High-heat-dissipation double-sided chip-on-film and chemical etching method thereof

The double-sided flip chip film with copper-plated via holes and a chemical etching process enhances thermal conductivity, effectively addressing the low heat dissipation efficiency of existing chip-on-film technologies by improving heat conduction and dissipation.

CN119072005AInactive Publication Date: 2024-12-03ZHEJIANG JINGYIN ELECTRONIC TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411321920.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing chip-on-film technologies suffer from low heat dissipation efficiency due to the insulating effect of adhesives, which hampers effective heat conduction and dissipation through bonded heat sinks.

Method used

A double-sided flip chip film with copper-plated via holes on both sides of the substrate, combined with a chemical etching process to form conductive layers and avoid circuit openings, enhancing thermal conductivity.

Benefits of technology

The copper-plated structure significantly improves heat dissipation efficiency by leveraging copper's thermal conductivity, addressing the low efficiency of existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072005A_ABST
    Figure CN119072005A_ABST
Patent Text Reader

Abstract

The invention discloses a high-heat-dissipation double-sided chip-on-film and a chemical etching method thereof, the high-heat-dissipation double-sided chip-on-film comprises a base material and a via hole, circuit boards are arranged on the upper side and the lower side of the base material, a chip is arranged on the side face, away from the base material, of each circuit board, the via hole is formed in the circuit boards and the base material in a penetrating mode, and heat conduction copper is arranged in the via hole. According to the high-heat-dissipation double-sided chip-on-film and the chemical etching method thereof, circuit holes are avoided in the circuit board and the base material through chemical etching, and then copper is plated in the via holes, that is, the heat conduction performance of copper is utilized to help heat dissipation, so that the heat dissipation efficiency of a device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chip-on-chip films, in particular to a double-sided chip-on-chip film with high heat dissipation performance and a chemical etching method thereof. Background Art

[0002] Chip-on-film is a soft film assembly technology for fixing the driver IC on a flexible circuit board. It is a technology that uses a soft additional circuit board as a chip packaging carrier to connect the chip with the flexible substrate circuit. After searching, it is found that the typical chip-on-film in the prior art is a chip-on-film and display device disclosed in publication number CN103887255A. The chip-on-film includes a driver chip body and a substrate. A heat insulation disk is provided at the bottom of the driver chip body. The driver chip body and the substrate are connected through the heat insulation disk. A heat dissipation structure is provided on the substrate, and the heat insulation disk is connected to the heat dissipation structure. Its main feature is that the heat dissipation effect of the chip-on-film is enhanced by setting a heat dissipation structure, thereby reducing the temperature and avoiding the use failure of the driver chip due to excessive temperature.

[0003] In summary, the existing flip chip film mainly helps the circuit board to conduct heat and dissipate heat by bonding a heat sink to the circuit board. However, since the adhesive has a certain heat insulation effect, the heat dissipation efficiency is low. In view of the above problems, the existing equipment needs to be improved. Summary of the invention

[0004] The purpose of the present invention is to provide a double-sided flip chip film with high heat dissipation and a chemical etching method thereof, so as to solve the problem that the existing flip chip film mentioned in the above background technology mainly helps it to conduct heat and dissipate heat by bonding a heat sink on the circuit board, but because the adhesive has a certain heat insulation effect, the heat dissipation efficiency is low.

[0005] To achieve the above object, the present invention provides the following technical solution: a double-sided flip chip film with high heat dissipation performance, comprising a substrate and a via hole, Circuit boards are arranged on both the upper and lower sides of the substrate, and a chip is arranged on one side of the circuit board away from the substrate. The via hole is opened on the circuit board and the substrate, and the via hole is filled with copper by electroplating.

[0006] A chemical etching method for a high heat dissipation double-sided flip chip film is applied to the high heat dissipation double-sided flip chip film as described above, comprising the following steps: S1. Raw material preparation: Select a suitable double-sided soft copper-clad substrate as the starting material, check the material quality to ensure there are no defects, and perform necessary pretreatment; S2, dry film lamination: accurately align the dry film and substrate, and use a laminating machine to press the dry film onto the substrate; S3, via hole exposure: the via hole position on the dry film is exposed through a photomask to cause a chemical reaction of the photosensitive material in the exposed part; S4, via hole development: using a developer to remove the dry film portion that is no longer needed after exposure, exposing the via hole position on the substrate; S5. Etching the copper surface of the via hole: etching the copper surface using an etchant through a chemical etching device; S6, Dry film stripping: Use stripping fluid or mechanical methods to remove the remaining dry film; S7, chemically etching PI vias: chemically etching the polyimide (PI) layer by chemical etching equipment to form a final via structure; S8, Black shadow: Use black shadow agent, which contains unique additives and conductive colloidal substances (graphite), attached to the wall of PI via hole to form a conductive layer function; S9, dry film lamination: align the dry film and substrate, and use a laminating machine at a certain temperature and pressure to firmly adhere the dry film to the substrate; S10, circuit exposure: exposing the dry film through a photomask to cause a chemical reaction in the photosensitive material of the exposed part; S11, circuit development: using a developer to remove the dry film portion that is no longer needed after exposure, exposing the copper layer on the substrate, and forming a circuit pattern; S12, Circuit copper plating: Use electroplating equipment to control the composition, temperature and current density of the electroplating solution, electroplate a layer of copper on the exposed copper layer, and also fill the via holes with copper plating; S13, dry film stripping: Use stripping liquid or mechanical method to remove the remaining dry film to expose the complete circuit pattern; S14, remove the bottom copper: remove the bottom copper of the raw material without layer increase to form the circuit; S15, Tinning: Use a tin-containing acid solution on the copper surface with circuits, and use a special tinning equipment to chemically deposit a layer of tin on the copper surface. The purpose is to bind the IC and form a eutectic package with the IC's gold bumps; S16, Solder mask printing: Use screen printing in the non-bonding area to print a layer of solder mask on the conductive area of ​​the circuit to prevent the outer layer from oxidation or contact short circuit.

[0007] Compared with the prior art, the invention has the following beneficial effects: the high heat dissipation double-sided chip-on-chip film and the chemical etching method thereof, The present invention can effectively solve the problem of low heat dissipation efficiency in the existing chip-on-chip film by cooperating with its internal copper-plated structure. The present invention mainly helps heat conduction and heat dissipation by bonding a heat sink to the circuit board, but the adhesive has a certain heat insulation effect, thereby resulting in low heat dissipation efficiency. By chemically etching to avoid circuit openings on the circuit board and the substrate, and then copper is plated inside the conductive hole, the thermal conductivity of copper is used to help it dissipate heat, thereby improving the heat dissipation efficiency of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 It is a cross-sectional schematic diagram of the present invention; Figure 2 This is a schematic diagram of a finished chip-on-chip film produced by the present invention. DETAILED DESCRIPTION

[0009] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0010] See also Figure 1-2 The present invention provides a technical solution: a high heat dissipation double-sided chip-on-chip film and a chemical etching method thereof, Example

[0011] A double-sided flip chip film with high heat dissipation, circuit boards are arranged on the upper and lower sides of a substrate, and a chip is arranged on the side of the circuit board away from the substrate, a via hole is opened on the circuit board and the substrate, and copper is plated in the via hole, and the circuit opening is avoided on the circuit board and the substrate by chemical etching, the diameter of the via hole is 20-50μm, and then copper is plated inside the via hole, that is, the thermal conductivity of copper is used to help it dissipate heat, thereby improving the heat dissipation efficiency of the device. Example

[0012] This embodiment is a further description of the above embodiment. It should be understood that this embodiment includes all the aforementioned technical features and is further described in detail.

[0013] A chemical etching method for a high heat dissipation double-sided flip chip film is applied to the high heat dissipation double-sided flip chip film as described above, comprising the following steps: S1. Raw material preparation: Select suitable materials as starting materials, check the quality of materials to ensure that there are no defects, and perform necessary pretreatments, using solvents, sandpaper or mechanical polishing to clean the surface of the substrate; S2, dry film lamination: accurately align the dry film and substrate, and use a laminator to press the dry film (a film containing photosensitive substances) onto the substrate in preparation for subsequent pattern exposure; S3, via hole exposure: the via hole position on the dry film is exposed through a photomask to cause a chemical reaction of the photosensitive material in the exposed part; S4, via hole development: using a developer to remove the dry film portion that is no longer needed after exposure, exposing the via hole position on the substrate; S5. Etching the copper surface of the via hole: etching the copper surface using an etchant through a chemical etching device; S6, Dry film stripping: Use stripping fluid or mechanical methods to remove the remaining dry film; S7, chemical etching of PI vias: chemically etching the polyimide (PI) layer by chemical etching equipment to process surface defects such as burrs on the PI layer to form the final via structure; S8, Black shadow: Use black shadow agent, which contains unique additives and conductive colloidal substances (graphite), attached to the wall of PI via hole to form a conductive layer function; S9, dry film lamination: align the dry film and substrate, and use a laminating machine at a certain temperature and pressure to firmly adhere the dry film to the substrate; S10, circuit exposure: exposing the dry film through a photomask to cause a chemical reaction in the photosensitive material of the exposed part; S11, circuit development: using a developer to remove the dry film portion that is no longer needed after exposure, exposing the copper layer on the substrate, and forming a circuit pattern; S12, circuit copper plating: before copper electroplating, use chemical agents for activation treatment, and coat a conductive layer on the hole wall and the circuit. Use electroplating equipment to control the composition, temperature and current density of the electroplating solution, electroplate a layer of copper on the exposed copper layer, and also fill the conductive hole with copper plating; and after the electroplating is completed, take the substrate out of the electroplating tank and clean it to remove the electroplating solution residue and impurities on the surface, and perform deoxidation treatment to remove the oxides generated during the electroplating process; S13, dry film stripping: Use stripping liquid or mechanical method to remove the remaining dry film to expose the complete circuit pattern; S14, remove the bottom copper: remove the bottom copper of the raw material without layer increase to form the circuit; S15, Tinning: Use a tin-containing acid solution on the copper surface with circuits, and use a special tinning equipment to chemically deposit a layer of tin on the copper surface. The purpose is to bind the IC and form a eutectic package with the IC's gold bumps; S16. Solder resist ink printing: Use screen printing in non-bonding areas to print a layer of solder resist ink on the conductive area of ​​the circuit to prevent the outer layer of the circuit from oxidation or contact short circuit. The solder resist ink is used to form a protective film on the circuit board, and needs to be dried and cured after printing to form a solid solder resist layer. The solder resist ink is divided into thermal curing type, UV curing type and liquid photosensitive type according to the curing method.

[0014] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A double-sided flip chip film with high heat dissipation, comprising a substrate and a via, Features: Circuit boards are arranged on both the upper and lower sides of the substrate, and a chip is arranged on one side of the circuit board away from the substrate. The via hole is opened on the circuit board and the substrate, and the via hole is filled with copper by electroplating.

2. A chemical etching method for a double-sided chip-on-chip film with high heat dissipation, which is used to prepare a double-sided chip-on-chip film with high heat dissipation as claimed in claim 1, It is characterized in that The following steps are involved: S1. Raw material preparation: Select a suitable double-sided soft copper-clad substrate as the starting material, check the material quality to ensure there are no defects, and perform necessary pretreatment; S2, dry film lamination: accurately align the dry film and substrate, and use a laminating machine to press the dry film onto the substrate; S3, via hole exposure: the via hole position on the dry film is exposed through a photomask to cause a chemical reaction of the photosensitive material in the exposed part; S4, via hole development: using a developer to remove the dry film portion that is no longer needed after exposure, exposing the via hole position on the substrate; S5. Etching the copper surface of the via hole: etching the copper surface using an etchant through a chemical etching device; S6, Dry film stripping: Use stripping fluid or mechanical methods to remove the remaining dry film; S7. Chemically etching PI via holes: chemically etching the polyimide layer through chemical etching equipment to form a final via hole structure.

3. A chemical etching method for double-sided chip-on-chip film with high heat dissipation according to claim 2, It is characterized in that Also includes the steps: S8, Black shadow: Use black shadow agent, which contains unique additives and conductive colloidal substances, to adhere to the wall of PI via hole to form a conductive layer function; S9, dry film lamination: align the dry film and substrate, and use a laminating machine at a certain temperature and pressure to firmly adhere the dry film to the substrate; S10, circuit exposure: exposing the dry film through a photomask to cause a chemical reaction in the photosensitive material of the exposed part; S11, circuit development: Use developer to remove the dry film part that is no longer needed after exposure, expose the copper layer on the substrate, and form a circuit pattern.

4. A chemical etching method for double-sided chip-on-chip film with high heat dissipation according to claim 3, It is characterized in that Also includes the steps: S12, Circuit copper plating: Use electroplating equipment to control the composition, temperature and current density of the electroplating solution, electroplate a layer of copper on the exposed copper layer, and also fill the via holes with copper plating; S13, dry film stripping: Use stripping liquid or mechanical method to remove the remaining dry film to expose the complete circuit pattern; S14, remove the bottom copper: remove the bottom copper of the raw material without the added layer to form the circuit.

5. A chemical etching method for double-sided chip-on-chip film with high heat dissipation according to claim 4, It is characterized in that Also includes the steps: S15, Tinning: Use a tin-containing acid solution on the copper surface with circuits, and use a special tinning equipment to chemically deposit a layer of tin on the copper surface. The purpose is to bind the IC and form a eutectic package with the IC's gold bumps; S16, Solder mask printing: Use screen printing in the non-bonding area to print a layer of solder mask on the conductive area of ​​the circuit to prevent the outer layer from oxidation or contact short circuit.

Citation Information

Patent Citations

  • Camera-shooting module

    CN103037150A

  • Printed circuit board with bonded IC

    CN2717170Y

  • Printed circuit board

    JP1993160527A

  • Method of forming through holes in printed wiring board substrates

    US5352325A