding ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue to react for 2 minutes, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high-specific surface area cobalt hydroxide oxide.

[0031] The microscopic morphologies of Examples 1 to 7 and Comparative Examples 1 to 3 of the present invention were observed using a scanning electron microscope, and the results were as follows: Figure 1-10 shown.

[0032] The specific surface areas of the materials prepared in the examples and comparative examples were tested by nitrogen adsorption and desorption experiments. The results are shown in Table 1.

[0033] Comparative Example 4 A method for preparing cobalt oxyhydroxide with high specific surface area, comprising the following steps: Step 1, dissolving cobalt chloride hexahydrate in water to prepare solution A, wherein the concentration of cobalt chloride hexahydrate in solution A is 130 g / L; Step 2, respectively dissolving sodium hydroxide and sodium hypochlorite in water to prepare a sodium hydroxide solution and a sodium hypochlorite solution with mass concentrations of 5% and 8%, respectively, and mixing the sodium hydroxide solution and the sodium hypochlorite solution in a volume ratio of 1:3 to obtain a solution B; Step 3, add solution B into the reactor, the amount added is 30% of the volume of the reactor; Step 4, start the heating and stirring of the reactor, raise the temperature of solution B to 75°C and keep stirring at a stirring rate of 600 rpm, and within 0.5 min, evenly and quickly introduce solution A into the reactor through the four feed ports of the reactor. When the feeding is completed, the pH of the mixed solution is 8.5, and then continue the reaction for 2 min, centrifuge, wash, dry, and crush through a 200-mesh sieve to obtain high specific surface area cobalt hydroxide oxide.

[0034] Comparative Example 5 A method for preparing cobalt oxyhydroxide, according to a traditional preparation method, the steps are as follows: S1. Weigh 1816 g of cobalt chloride hexahydrate, add pure water, dilute to 4 L, filter to remove solid impurities, and obtain a clean cobalt chloride solution; S2, measure 30 mL of hydrogen peroxide and add it to the cobalt chloride solution, mix well to obtain a mixed solution A; S3, measuring 1140 mL of 10% ammonia aqueous solution, adding it to 2000 mL of 30% sodium hydroxide aqueous solution, and mixing them to obtain a mixed solution B; S4. Use a peristaltic pump to pump the mixed solution B into the reactor as the bottom liquid within 10 minutes. Set the speed to 600r / min, the temperature to 60°C, and the compressed air flow rate to 5L / min. S5. At 60° C., use a peristaltic pump to pump the mixed solution A into the reactor in step S4 within 30 minutes, and keep the mixture warm for 2 hours to obtain a cobalt oxyhydroxide slurry; S6. Wash the sodium content of the cobalt oxyhydroxide slurry to below 500 ppm, transfer it to a 100° C. drying oven and dry it for 12 hours, and crush it through a 200-mesh sieve to obtain cobalt oxyhydroxide.

[0035] Comparative Example 6 Commercially available cobalt oxyhydroxide.

[0036] Table 1 Specific surface area test results

[0037] Combination Figure 1 , Figure 2 , Figure 3 and Fig. 9 , and the relevant data in Table 1, except for the different compositions of liquid B, the other conditions of Examples 1 to 3 and Comparative Example 2 are the same, which shows that the proportion of sodium hypochlorite in liquid B has a great influence on the morphology and specific surface area of ​​cobalt oxyhydroxide. At the same time, if the proportion of sodium hypochlorite is too high, it will make the cobalt oxyhydroxide difficult to be ground and crushed ( Fig. 9 ). Combined Figure 2 and Figure 4, as well as the specific surface areas of Example 2 and Example 4, it is shown that under the same other conditions, a higher cobalt concentration is beneficial to the preparation of cobalt oxyhydroxide with a high specific surface area. This is because the higher the cobalt concentration, the local supersaturation of cobalt ions after entering the reaction system, which is conducive to the formation of crystal nuclei, and the finer the primary particles, the higher the specific surface area of ​​the product. Figure 2 and Figure 5 , as well as the specific surface areas of Example 2 and Example 5, it is shown that under the same reaction conditions, the selection of cobalt source can further optimize the specific surface area. Figure 2 , Figure 6 , Fig.10 , as well as the specific surface areas of Example 2, Example 6 and Comparative Example 3, it is shown that the feeding time of solution A has an effect; the shorter the feeding time, that is, the faster the feeding speed, the local supersaturation of cobalt ions after entering the reaction system, which is conducive to the formation of crystal nuclei, and the smaller the primary particles, the higher the specific surface area of ​​the product. Figure 2 and Figure 7 , as well as the specific surface areas of Example 2 and Example 7, indicating that a shorter reaction time can inhibit the growth of crystal nuclei, so that the product has a higher specific surface area. Figure 2 , Figure 7 and Figure 8 , as well as the specific surface areas of Example 2, Example 7 and Comparative Example 1. Compared with Example 2, in Comparative Example 1, no EDTA-2Na was added to solution A, and its specific surface area decreased significantly. This is because EDTA-2Na can stabilize cobalt ions through coordination, reduce its hydrolysis rate, and make the product more uniform and fine, thereby increasing the specific surface area; compared with Example 2, the amount of EDTA-2Na added in Example 7 is less, and the coordination effect on cobalt ions is weakened, which is not conducive to making the product finer and more uniform.

[0038] The feeding time of Comparative Example 4 is only 0.5 min. Compared with the regular shape of Example 2, it is almost completely unable to be formed and has the lowest specific surface area. Fig.12 It can be seen that in Comparative Example 5 using the traditional preparation method, the cobalt oxyhydroxide prepared is obviously agglomerated and has a larger particle size. Fig.13 The morphology of the commercial cobalt oxyhydroxide of Comparative Example 6 is shown, which has a distinct smaller particle size lamellar structure, but its specific surface area is only 58.5 m 2 / g.

[0039] In summary, the present invention adopts a rapid feeding method, by controlling the feeding time of the cobalt source precursor solution and the pH of the reaction system obtained after the feeding is completed, which not only significantly reduces the reaction time (total feeding time, the overall reaction time does not exceed 15min), reduces the reaction energy consumption, and reduces the production cost, but also successfully prepares a cobalt source precursor solution with a specific surface area of ​​up to 149m 2 / g of cobalt hydroxide oxide. At the same time, the preparation method of the present invention is very simple, with few process control points, low pH of the mother liquor, low cobalt ion concentration in the cobalt source precursor, and low subsequent water treatment cost.

[0040] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing cobalt oxyhydroxide with high specific surface area, characterized in that: include, Obtaining solution A and solution B, wherein solution A comprises a cobalt source and a chelating agent, and solution B comprises a precipitant and an oxidant; The feeding time of solution A and the pH of the mixed solution when the feeding is completed are controlled, solution A is added to the stirred solution B for reaction, and the product is collected.

2. The method for preparing cobalt oxyhydroxide with high specific surface area according to claim 1, characterized in that: The feeding time is 1-10min; The pH of the mixed solution is 8.0-9.

0.

3. The method for preparing cobalt oxyhydroxide with high specific surface area according to claim 1, characterized in that: After the feeding of solution A was completed, the mixed solution was allowed to react for 1-3 minutes.

4. The method for preparing cobalt oxyhydroxide with high specific surface area according to claim 1, characterized in that: The reaction is carried out at a rotation speed of 300-750 rpm and a temperature of 45-85°C.

5. The method for preparing cobalt oxyhydroxide with high specific surface area according to claim 1, characterized in that: The concentration of the cobalt source in the solution A is 45-130 g / L; The mass of the chelating agent in the solution A is 0.01-0.05 times the mass of the cobalt source.

6. The method for preparing cobalt oxyhydroxide with high specific surface area according to claim 1, characterized in that: The cobalt source includes at least one of cobalt chloride, cobalt sulfate, cobalt nitrate and cobalt acetate; The chelating agent includes at least one of disodium ethylenediaminetetraacetate, ethylenediaminetetraacetic acid, and sodium nitrilotriacetate.

7. The method for preparing cobalt oxyhydroxide with high specific surface area according to claim 1, characterized in that: The solution B is obtained by mixing a precipitant solution with a mass concentration of 3%-8% and an oxidant solution with a mass concentration of 5%-10% in a volume ratio of 1:1-5.

8. The method for preparing cobalt oxyhydroxide with high specific surface area according to claim 1, characterized in that: The precipitant includes at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide; The oxidant includes at least one of sodium hypochlorite, potassium hypochlorite and lithium hypochlorite.

9. A cobalt oxyhydroxide with a high specific surface area, characterized in that: The method is prepared by any one of claims 1 to 8.

10. Use of the cobalt oxyhydroxide with high specific surface area as claimed in claim 9 in the preparation of lithium cobalt oxide.

Citation Information

Patent Citations

  • Preparation method and application of hydroxyl cobalt oxide

    CN116062800A