Zeolite, method for producing zeolite, composition, liquid sealant, resin composite material, sealing material, method for producing sealing material, and electronic device

By combining spherical aluminosilicate phase zeolite with particle size of 0.05 μm to 1.0 μm and resin, the thermal expansion coefficient and injection properties of the liquid sealant are solved, and a resin composite with low viscosity and low thermal expansion coefficient is realized, suitable for narrow gaps Filling improves the heat resistance and reliability of the sealing material.

CN119072454APending Publication Date: 2024-12-03MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380036006.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The thermal expansion coefficient of silica fillers in existing liquid sealants is not low enough, resulting in insufficient thermal cycle resistance. At the same time, the increased viscosity of the filler material leads to a decrease in the injection property, and it cannot be completely filled in the narrow gap, forming a void, affecting the reliability of the solder. sex.

Method used

The spherical aluminosilicate zeolite with a particle size of 0.05 μm or more and less than 1.0 μm is combined with an epoxy resin or a polyimide resin to prepare the zeolite through the hydrothermal synthesis and sintering process, and the silane coupling agent is combined to control the particle size. and shape, forming a composition with low viscosity and low coefficient of thermal expansion.

Benefits of technology

The resin composite material with low viscosity and low thermal expansion coefficient can be fully filled in the narrow gap without forming a void, which improves the heat resistance and injection properties of the sealing material, and enhances the reliability of the solder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072454A_ABST
    Figure CN119072454A_ABST
Patent Text Reader

Abstract

A zeolite which is a spherical aluminosilicate, has a particle diameter of 0.05 [mu] m or more but less than 1.0 [mu] m, and has d6r as CBU. The present invention can provide a zeolite having a small coefficient of thermal expansion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to zeolite, a method for producing zeolite, a composition, a liquid sealant, a resin composite material, a sealing material, a method for producing a sealing material and an electronic device. Background Art

[0002] Liquid sealants used as bottom filling materials are required to have excellent injectability, adhesion, curability, storage stability, etc., and no voids. In addition, the parts sealed by the liquid sealant are required to have excellent moisture resistance, heat cycle resistance, reflow resistance, crack resistance, warping resistance, etc. In order to meet the above requirements, liquid sealants with epoxy resin as the main agent are widely used as bottom filling materials.

[0003] In addition, it is known that in order to improve the moisture resistance and heat cycle resistance, especially the heat cycle resistance, of the parts sealed by the liquid sealant, a filling material formed by an inorganic substance such as a silica filler (hereinafter referred to as an "inorganic filler") is used in the liquid sealant to control the difference in thermal expansion coefficients between the substrate made of organic materials such as epoxy resin and the semiconductor element, and to strengthen the bump electrode (see patent document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-56070 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The thermal expansion coefficient of liquid sealants using inorganic fillers such as silica fillers is not low enough, and it is required to further reduce the thermal expansion coefficient from the viewpoint of heat cycle resistance, etc. In addition, zeolite is known as an inorganic filler with a low thermal expansion coefficient, but the viscosity of the liquid composition containing zeolite tends to increase, and the injectability when used as an underfill material is reduced. Therefore, it is difficult to obtain a liquid sealant that reduces the thermal expansion coefficient of the cured product and has good injectability.

[0009] In addition, in the application of liquid sealants that fill gaps of about tens of μm, such as bottom filling materials suitable for narrow gaps, if the particle size of the inorganic filler is too large, the liquid composition will not be able to spread in the gap due to the inorganic filler and cannot be completely filled in the desired gap, which may form voids.

[0010] It is generally believed that if a gap is formed during filling of the liquid sealant, only a portion of the solder is exposed, which may cause the solder to break and adversely affect reliability. Therefore, the particle size of the inorganic filler used in the liquid sealant is preferably less than about 1 / 10 of the gap width.

[0011] It is expected that the miniaturization of devices and components constituting the devices will continue to advance in the future, and semiconductor chips are also expected to be miniaturized, thinned, and 3D stacked. It is believed that in such applications, it is necessary to install in a gap of about 25μm, which is narrower than the current narrow gap of about 50μm. In other words, it is necessary to develop a small-particle negative expansion filler that can also cope with such applications.

[0012] Therefore, an object of the present invention is to provide a composition having a low viscosity and a low thermal expansion coefficient after curing, and a resin composite material obtained by curing the composition.

[0013] Another object of the present invention is to provide a zeolite suitable for obtaining a composition having a low viscosity and a low thermal expansion coefficient after curing, and a method for producing the zeolite.

[0014] In addition, if it is a zeolite with a lower thermal expansion coefficient, the thermal expansion coefficient of the resin composite material can be reduced by a smaller amount, and it can be expected that the viscosity increase can be suppressed by using zeolite. Such a low zeolite with a thermal expansion coefficient can be applied to various purposes requiring the suppression of thermal expansion of resin substrates, etc. Therefore, the present invention also aims to provide a zeolite with a lower thermal expansion coefficient.

[0015] Solutions to the problem

[0016] The gist of the present invention is as follows.

[0017] [1] A zeolite which is a spherical aluminosilicate having a particle size of 0.05 μm or more and less than 1.0 μm and having d6r as a CBU.

[0018] [2] The zeolite according to [1] above, which has a sphericity of 0.7 or more.

[0019] [3] The zeolite according to [1] or [2] above, which is a CHA-type zeolite.

[0020] [4] A composition comprising the zeolite according to any one of [1] to [3] above and a resin.

[0021] [5] The composition according to [4] above, wherein

[0022] The resin is at least one selected from epoxy resins and polyimide resins.

[0023] [6] The composition according to [4] or [5], further comprising an inorganic filler having a particle size of 1.0 μm or more and 10 μm or less.

[0024] [7] The composition according to any one of [4] to [6] above, wherein

[0025] The content of the zeolite described in any one of [1] to [3] in the entire filler is 90% by mass or more.

[0026] [8] The composition according to any one of [4] to [7] above, wherein

[0027] The content of the zeolite is 40 to 70% by mass, the resin is an epoxy resin, and the viscosity of the composition at 23° C. is 0.1 Pa·s or more and 250 Pa·s or less.

[0028] [9] A resin composite material, comprising the composition described in any one of [4] to [8], wherein:

[0029] The content of the zeolite is 40 to 70% by mass, the resin is an epoxy resin, and the average thermal expansion coefficient of the resin composite material at 25 to 100° C. is 10 to 30 ppm / K.

[0030]

[10] A liquid sealant comprising the composition according to any one of [4] to [8] above.

[0031]

[11] A sealing material formed from the resin composite material described in [9] above.

[0032]

[12] An electronic device comprising the resin composite material described in [9] above.

[0033]

[13] A method for manufacturing a sealing material, the method comprising:

[0034] A step of filling the gap with the composition according to any one of [4] to [8] above and then curing the gap.

[0035]

[14] A method for producing zeolite, the method comprising:

[0036] The process of subjecting a raw material composition including a silicon atom raw material, a water-soluble aluminum atom raw material, an organic structure directing agent, a silane coupling agent and water to hydrothermal synthesis.

[0037]

[15] The method for producing zeolite according to

[14] above, further comprising a calcining step.

[0038] Effects of the Invention

[0039] According to the present invention, a low-viscosity composition can be obtained by using zeolite having a specific particle size, and a resin composite material having a low thermal expansion coefficient can be provided by curing the composition.

[0040] In addition, it is possible to provide zeolite having a low coefficient of thermal expansion that is suitable for suppressing the thermal expansion of resin.

[0041] In addition, it is possible to provide a negative expansion filler with a small particle size that can be used for applications such as underfill materials suitable for narrow gaps. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a SEM photograph of the zeolite of Example 1.

[0043] Figure 2 This is a SEM photograph of the zeolite of Comparative Example 1. DETAILED DESCRIPTION

[0044] Hereinafter, the present invention will be described with reference to embodiments.

[0045] [First embodiment]

[0046] <Zeolite>

[0047] The zeolite of the first embodiment of the present invention is a spherical aluminosilicate having a particle size of 0.05 μm or more and less than 1.0 μm and having d6r as CBU. The zeolite of the present invention preferably has a high sphericity. The sphericity will be described in detail later.

[0048] (Zeolite particle size)

[0049] The particle size of the zeolite of the first embodiment of the present invention refers to the diameter (equivalent circle diameter) of a circle having an area equal to the projected area of ​​the particle and becoming the maximum diameter in particle observation using a scanning electron microscope (SEM). For the zeolite of the first embodiment of the present invention, a plurality of zeolite particles can be condensed to form secondary particles. In this case, the particle size of the zeolite is the particle size of the primary particles.

[0050] The zeolite of the first embodiment of the present invention preferably has a large particle size because the viscosity thereof is not easily increased when added to a resin. In addition, on the other hand, the particle size is preferably small because it is easy to mix evenly with other components such as a resin and the smoothness of the surface is easy to increase. Specifically, it is 0.05 μm or more, preferably 0.1 μm or more, more preferably 0.2 μm or more, particularly preferably 0.3 μm or more, and most preferably 0.4 μm or more. In addition, on the other hand, it is less than 1.0 μm, preferably 0.9 μm or less, and more preferably 0.8 μm or less.

[0051] When using zeolite, usually, the zeolite particles are not one, but are used in the form of a plurality of zeolite particle groups. That is, in one embodiment of the present invention, it is preferably used in the form of a zeolite group containing at least the zeolite particles of the first embodiment of the present invention. The average primary particle size of the zeolite in such a mode formed by a plurality of zeolite particles is preferably in the range of 0.2 to 0.8 μm, more preferably 0.25 to 0.75 μm, and further preferably 0.3 to 0.7 μm. For the average primary particle size of the zeolite, 50 zeolites (powders, particles in the liquid composition or resin composite material described later) are randomly selected to measure their particle sizes and take the average value.

[0052] In addition, as the particle size distribution of the zeolite on a volume basis, the median particle size (d50) is preferably in the range of 0.1 to 0.9 μm, more preferably in the range of 0.2 to 0.8 μm, and further preferably in the range of 0.3 to 0.7 μm. By making the median particle size within this range, the proportion of zeolite that exerts the effect of the present invention increases, and it is easy to obtain the effect of the present invention with a smaller amount.

[0053] (Structure of Zeolite)

[0054] Zeolite refers to a compound composed of silicon or aluminum and oxygen and having a TO4 unit (T element refers to an element other than oxygen constituting the skeleton) as a basic unit. Specifically, zeolite includes crystalline porous aluminosilicate (aluminosilicate), crystalline porous aluminophosphate (ALPO), or crystalline porous silicoaluminophosphate (SAPO), and the zeolite of the first embodiment of the present invention is aluminosilicate.

[0055] Zeolite is composed of a structural unit called a Composite Building Unit (CBU) in which a number (several to dozens) of TO4 units are linked together, and therefore has regular channels (tubular pores) and cavities (holes).

[0056] The crystal structure of the CBU and the zeolite described later can be represented by the code for defining the structure of the zeolite established by the International Zeolite Association (IZA). It should be noted that the structure of the zeolite can be determined based on an X-ray diffraction pattern obtained by an X-ray structure analyzer (e.g., a desktop X-ray diffraction device D2PHASER manufactured by BRUKER) and using the 2018 edition of the Zeolite Structure Database (http: / / www.iza-structure.org / databases / ).

[0057] (Skeleton of zeolite)

[0058] The framework of the zeolite according to the first embodiment of the present invention has d6r as CBU. By having d6r, it is easy to obtain a resin composite material having a low thermal expansion coefficient as described in detail later.

[0059] As zeolites having d6r as CBU, there can be mentioned AEI, AFT, AFV, AFX, AVL, CHA, EAB, EMT, ERI, FAU, GME, JSR, KFI, LEV, LTL, LTN, MOZ, MSO, MWW, OFF, SAS, SAT, SAV, SBS, SBT, SFW, SSF, SZR, TSC, and -WEN type structure zeolites.

[0060] Among them, from the viewpoint of easy control of particle size, zeolites with structures below 8-membered oxygen rings are particularly preferred. Zeolites with structures below 8-membered oxygen rings include AEI, AFT, AFX, CHA, ERI, KFI, SAT, SAV, SFW, and TSC type zeolites. Among them, from the aspect that the structure is stable even if shape control is performed, zeolites with AEI, AFX, CHA, and ERI type structures are particularly preferred, and zeolites with CHA type structures are most preferred. It should be noted that in this specification, a structure with 8-membered oxygen rings refers to a structure in which the number of oxygen elements in the pores composed of oxygen and T elements (elements other than oxygen that constitute the skeleton) forming the zeolite skeleton is the largest when the number of oxygen elements is 8.

[0061] (Average thermal expansion coefficient of zeolite)

[0062] From the aspect of being easy to reduce the average thermal expansion coefficient of the liquid composition and the resin composite material described later with a small amount, it is preferred that the average thermal expansion coefficient of the zeolite of the first embodiment of the present invention is low. In addition, it is also preferred to consider that the various physical properties of the resin are not easy to change due to the addition of zeolite by making the zeolite a small amount. In particular, from the aspect of being able to suppress the viscosity rise of the liquid composition described later, it is also preferred that the average thermal expansion coefficient is low. Specifically, the average thermal expansion coefficient of zeolite is usually less than 0ppm / K, preferably below -2ppm / K, more preferably below -3ppm / K, further preferably below -5ppm / K, particularly preferably below -6ppm / K, and most preferably below -8ppm / K.

[0063] On the other hand, if it is considered that the liquid composition and resin composite material containing zeolite and resin described later are used, then from the aspect that the difference with the average thermal expansion coefficient of resin is small, zeolite and resin are not easy to peel off, the average thermal expansion coefficient of preferred zeolite is high. Therefore, the average thermal expansion coefficient of zeolite is usually more than -1000ppm / K, preferably more than -900ppm / K, more preferably more than -800ppm / K, more preferably more than -700ppm / K, particularly preferably more than -500ppm / K, more preferably more than -300ppm / K. And, particularly in the case of the purposes connected with other materials such as sealing material and substrate, the average thermal expansion coefficient of preferred zeolite is high, specifically preferably more than -100ppm / K, more preferably more than -50ppm / K, more preferably more than -40ppm / K, particularly preferably more than -30ppm / K, more preferably more than -25ppm / K, most preferably more than -20ppm / K.

[0064] The average thermal expansion coefficient of zeolite can be measured by calculating the lattice constant using an X-ray diffraction apparatus "D8ADVANCE" manufactured by BRUKER and X-ray diffraction analysis software "JADE". Here, zeolite is usually measured in a dry state in order to eliminate the influence of water detachment.

[0065] The average thermal expansion coefficient of zeolite is usually measured in the range of 50 to 100°C. That is, it is a numerical value representing the displacement of the lattice constant per 1°C based on the average lattice constant at 50°C and the average lattice constant at 100°C when the temperature of zeolite is increased. Here, the average lattice constant at each temperature is the average value of the lattice constants of the a-axis, b-axis, and c-axis. It should be noted that the measurement of the average thermal expansion coefficient is performed by slowly increasing the temperature after waiting for the lattice constant to stabilize.

[0066] Generally, the thermal expansion coefficient of resin increases in high temperature regions. Therefore, the average thermal expansion coefficient of zeolite is particularly preferably low during the process of heating to the high temperature region. Specifically, the average thermal expansion coefficient in the range of 50 to 350°C (high temperature region) is preferably below -9.5ppm / K, more preferably below -10.0ppm / K, and further preferably below -12.5ppm / K. It should be noted that, here, the average thermal expansion coefficient of zeolite (high temperature region) is a numerical value representing the displacement of the lattice constant per 1°C based on the average lattice constant at 50°C and the average lattice constant at 350°C when the zeolite is heated.

[0067] (Shape of zeolite)

[0068] The zeolite of the first embodiment of the present invention is preferably spherical in shape from the viewpoint of being easy to incorporate while suppressing an increase in the viscosity of the composition containing the zeolite. Specifically, the sphericity and roundness are preferably as follows.

[0069] <<Sphericity>>

[0070] The sphericity of zeolite is preferably 0.6 or more, more preferably 0.65 or more, particularly preferably 0.7 or more, and most preferably 0.8 or more. In addition, the upper limit of sphericity is not particularly limited, and the sphericity can be 1 or less. It should be noted that the sphericity of zeolite is usually 0.58 when it is a cube. It should be noted that in the present application, "sphericity" is the average value of 10 particles obtained by scanning electron microscopy (SEM).

[0071] In this specification, “sphericity” is defined as “the ratio of the minimum diameter to the maximum diameter of a particle.” The maximum diameter and the minimum diameter can be obtained by observation using a scanning electron microscope (SEM).

[0072] <<Roundness>>

[0073] The roundness of the zeolite of the first embodiment of the present invention is preferably 0.786 or more, more preferably 0.790 or more, further preferably 0.795 or more, further preferably 0.800 or more, further preferably 0.805 or more, particularly preferably 0.810 or more, particularly preferably 0.815 or more, and most preferably 0.820 or more. In addition, the upper limit of the roundness is not particularly limited, and the roundness can be 1 or less. It should be noted that the roundness of zeolite is usually 0.785 when it is mostly cubic.

[0074] In this specification, "circularity" is defined as "4×π×area / (circumference) 2 ". The area and circumference can be obtained by observation using a scanning electron microscope (SEM). It should be noted that in the present application, "roundness" is the average value of 10 particles obtained by a scanning electron microscope (SEM).

[0075] (Skeleton density of zeolite)

[0076] The skeleton density of the zeolite of the first embodiment of the present invention is not particularly limited as long as it does not impair the effect of the present invention. From the perspective of the zeolite's structural vibration and the average thermal expansion coefficient being easily reduced, the zeolite's skeleton density is preferably low. Therefore, the zeolite's skeleton density is preferably The following, more preferably the following.

[0077] On the other hand, from the viewpoint that the structural stability of the zeolite is easily increased, it is preferred that the framework density of the zeolite is high. The framework density of the zeolite is preferably More preferably The above, more preferably When the skeleton density is within the above range, the zeolite can be used as a stable filler.

[0078] It should be noted that the framework density represents the number of T atoms present per unit volume of zeolite and is a value determined by the structure of the zeolite. In this specification, the values ​​described in the 2017 edition of the IZA Zeolite Structure Database (http: / / www.iza-structure.org / databases / ) may be used.

[0079] As the skeleton density is greater than And for Examples of the following zeolites include zeolites having ERI, LTL, LTN, MOZ, OFF, SAT, SSF, and -WEN type structures.

[0080] As the skeleton density is greater than And for Examples of the following zeolites include AEI, AFT, AFV, AFX, AVL, EAB, GME, LEV, MWW, and SFW type zeolites.

[0081] As the skeleton density is greater than And for Examples of the following zeolites include zeolites having CHA, KFI, SAS, and SAV type structures.

[0082] As the skeleton density exists in Examples of zeolites within the following range include EMT, FAU, JSR, SBS, SBT, and TSC type zeolites.

[0083] (Silica / alumina molar ratio (SAR) of zeolite)

[0084] The silica / alumina molar ratio (sometimes referred to as "SAR", "Si / Al2 molar ratio" or "Si / Al2 ratio") of the zeolite of the first embodiment of the present invention is not particularly limited as long as it is a mode that does not impair the effect of the present invention. From the perspective that the moisture resistance of the resin composite material described later is easily increased and the amount of counter cations is easily controlled, the SAR (Si / Al2 ratio) of the zeolite is preferably high. Therefore, the SAR (Si / Al2 ratio) of the zeolite is usually 2 or more, preferably 3 or more, more preferably 3.5 or more, further preferably 4 or more, particularly preferably 4.5 or more, and most preferably 5 or more.

[0085] On the other hand, from the perspective of easy and inexpensive production, the SAR (Si / Al2 ratio) of the zeolite is preferably low. Therefore, the SAR (Si / Al2 ratio) of the zeolite is usually 2000 or less, preferably 1000 or less, more preferably 500 or less, and further preferably 100 or less. When the Si / Al2 ratio is within the above range, it is easy to control the amount of counter cations, and the production cost of the zeolite is also low.

[0086] (Counter cation of zeolite)

[0087] The counter cation of the zeolite of the first embodiment of the present invention is not particularly limited as long as it is a mode that does not damage the effect of the present invention. The counter cation of the zeolite is generally a proton, an alkali metal ion, and an alkaline earth metal ion. Preferably, it is a proton, an alkali metal ion, and more preferably a proton, a Li ion, a Na ion, and a K ion. In the case of an alkali metal ion and an alkaline earth metal ion, the smaller its size, the easier it is for the zeolite to show an average thermal expansion coefficient less than 0ppm / K, and thus it is preferred. Among them, in the case where the counter cation of the zeolite is a proton, it is easy to reduce the average thermal expansion coefficient of the resin composite material, and thus it is preferred. That is, as a zeolite, it is preferably a proton type, an alkali metal type, and more preferably a proton type, a Li type, a Na type, and a K type.

[0088] (Crystallinity of zeolite)

[0089] The crystallinity of the zeolite of the first embodiment of the present invention is not particularly limited as long as it is a mode that does not damage the effect of the present invention. As the reason, it can be inferred that the Composite Building Unit (CBU) is a factor that has a greater impact on the average thermal expansion coefficient of epoxy resin composite materials compared to the structure determined by IZA through coding. It should be noted that the crystallinity of the zeolite can be obtained by an X-ray diffraction device (for example, a desktop X-ray diffraction device D2PHASER manufactured by BRUKER), or can be obtained by comparing the X-ray diffraction peak of the zeolite with the X-ray diffraction peak as a benchmark. As a specific calculation example, the crystallinity of the LTA type zeolite of Scientific Reports 2016, 6, Article number: 29210 can be cited.

[0090] (Surface treatment of zeolite)

[0091] Zeolite may be subjected to surface treatment such as silylation treatment and fluorination treatment within a range not impairing the effects of the present invention. The surface treatment may be a physical treatment or a chemical treatment.

[0092] <Method for producing zeolite>

[0093] A known method can be applied to the production method of zeolite. For example, when producing CHA type zeolite, it can be produced by referring to the method described in Japanese Patent Application Laid-Open No. 2009-097856.

[0094] On the other hand, when producing the zeolite of the first embodiment of the present invention (spherical zeolite having a small particle size), a preferred method is to use a silane coupling agent during hydrothermal synthesis. The silane coupling agent will be described in detail later.

[0095] The above particularly preferred zeolite can be produced by the following method (hereinafter sometimes referred to as "the method for producing the zeolite of the present invention").

[0096] The method for producing zeolite of the present invention comprises a step of hydrothermally synthesizing a raw material composition comprising a silicon atom raw material, a water-soluble aluminum atom raw material, an organic structure directing agent, a silane coupling agent and water. In addition, the method for producing zeolite of the present invention preferably further comprises a calcining step.

[0097] In addition, a desired zeolite (hereinafter sometimes referred to as "seed zeolite") may be used as necessary.

[0098] <<Silicon Atom Raw Materials>>

[0099] The silicon atom raw material used in the present invention is not particularly limited, and various known substances can be used. For example, colloidal silica, amorphous silica, sodium silicate, trimethylethoxysilane, tetraethyl orthosilicate, aluminosilicate gel, and zeolite can be used. These can be used alone or in any combination and ratio.

[0100] <<Aluminum Atom Raw Materials>>

[0101] As the aluminum atom raw material, a water-soluble raw material is preferably used. In addition, aluminum hydroxide is preferred from the viewpoint of low alkali metal content.

[0102] <<Organic structure directing agent>>

[0103] As the organic structure directing agent, various known substances such as tetraethylammonium hydroxide (TEAOH) and tetrapropylammonium hydroxide (TPAOH) can be used. Among them, N,N,N-trimethyl-1-adamantanammonium hydroxide (TMAdaOH) is preferred.

[0104] The amount of the organic structure directing agent used is usually 0.01 or more, preferably 0.02 or more, more preferably 0.03 or more, particularly preferably 0.04 or more, and most preferably 0.05 or more, in terms of molar ratio relative to silicon (Si) contained in the raw material composition. On the other hand, it is usually 1 or less, preferably 0.6 or less, more preferably 0.55 or less, and further preferably 0.5 or less. It is believed that by using within this range, high-purity spherical zeolite with less by-products is easily grown.

[0105] <<Water>>

[0106] From the viewpoint of easily generating crystals, when using the seed zeolite described later, the amount of water used can be generally more than 5, preferably more than 7, more preferably more than 9, and more preferably more than 10 relative to the molar ratio of silicon (Si) contained in the raw material composition other than the seed zeolite. By setting it within this range, it is preferred to easily generate crystals. In addition, it can be considered that by increasing the amount of water and diluting the raw material concentration, zeolite is easily manufactured with a large particle size. From the aspect of the effect of the cost reduction consumed by the waste liquid treatment being easy to obtain, it can be generally less than 50, preferably less than 40, more preferably less than 30, and more preferably less than 25 relative to the molar ratio of silicon (Si).

[0107] <<Silane coupling agent>>

[0108] For the manufacturing method of the zeolite of the present invention, by using a silane coupling agent during hydrothermal synthesis, it is easy to obtain a zeolite with high sphericity and small particle size. As the silane coupling agent, various known silane coupling agents having an acryl group, an amine structure, etc. can be used. Among them, a silane coupling agent having an epoxy group is preferred. As a silane coupling agent having an epoxy group, there is 3-glycidoxypropyltrimethoxysilane, etc.

[0109] From the perspective of easily obtaining a shape control effect, the amount of a silane coupling agent used may be generally 0.01 or more, preferably 0.015 or more, and more preferably 0.02 or more in terms of a molar ratio relative to silicon (Si). On the other hand, from the perspective of not being prone to hindering crystal growth due to excessive addition, it is generally 1 or less, preferably 0.5 or less, and more preferably 0.1 or less.

[0110] <<Alkali Metal Atom Raw Materials>>

[0111] The manufacture of zeolite can use alkali metal atom raw materials. The alkali metal atom in the case of using alkali metal atom raw materials is not particularly limited, and the known alkali metal atoms used in the synthesis of zeolite can be used, preferably at least one alkali metal selected from lithium, sodium, potassium, rubidium and cesium. It should be noted that a variety of alkali metal atoms can be used.

[0112] <<Seed Zeolite>>

[0113] In the method for producing zeolite, a zeolite serving as a seed crystal may be used. When a seed crystal zeolite is used, one type may be used alone, or two or more types may be used in any combination and ratio.

[0114] <<Mixing of raw materials (preparation of raw material composition before reaction)>>

[0115] The raw material composition can be generally obtained by mixing a silicon atom raw material, an aluminum atom raw material, an organic structure directing agent and water and then adding the seed zeolite when used. In the method for producing zeolite of the present invention, a silane coupling agent is preferably mixed with these raw materials.

[0116] In the production of zeolite, in addition to the above-mentioned components, components such as an acid component that accelerates the reaction and a metal stabilizer such as polyamine may be added in an arbitrary step as necessary.

[0117] <<Maturation>>

[0118] The raw material composition prepared as described above can be hydrothermally synthesized immediately after preparation, but in order to obtain a zeolite with higher crystallinity, it is preferably matured for a certain period of time under given temperature conditions. In particular, when the reaction scale is expanded, it is preferred to mature the raw material while stirring it for a certain period of time in order to improve the stirring property and make the raw material more uniform. The temperature in the case of ripening is usually below 100°C, preferably below 95°C, and more preferably below 90°C. The lower limit is not particularly set, and the temperature in the case of ripening is usually above 0°C, preferably above 10°C. The ripening temperature can be constant during ripening, or it can be changed in stages or continuously. The ripening time is not particularly limited, and is usually more than 2 hours, preferably more than 3 hours, and more preferably more than 5 hours. In addition, on the other hand, it is usually less than 30 days, preferably less than 10 days, and more preferably less than 4 days.

[0119] <<Hydrothermal Synthesis>>

[0120] Next, the obtained raw material composition is subjected to hydrothermal synthesis.

[0121] The hydrothermal synthesis is usually carried out as follows: the raw material composition prepared as described above or the aqueous gel obtained by aging the raw material composition is placed in a pressure-resistant container, and a given temperature is maintained under spontaneous pressure or gas pressure to a degree that does not hinder crystallization, while stirring, or by rotating or shaking the container, or in a static state.

[0122] In order to speed up the reaction rate, the reaction temperature during hydrothermal synthesis is usually 120°C or more, preferably 130°C or more, more preferably 140°C or more, and particularly preferably 150°C or more. In addition, on the other hand, it is usually 230°C or less, preferably 220°C or less, more preferably 200°C or less, and further preferably 190°C or less. The reaction time is not particularly limited, but is usually 2 hours or more, preferably 3 hours or more, and more preferably 5 hours or more. In addition, on the other hand, it is usually 30 days or less, preferably 10 days or less, more preferably 7 days or less, and further preferably 5 days or less. The reaction temperature may be constant during the reaction, or may be changed in stages or continuously.

[0123] It is considered that the reason why particularly preferred zeolite can be produced by the method for producing zeolite of the present invention is that the silane coupling agent is adsorbed on the surface of the growing zeolite crystal, thereby forming a state of a micelle structure close to a sphere and growing.

[0124] [Second embodiment]

[0125] <Composition>

[0126] The composition of the second embodiment of the present invention is a composition containing the zeolite of the above-mentioned first embodiment and a resin. As described later, the average thermal expansion coefficient of the zeolite of the first embodiment is easy to become very low. Therefore, by containing this zeolite, the thermal expansion of the composite material formed by the composition of the second embodiment can be suppressed.

[0127] From the viewpoint of reducing the thermal expansion coefficient while suppressing the viscosity increase, the content of the zeolite of the first embodiment contained in the resin composition is preferably 25% by mass or more, more preferably 30% by mass or more, further preferably 35% by mass or more, further preferably 40% by mass or more, particularly preferably 45% by mass or more, and particularly preferably 50% by mass or more, relative to the total amount of the composition. On the other hand, it is preferably 90% by mass or less, more preferably 80% by mass or less, further preferably 75% by mass or less, and particularly preferably 70% by mass or less.

[0128] In addition, from the perspective of reducing the viscosity increase during resin kneading and easily reducing the thermal expansion coefficient of the cured product, the content of the zeolite of the present invention in all fillers when the resin composition contains fillers other than zeolite of the first embodiment is preferably 10% by mass or more, more preferably 30% by mass or more, further preferably 50% by mass or more, particularly preferably 70% by mass or more, and most preferably 90% by mass or more.

[0129] (resin)

[0130] The resin used in the composition of the second embodiment of the present invention is not particularly limited as long as it can exert the effect of the present invention. From the viewpoint of more easily showing the effect as a composite material, it is preferably at least one selected from epoxy resins and polyimide resins. In particular, when the composition of the second embodiment of the present invention is used as a useful liquid composition such as a sealant, epoxy resin is preferably used. In addition, when used as a useful composition such as a substrate, polyimide resin is preferably used.

[0131] From the viewpoint of maintaining the excellent physical properties of the resin and the heat resistance (hardness of thermal expansion) of the cured resin composition, the amount of the resin contained in the composition of the present invention is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the composition. On the other hand, it is preferably 50% by mass or less, more preferably 25% by mass or less, and particularly preferably 15% by mass or less.

[0132] <<Epoxy Resin>>

[0133] The epoxy resin used in the present invention will be described in detail in the fourth embodiment of the present invention described later.

[0134] <<Polyimide resin>>

[0135] The polyimide resin used in the present invention is preferably a polyimide obtained from tetracarboxylic dianhydride and diamine, and particularly preferably an aromatic polyimide obtained from aromatic tetracarboxylic dianhydride and aromatic diamine, since the thermal expansion coefficient of the resin composite material can be easily reduced and the heat resistance, mechanical strength, electrical properties, solvent resistance and other properties are excellent.

[0136] More specifically, an aromatic tetracarboxylic acid component and p-phenylenediamine are polymerized and imidized, a polyimide precursor solution is dispersed in the obtained polyimide resin powder, and granulated, and the obtained polyimide powder is composited with a filler to prepare a resin composite material.

[0137] It should be noted that the polyimide powder is formed by combining the particles of the polyimide powder with each other by a polyimide precursor and granulating them, and in the aggregate, the polyimide precursor acts as a binder. As the polyimide precursor, for example, polyamic acid is used, and the polyimide precursor solution used as a raw material can use water and / or an alcohol solvent as a reaction solvent, and a polyamic acid produced by reacting tetracarboxylic dianhydride with diamine in the presence of a basic compound having a pKa of 7.5 or more.

[0138] As a preferred embodiment of the second embodiment, there is a composition using epoxy resin as the resin and containing the zeolite of the first embodiment, wherein the viscosity of the composition at 23° C. is 0.1 Pa·s or more and 250 Pa·s or less, and the content of the zeolite is 40 to 70% by mass. Here, the viscosity at 23° C. is preferably 1 Pa·s or more and 30 Pa·s or less.

[0139] This liquid resin composition is useful as an underfill material (hereinafter, sometimes referred to as a "liquid sealant"), and can reduce the average thermal expansion coefficient after curing, and is suitable as a sealant.

[0140] In addition, as another preferred embodiment of the second embodiment, there can be cited a resin composite material using epoxy resin as the resin and containing the zeolite of the first embodiment, wherein the zeolite content of the resin composite material is 40 to 70% by mass and the average thermal expansion coefficient at 25 to 100°C is 10 to 30 ppm / K.

[0141] This composite material has a low average thermal expansion coefficient at a temperature not higher than the glass transition temperature and is therefore useful as various materials, and is particularly effective for electronic devices.

[0142] [Third embodiment]

[0143] <Composition>

[0144] The composition of the third embodiment of the present invention contains the zeolite (small particle size zeolite) of the first embodiment described above, a resin, and an inorganic filler having a particle size of 1.0 μm to 50 μm (hereinafter also referred to as a large particle size inorganic filler).

[0145] (Inorganic filler)

[0146] In the case of a liquid composition, from the perspective of being easy to fill the liquid composition even in a narrow space, it is preferred that the particle size of the inorganic filler is small. In addition, on the other hand, from the perspective of the viscosity of the liquid composition being difficult to increase, it is preferred that the particle size of the inorganic filler is large. When a filler having a small specific surface area of ​​the filler is used in combination with a filler having a large specific surface area, when the specific surface area is large, the interaction between the filler and the resin increases, and the viscosity of the liquid composition tends to increase. Therefore, in order to reduce the viscosity of the liquid composition, it is preferred that the specific surface area of ​​the filler is small. The smaller the particle size, the easier it is for the specific surface area to become larger. In addition, the specific surface area is also different because of the shape of the filler, and the spherical specific surface area is the smallest. Therefore, if considered from the viewpoint of reducing the viscosity, it is preferred that the inorganic filler is close to a spherical shape and has a large particle size.

[0147] The composition of the third embodiment of the present invention uses a small-diameter zeolite, and from the viewpoint of reducing the viscosity, the surface area per unit volume is preferably 120×10 -6 ( / m) or less, more preferably 80×10 -6 ( / m) or less.

[0148] In the composition of the third embodiment of the present invention, by using a combination of a small-particle-size and a large-particle-size filler, the small particles enter the gaps between the large particles, the filling amount can be increased, the thermal expansion coefficient can be reduced, and the viscosity increase can also be reduced. Therefore, from the aspect that the thermal expansion coefficient is easily reduced, the composition of the present invention preferably contains a small-particle-size zeolite and a large-particle-size inorganic filler.

[0149] The particle size of the inorganic filler is measured in the same manner as the zeolite of the first embodiment described above. That is, the particle size of the inorganic filler refers to the diameter (equivalent circle diameter) of a circle having an area equal to the projected area of ​​the particle and becoming the maximum diameter in the observation of the particle using a scanning electron microscope (SEM). In addition, the particle size is the particle size of the primary particle.

[0150] Examples of the inorganic filler used in the composition of the present invention include zeolite and inorganic fillers other than zeolite.

[0151] Zeolite is an inorganic filler with a low thermal expansion coefficient, and can reduce the thermal expansion coefficient of the cured product of the liquid composition, i.e., the epoxy resin composite material, which is one of the preferred embodiments of the present invention. However, since it has a porous structure, the specific surface area is large, and if it is mixed in large quantities, the viscosity of the liquid composition tends to increase. Various studies have been conducted in the present invention, and it has been found that by including a large-particle-size inorganic filler in the liquid composition in addition to the small-particle-size zeolite such as the zeolite of the first embodiment described above, for example, it is possible to reduce the thermal expansion coefficient of the liquid epoxy resin composite material while preventing the viscosity from increasing, thereby achieving a low viscosity of the liquid composition.

[0152] As inorganic fillers other than zeolite, at least one selected from metals, carbon, metal carbides, metal oxides and metal nitrides can be cited. Examples of metals include silver, copper, aluminum, gold, nickel, iron and titanium. Examples of carbon include carbon black, carbon fiber, graphite, fullerene, diamond and the like. Examples of metal carbides include silicon carbide, titanium carbide, tungsten carbide and the like. Examples of metal oxides include magnesium oxide, aluminum oxide (alumina), silicon dioxide and other silicon oxides, calcium oxide, zinc oxide, yttrium oxide, zirconium oxide, cerium oxide, ytterbium oxide, sialon (ceramic formed by silicon, aluminum, oxygen and nitrogen) and the like. Examples of metal nitrides include boron nitride, aluminum nitride, silicon nitride and the like.

[0153] (Large particle size inorganic filler)

[0154] The large-particle inorganic filler may be zeolite or an inorganic filler other than zeolite. Specific examples of the inorganic filler other than zeolite are as described above.

[0155] From the viewpoint of reducing the thermal expansion coefficient, the large-particle-size inorganic filler is preferably zeolite, metal nitride, metal oxide, or the like.

[0156] (Content of large particle size inorganic filler)

[0157] In the composition of the 3rd embodiment of the present invention, from the aspect of easily fully showing the effect of use of filler, the content of the large-particle diameter inorganic filler in the preferred composition is many. On the other hand, when the resin combination is a liquid composition, from the aspect of improving the fluidity of the liquid composition, being easily filled in a narrow space, the content of the large-particle diameter inorganic filler in the preferred composition is few. Particularly because the specific surface area of ​​the large-particle diameter inorganic filler is small, viscosity is difficult to rise, therefore, by increasing the dosage, fluidity is easily improved.

[0158] Specifically, from the viewpoint of suppressing the viscosity increase and reducing the thermal expansion coefficient, the content of the large-particle inorganic filler is preferably 20% by mass or more, more preferably 25% by mass or more, further preferably 30% by mass or more, particularly preferably 40% by mass or more, and most preferably 45% by mass or more, relative to the total amount of the liquid composition. In addition, on the other hand, it is preferably 90% by mass or less, more preferably 80% by mass or less, further preferably 75% by mass or less, and particularly preferably 70% by mass or less.

[0159] (Shape of large particle size inorganic filler)

[0160] As long as the composition and the resin composite material can show preferred properties, the shape of the large-particle inorganic filler is not particularly limited and can be spherical, whisker-like, fibrous, plate-like, or aggregates thereof. From the perspective of containing it while suppressing the increase in viscosity, spherical is preferred.

[0161] The sphericity of the large-diameter inorganic filler is preferably 0.6 or more, more preferably 0.65 or more, and particularly preferably 0.70 or more. The upper limit of the sphericity is not particularly limited, and the sphericity may be 1 or less.

[0162] Therefore, in the third embodiment of the present invention, the sphericity of the small-diameter zeolite and the large-diameter inorganic filler in the first embodiment of the present invention is preferably 0.6 or more, more preferably 0.65 or more, and particularly preferably 0.70 or more. In addition, the sphericity of the large-diameter inorganic filler is preferably higher than that of the small-diameter zeolite.

[0163] In addition, the roundness of the large-particle inorganic filler is preferably 0.786 or more, more preferably 0.790 or more, further preferably 0.795 or more, further preferably 0.800 or more, further preferably 0.805 or more, particularly preferably 0.810 or more, particularly preferably 0.815 or more, and most preferably 0.820 or more. In addition, the upper limit of the roundness is not particularly limited, and the roundness can be less than 1. It should be noted that the determination method of sphericity and roundness is as described above.

[0164] (Small particle size zeolite)

[0165] In the composition of the third embodiment of the present invention, when the resin composition is a liquid composition, specifically, the content of the zeolite (small particle size zeolite) of the first embodiment in the composition is preferably 1% by mass or more, more preferably 5% by mass or more, and particularly preferably 10% by mass or more relative to the total amount of the composition. On the other hand, it is preferably 50% by mass or less, more preferably 45% by mass or less, and further preferably 40% by mass or less.

[0166] In addition, from the perspective of easily reducing the thermal expansion coefficient of the cured product, the content of zeolite (small particle size zeolite) in the entire filler is preferably 10 mass % or more, more preferably 30 mass % or more, further preferably 50 mass % or more, more particularly preferably 70 mass % or more, and most preferably 90 mass % or more.

[0167] When the large-particle inorganic filler is zeolite, from the perspective of easy filling in a narrow space, the content of small-particle zeolite in the entire filler is preferably high, more preferably 30 mass % or more, further preferably 50 mass % or more, more particularly preferably 70 mass % or more, and most preferably 90 mass % or more.

[0168] (Total inorganic filler content)

[0169] From the aspect of being easy to show the effect as a filling material, the total content of all inorganic fillers (total inorganic fillers) contained in the preferred composition is more. On the other hand, from the aspect of high fluidity in the case of a liquid composition and easy filling in a narrow space, the total content of all inorganic fillers (total inorganic fillers) contained in the preferred composition is less. Specifically, in the composition of the third embodiment of the present invention, relative to the total amount of the composition, the total content of all inorganic fillers is preferably 30% by mass or more, more preferably 35% by mass or more, and particularly preferably 40% by mass or more. On the other hand, preferably 95% by mass or less, more preferably 90% by mass or less, and particularly preferably 85% by mass or less.

[0170] In order to improve the dispersibility of the inorganic filler, the liquid composition of the second and third embodiments of the present invention may contain a dispersant. The dispersant contained in the liquid composition containing the resin and the filler is mainly added to the liquid composition containing the resin and the filler with a large difference in polarity, thereby improving the interface state of the two and improving the compatibility. As a result, it is possible to show effects in terms of reducing viscosity, improving the dispersibility of the filler, and preventing the aggregation and sedimentation of the filler.

[0171] For example, from the perspective of easily dispersing the inorganic filler in the case of the composition being in a liquid state, it is preferred that the content of the dispersant is high. On the other hand, from the perspective of not being prone to the increase in the thermal expansion coefficient caused by the phase separation of the inorganic filler and the resin such as the epoxy resin, it is preferred that the content of the dispersant is low. Therefore, from the perspective of easily filling the liquid composition in a narrow space and easily achieving a low thermal expansion coefficient after curing, the content of the dispersant is preferably 0.1% by mass or more and 30% by mass or less, more preferably 0.1% by mass or more and 25% by mass or less, relative to the total amount of the composition.

[0172] In each of the above embodiments, when the composition is a liquid composition, the viscosity of the liquid composition is preferably low from the perspective of being easy to fill the composition in a narrow space. On the other hand, from the perspective of preventing the liquid from dripping when the composition is filled, the viscosity of the liquid composition is preferably high. The viscosity of the liquid composition at 23°C is preferably 0.1 Pa·s or more, more preferably 1 Pa·s or more, further preferably 5 Pa·s or more, and particularly preferably 10 Pa·s or more. On the other hand, it is preferably 250 Pa·s or less, more preferably 200 Pa·s or less, further preferably 150 Pa·s or less, particularly preferably 60 Pa·s or less, and particularly preferably 30 Pa·s or less. In addition, the viscosity at 23°C is most preferably 1 Pa·s or more and 30 Pa·s or less.

[0173] As a preferred embodiment of the above-mentioned composition, it is preferred to use an epoxy resin as the resin and a liquid composition using the zeolite of the first embodiment as the zeolite. Here, the viscosity at 23° C. is preferably 0.1 Pa·s or more and 250 Pa·s or less, more preferably 1 Pa·s or more and 30 Pa·s or less. In addition, the content of zeolite is preferably 40 to 70% by mass.

[0174] The liquid composition is useful as an underfill material and can reduce the average thermal expansion coefficient after curing, and is therefore suitable as a sealant.

[0175] In the case where the composition in each of the above-mentioned 2nd or 3rd embodiments is liquid, it can be made into a resin composite material by being solidified. For example, when the resin is an epoxy resin, the resin composite material becomes an epoxy resin composite material. The details of the epoxy resin composite material are described later. In addition, when the resin is a polyimide resin, the resin composite material becomes a polyimide resin composite material.

[0176] The average thermal expansion coefficient of the resin composite material at 25 to 100° C. is preferably 0 ppm / K or more, more preferably 2 ppm / K or more, further preferably 4 ppm / K or more, and particularly preferably 10 ppm / K or more. On the other hand, it is preferably 200 ppm / K or less, further preferably 100 ppm / K or less, and particularly preferably 30 ppm / K or less.

[0177] In particular, in the composition of the second or third embodiment, when an epoxy resin is used as the resin and the zeolite of the first embodiment is used as the zeolite, the content of the zeolite is preferably 40 to 70% by mass, and the average thermal expansion coefficient at 25 to 100° C. is preferably 10 to 30 ppm / K.

[0178] Such a resin composite material has a low average thermal expansion coefficient at a temperature below the glass transition temperature and is therefore useful as a material requiring various heat resistances, and is particularly effective for application in electronic devices.

[0179] <Resin composite materials>

[0180] In one embodiment of the present invention, the resin composite material can be obtained by curing the above-mentioned composition (composition of the second or third embodiment). For example, when the resin is an epoxy resin, an epoxy resin composite material can be obtained. When the resin is an epoxy resin, the composition is preferably a liquid composition. About the manufacture method of epoxy resin composition and epoxy resin composite material, it is described in detail in the fourth embodiment of the invention described later.

[0181] When the resin is a polyimide resin, a polyimide resin composite material can be obtained. The polyimide resin composite material can be produced by, for example, the method described below.

[0182] (Method for producing polyimide resin composite material)

[0183] The molding of the polyimide resin composite material can use various known pressurizing devices for thermoplastic resin molding. The heating temperature during molding is also affected by the properties of the resin used, and is not particularly limited, but is usually 250°C or more, preferably 300°C or more, more preferably 350°C or more, and further preferably 390°C or more. In addition, from the viewpoint that resin degradation during heating and pressing is not likely to occur, it is preferred to use a vacuum pressurizing device that can reduce the amount of oxygen in the pressurizing machine during heating, or a pressurizing device equipped with a nitrogen replacement device.

[0184] [Fourth embodiment]

[0185] <Liquid composition>

[0186] The liquid composition according to the fourth embodiment of the present invention contains an epoxy resin and an inorganic filler.

[0187] (Inorganic filler)

[0188] In the liquid composition of the 4th embodiment, zeolite and inorganic fillers other than zeolite are used as inorganic fillers. As inorganic fillers other than zeolite, the same fillers as the inorganic fillers used in the 3rd embodiment are preferred, and the above-mentioned ranges are also preferred with respect to the preferred ranges, etc.

[0189] The inorganic filler contained in the liquid composition of the fourth embodiment of the present invention includes zeolite having a particle size of 0.05 μm or more and less than 1 μm (small particle size zeolite) and an inorganic filler having a particle size of 1 μm or more and less than 50 μm (large particle size inorganic filler).

[0190] Zeolite is an inorganic filler with a low thermal expansion coefficient, and can reduce the thermal expansion coefficient of the cured product of the liquid composition, that is, the epoxy resin composite material. It has a large specific surface area, and if it is mixed in large quantities, the viscosity of the liquid composition tends to increase. In the present invention, various studies have been conducted, and it has been found that even if a small-diameter zeolite is added to the liquid composition, by containing a large-diameter inorganic filler, it is possible to reduce the thermal expansion coefficient of the epoxy resin composite material while preventing the viscosity from increasing, thereby achieving low viscosity of the liquid composition.

[0191] From the perspective of being able to easily fill the liquid composition even in a narrow space, it is preferred that the particle size of the inorganic filler is small. On the other hand, from the perspective of preventing the viscosity of the liquid composition from increasing, it is preferred that the particle size of the inorganic filler is large. When a filler with a small specific surface area and a filler with a large specific surface area are used in combination, when the specific surface area is large, the interaction between the filler and the resin increases, and the viscosity of the liquid composition tends to increase. Therefore, in order to reduce the viscosity of the liquid composition, it is preferred that the filler have a small specific surface area. The smaller the particle size, the easier it is to increase the specific surface area. In addition, the specific surface area also varies depending on the shape of the filler, and the spherical specific surface area is the smallest. Therefore, from the perspective of reducing viscosity, it is preferred that the inorganic filler be close to spherical and have a large particle size. Therefore, in particular, with regard to small-particle zeolite, its specific surface area is preferably 120×10 -6 ( / m) or less, more preferably 80×10 -6 ( / m) or less.

[0192] In the present invention, by using a combination of fillers with small and large particle sizes, small particles enter the gaps between large particles, which can increase the filling amount, reduce the thermal expansion coefficient, and reduce the viscosity increase.

[0193] The particle size of an inorganic filler such as zeolite is the particle size of each particle, which refers to the diameter (equivalent circle diameter) of a circle having an area equal to the projected area of ​​the particle and having the maximum diameter when observing the particle using a scanning electron microscope (SEM). In addition, the particle size is the particle size of the primary particle.

[0194] (Content of small-size zeolite)

[0195] In the liquid composition of the fourth embodiment of the present invention, from the perspective of being easy to fully demonstrate the use effect of the filler, it is preferred that the content of the small-diameter zeolite is large. On the other hand, from the perspective of improving the fluidity of the liquid composition and being easy to fill in a narrow space, it is preferred that the content of the small-diameter zeolite is small. In particular, the specific surface area of ​​the small-diameter zeolite is large, and the viscosity is easy to increase. Therefore, by reducing the amount used, the fluidity is easily improved.

[0196] In the liquid composition of the fourth embodiment of the present invention, specifically, the content of the small-diameter zeolite is preferably 1% by mass or more, more preferably 5% by mass or more, and particularly preferably 10% by mass or more, relative to the total amount of the liquid composition. On the other hand, it is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less.

[0197] (Large particle size inorganic filler)

[0198] The large-particle inorganic filler may be zeolite or an inorganic filler other than zeolite. Specific examples of the inorganic filler other than zeolite are as described above.

[0199] From the viewpoint of reducing the thermal expansion coefficient, the large-particle-size inorganic filler is preferably zeolite, metal nitride, metal oxide, or the like.

[0200] From the aspect of easily showing the effect of reducing the average thermal expansion coefficient, it is preferred that the content of the large-particle-diameter inorganic filler is high. On the other hand, from the aspect of improving the fluidity of the liquid composition and being easy to fill in a narrow space, it is preferred that the content of the large-particle-diameter inorganic filler is small. Specifically, relative to the total amount of the liquid composition, the content of the large-particle-diameter inorganic filler is preferably more than 20% by mass, more preferably more than 25% by mass, and particularly preferably more than 30% by mass. In addition, the content of the large-particle-diameter inorganic filler is preferably less than 80% by mass, more preferably less than 75% by mass, and particularly preferably less than 70% by mass.

[0201] In particular, since inorganic fillers with large particle sizes have a small specific surface area and are less likely to increase viscosity, the fluidity can be easily improved by increasing the amount used.

[0202] (Zeolite)

[0203] Below, the zeolite used in the present invention is described in more detail.It should be noted that, in the following description, when not particularly specified, it is a description for small-particle zeolite, but when used as a zeolite of an inorganic filler other than the small-particle zeolite, except for the particle diameter, it is also preferably characterized by the following description.For example, when using zeolite as a large-particle inorganic filler, it is preferred that the zeolite used as a large-particle inorganic filler also has the following description.In addition, it is also the same about the zeolite in the 5th and 6th embodiments described later.

[0204] In addition, as a small particle diameter zeolite, the zeolite of the above-mentioned 1st embodiment is preferable.

[0205] (Structure of Zeolite)

[0206] Zeolite refers to a compound composed of silicon or aluminum and oxygen and having a TO4 unit (T element refers to an element other than oxygen constituting the skeleton) as a basic unit. Zeolite specifically includes crystalline porous aluminosilicates, crystalline porous aluminophosphates (ALPO), or crystalline porous silicoaluminophosphates (SAPO). Among them, the zeolite of the fourth embodiment is preferably aluminosilicates.

[0207] Zeolite is composed of a structural unit called a Composite Building Unit (hereinafter sometimes referred to as "CBU") formed by linking a number (several to dozens) of TO4 units, and therefore has regular channels (tubular pores) and cavities (holes).

[0208] The crystal structure of the CBU and the zeolite described later can be represented by the code for defining the structure of the zeolite established by the International Zeolite Association (IZA). It should be noted that the structure of the zeolite can be determined based on an X-ray diffraction pattern obtained by an X-ray structure analyzer (e.g., a desktop X-ray diffraction device "D2PHASER" manufactured by BRUKER) and using the Zeolite Structure Database 2018 Edition (http: / / www.iza-structure.org / databases / ).

[0209] (Composition of Zeolite)

[0210] The zeolite of the present invention is not particularly limited as long as it is in a form that does not impair the effects of the present invention, and is preferably an aluminosilicate containing at least aluminum atoms and silicon atoms in the framework structure from the perspective of being advantageous for the application of filler purposes. Zeolites may be used alone or in any combination and ratio.

[0211] (Skeleton of zeolite)

[0212] As long as the liquid composition and the epoxy resin composite material obtained by curing the liquid composition described later show preferred performance, the skeleton of the zeolite is not particularly limited. From the perspective of easily obtaining an epoxy resin composite material with a low thermal expansion coefficient by curing the liquid composition, the skeleton of the zeolite preferably contains at least any structure of D6R and MTW as CBU, and more preferably has D6R. Specifically, the liquid composition and the epoxy resin composite material preferably contain more than 1% by mass of the zeolite of the above-mentioned preferred structure as (CBU) and an epoxy resin.

[0213] As zeolites having d6r as CBU, there can be mentioned AEI, AFT, AFV, AFX, AVL, CHA, EAB, EMT, ERI, FAU, GME, JSR, KFI, LEV, LTL, LTN, MOZ, MSO, MWW, OFF, SAS, SAT, SAV, SBS, SBT, SFW, SSF, SZR, TSC, and -WEN type structure zeolites.

[0214] Examples of zeolites having mtw as CBU include *BEA, BEC, CSV, GON, ISV, ITG, *-ITN, IWS, MSE, MTW, SFH, SFN, SSF, *-SSO, UOS, and UOV type structure zeolites.

[0215] In order to have a three-dimensional interaction with a part of the epoxy groups contained in the epoxy resin, a zeolite having a further three-dimensional channel is more preferred. Examples thereof include AEI, AFT, AFX, *BEA, BEC, CHA, EMT, ERI, FAU, GME, ISV, ITG, *-ITN, IWS, JSR, KFI, MOZ, MSE, OFF, SAT, SAV, SBS, SBT, SFW, SZR, TSC, UOS, UOV, and -WEN type zeolites.

[0216] Among them, from the viewpoint of easy control of particle size, zeolite with a structure below 8-membered oxygen ring is particularly preferred. Zeolites with a structure below 8-membered oxygen ring include AEI, AFT, AFX, CHA, ERI, KFI, SAT, SAV, SFW, and TSC type zeolites. Among them, from the aspect that the structure is stable even if shape control is performed, zeolites with AEI, AFX, CHA, and ERI type structures can be further preferred, and CHA type structures are most preferably used. It should be noted that in this specification, a structure with an 8-membered oxygen ring refers to a structure in which the number of oxygen elements in the pores formed by oxygen and T elements (elements other than oxygen that constitute the skeleton) forming the zeolite skeleton is the largest when the number of oxygen elements is 8.

[0217] (Average thermal expansion coefficient of zeolite)

[0218] As long as the liquid composition and the epoxy resin composite material obtained by curing the liquid composition show preferred performance, the average thermal expansion coefficient of zeolite is not particularly limited. From the aspect of being easy to reduce the average thermal expansion coefficient of the liquid composition and the epoxy resin composite material with a small amount, it is preferred that the average thermal expansion coefficient of zeolite is low. In addition, from the aspect of being able to suppress the viscosity rise of the liquid composition caused by adding fillers in a small amount, it is also preferred that the average thermal expansion coefficient of zeolite is low. Therefore, the average thermal expansion coefficient of zeolite is usually less than 0ppm / K, preferably below-2ppm / K, more preferably below-3ppm / K, further preferably below-5ppm / K, particularly preferably below-6ppm / K, most preferably below-8ppm / K.

[0219] On the other hand, from the perspective of the small difference in average thermal expansion coefficient from the resin and the difficulty in peeling off the zeolite and the resin, the average thermal expansion coefficient of the zeolite is preferably high. Therefore, the average thermal expansion coefficient of the zeolite is usually above -1000ppm / K, preferably above -900ppm / K, more preferably above -800ppm / K, further preferably above -700ppm / K, particularly preferably above -500ppm / K, and most preferably above -300ppm / K.

[0220] That is, if the average thermal expansion coefficient of zeolite is within the above range, the viscosity of the liquid composition can be suppressed from rising, the gaps between various components can be easily filled, and the average thermal expansion coefficient of the epoxy resin composite material after curing can be reduced. It should be noted that the average thermal expansion coefficient of zeolite can be measured by calculating the lattice constant using an X-ray diffraction device "D8ADVANCE" manufactured by BRUKER and X-ray diffraction analysis software "JADE".

[0221] (Shape of zeolite)

[0222] As long as the liquid composition and the epoxy resin composite material can show preferred performance, the shape of the zeolite is not particularly limited and can be spherical, whisker-like, fibrous, plate-like, or aggregates thereof. From the perspective of being easy to contain while suppressing viscosity increase, spherical is preferred.

[0223] The sphericity of the zeolite is preferably 0.6 or more, more preferably 0.65 or more, and particularly preferably 0.70 or more. The upper limit of the sphericity is not particularly limited as long as it is 1 or less.

[0224] It should be noted that, in this specification, "sphericity" is defined as "the ratio of the minimum diameter of the particle to the maximum diameter". Zeolites contained in 50 liquid compositions and epoxy resin composite materials were randomly selected, and the sphericity was measured and the average value was taken. The maximum diameter and the minimum diameter can be obtained by observation using a scanning electron microscope (SEM), respectively. It should be noted that, with respect to sphericity, in the first embodiment, as described above, the sphericity of the small-particle zeolite can be within the above range.

[0225] (Skeleton density of zeolite)

[0226] The skeleton density of the zeolite is not particularly limited as long as it does not impair the effect of the present invention. From the perspective of the structural vibration of the zeolite and the easy reduction of the average thermal expansion coefficient, the skeleton density of the zeolite is preferably low. Therefore, the skeleton density of the zeolite is preferably The following, more preferably the following.

[0227] On the other hand, from the viewpoint that the structural stability of the zeolite is easily increased, it is preferred that the framework density of the zeolite is high. The framework density of the zeolite is preferably More preferably The above, more preferably When the skeleton density is within the above range, the zeolite can be used as a stable filler.

[0228] It should be noted that the framework density represents the number of T atoms present per unit volume of zeolite and is a value determined by the structure of the zeolite. In this specification, the values ​​described in the 2017 edition of the IZA Zeolite Structure Database (http: / / www.iza-structure.org / databases / ) may be used.

[0229] As the skeleton density is greater than And for Examples of the following zeolites include zeolites having CSV, ERI, ITG, LTL, LTN, MOZ, MSE, OFF, SAT, SFH, SFN, SSF, *-SSO, and -WEN type structures.

[0230] As the skeleton density is greater than And for Examples of the following zeolites include AEI, AFT, AFV, AFX, AVL, *BEA, BEC, EAB, GME, *-ITN, LEV, MWW, and SFW type zeolites.

[0231] As the skeleton density is greater than And for Examples of the following zeolites include zeolites having CHA, ISV, IWS, KFI, SAS, and SAV type structures.

[0232] As the skeleton density exists in Examples of zeolites within the following range include EMT, FAU, JSR, SBS, SBT, and TSC type zeolites.

[0233] (Silica / alumina molar ratio (SAR) of zeolite)

[0234] The molar ratio of silica / alumina of the zeolite (sometimes referred to as "SAR", "Si / Al2 molar ratio", or "Si / Al2 ratio") is not particularly limited as long as it is a mode that does not impair the effect of the present invention. From the perspective of the easy increase in moisture resistance of the resin composite material described later and the easy control of the amount of counter cations, the SAR (Si / Al2 ratio) of the zeolite is preferably high. Therefore, the SAR (Si / Al2 ratio) of the zeolite is usually 2 or more, preferably 3 or more, more preferably 3.5 or more, further preferably 4 or more, particularly preferably 4.5 or more, and most preferably 5 or more.

[0235] On the other hand, from the perspective of easy and inexpensive production, the SAR (Si / Al2 ratio) of the zeolite is preferably low. Therefore, the SAR (Si / Al2 ratio) of the zeolite is usually 2000 or less, preferably 1000 or less, more preferably 500 or less, and further preferably 100 or less. When the Si / Al2 ratio is within the above range, it is easy to control the amount of counter cations, and the production cost of the zeolite is also low.

[0236] It should be noted that, when gallium, iron, boron, titanium, zirconium, tin, zinc, phosphorus or other elements are used to replace silicon or aluminum, the molar ratio of the oxide of the element to be the replacement element can be converted into the molar ratio of aluminum oxide or silicon dioxide. Specifically, when gallium is used to replace aluminum, the molar ratio of gallium oxide can be converted into the molar ratio of aluminum oxide.

[0237] The Si / Al2 ratio of zeolite can be adjusted by the type and ratio of the silicon-containing compound and the aluminum-containing compound in the raw materials, the type and amount of the structure directing agent, the use of seed crystals, and the synthesis conditions such as temperature and time.

[0238] (Counter cation of zeolite)

[0239] The counter cation of zeolite is not particularly limited as long as it is a mode that does not damage the effect of the present invention. The counter cation of zeolite is generally a structure directing agent, a proton, an alkali metal ion, an alkaline earth metal ion, preferably a structure directing agent, a proton, an alkali metal ion, and more preferably a structure directing agent, a proton, a Li ion, a Na ion, and a K ion. In the case where the counter cation of zeolite is a structure directing agent, compared with alkali metal ions and alkaline earth metal ions, it has flexibility, so zeolite is more likely to show an average thermal expansion coefficient less than 0ppm / K, and is therefore preferred. In addition, the smaller the size of the alkali metal ion and the alkaline earth metal ion, the easier it is for the zeolite to show an average thermal expansion coefficient less than 0ppm / K, and is therefore preferred. Among them, in the case where the counter cation of zeolite is a proton, it is easy to reduce the average thermal expansion coefficient of the resin composite material, and is therefore preferred. That is, as a zeolite, it is preferably as-made (structure directing agent containing type), proton type, alkali metal type, and more preferably as-made, proton type, Li type, Na type, K type. It should be noted that the structure directing agent refers to the template used in the manufacture of zeolite.

[0240] (Crystallinity of zeolite)

[0241] The crystallinity of zeolite is not particularly limited as long as it is a mode that does not damage the effect of the present invention. As the reason, it can be inferred that the Composite Building Unit (CBU) is a factor that has a greater impact on the average thermal expansion coefficient of epoxy resin composite materials compared to the structure determined by coding with IZA. It should be noted that the crystallinity of zeolite can be obtained by an X-ray diffraction device (for example, a desktop X-ray diffraction device "D2PHASER" made by BRUKER), or can be obtained by comparing the X-ray diffraction peak of a zeolite with the X-ray diffraction peak as a benchmark. As a specific calculation example, the crystallinity of the LTA type zeolite of Scientific Reports 2016,6, Article number:29210 can be cited.

[0242] (Surface treatment of zeolite)

[0243] Zeolite may be subjected to surface treatment such as silylation treatment and fluorination treatment within a range not impairing the effects of the present invention. The surface treatment may be a physical treatment or a chemical treatment.

[0244] (Method for producing zeolite)

[0245] The manufacturing method of zeolite can apply known methods. For example, in the case of manufacturing CHA type zeolite, it can be manufactured with reference to the method described in Japanese Patent Publication No. 2009-097856. In the case of manufacturing zeolite with large particle size, the type and ratio of raw materials, synthesis time, temperature, etc. can be appropriately controlled to carry out hydrothermal synthesis. Specifically, for example, the amount of water during synthesis can be increased by the method described in Microporous and Mesoporous Materials 21 (1998) 24., and the synthesis is carried out under the condition of diluting the raw material concentration, thereby manufacturing zeolite with large particle size.

[0246] (Shape of large particle size inorganic filler)

[0247] As long as the liquid composition and the resin composite material show preferred properties, the shape of the large-particle inorganic filler is not particularly limited and can be spherical, whisker-like, fibrous, plate-like, or aggregates thereof. From the perspective of suppressing viscosity increase while containing it, spherical is preferred.

[0248] The sphericity of the large-diameter inorganic filler is preferably 0.6 or more, more preferably 0.65 or more, and particularly preferably 0.70 or more. The upper limit of the sphericity is not particularly limited, and the sphericity may be 1 or less.

[0249] Therefore, in the fourth embodiment of the present invention, the sphericity of both the small-diameter zeolite and the large-diameter inorganic filler is preferably 0.6 or more, more preferably 0.65 or more, and particularly preferably 0.70 or more.

[0250] In addition, the sphericity of the inorganic filler having a large particle size is preferably higher than that of the zeolite having a small particle size.

[0251] (Total inorganic filler content)

[0252] From the aspect of easily showing the effect as a filling material, it is preferred that the total content of all inorganic fillers (total inorganic fillers) contained in the liquid composition is more. On the other hand, from the aspect of the high fluidity of the liquid composition and the easy filling in a narrow space, it is preferred that the total content is less. Specifically, in the liquid composition of the 4th embodiment of the present invention, relative to the total amount of the composition, the total content of all inorganic fillers is preferably more than 30% by mass, more preferably more than 35% by mass, and particularly preferably more than 40% by mass. On the other hand, it is preferably less than 95% by mass, more preferably less than 90% by mass, and particularly preferably less than 85% by mass.

[0253] (Epoxy resin)

[0254] As the epoxy resin used in the present invention, since the thermal expansion coefficient of the epoxy resin composite material obtained by curing the liquid composition is likely to be low, an epoxy compound having an aromatic ring such as a bisphenol A skeleton, a bisphenol F skeleton, or a biphenyl skeleton is preferably used. Specific examples include: bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, biphenyl type epoxy resin, naphthalene ring-containing epoxy resin, epoxy resin having a dicyclopentadiene skeleton, phenol novolac type resin, cresol novolac type epoxy resin, triphenylmethane type epoxy resin, aminophenol type epoxy resin, aliphatic epoxy resin, copolymer epoxy resin of aliphatic epoxy resin and aromatic epoxy resin, etc. Among them, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, biphenyl type epoxy resin, naphthalene ring-containing epoxy resin are preferred, and bisphenol A type epoxy resin, bisphenol F type epoxy resin, naphthalene ring-containing epoxy resin, aminophenol type epoxy resin, and biphenyl type epoxy resin are more preferred.

[0255] Consider the aspect that the glass transition temperature of the epoxy resin composite material formed by the heat curing of the liquid composition is easily increased, preferably use multifunctional epoxy resin.As multifunctional epoxy resin, preferably the glycidyl ether type multifunctional epoxy resins such as the epoxy resin manufactured by various phenolic compounds and epihalohydrin, this phenolic compound is phenol novolac resin, cresol novolac resin, bisphenol A novolac resin, dicyclopentadiene phenolic resin, phenol aralkyl resin, naphthol novolac resin, biphenyl novolac resin, terpene phenolic resin, heavy oil modified phenolic resin etc. are obtained by various phenols, various phenols and the polyphenolic resin etc. of the condensation reaction of the various aldehydes such as hydroxybenzaldehyde, crotonaldehyde, glyoxal.

[0256] From the viewpoint of fluidity, the viscosity of the epoxy resin used in the present invention at 23°C is preferably 5 Pa·s or less, and more preferably 0.1 to 3 Pa·s. The viscosity measurement method of the epoxy resin is specified by JIS K7233 (1986), and the single cylinder rotation viscometer method is suitable. The viscosity of the epoxy resin used in the present invention at 23°C can be measured using a B-type rotational viscometer ("LVDV-1Pri", manufactured by Brookfield, spindle: S62), which is one of the single cylinder rotational viscometer methods.

[0257] From the viewpoint of viscosity control, the epoxy equivalent of the epoxy resin is preferably 50 g / equivalent or more and 500 g / equivalent or less, more preferably 90 g / equivalent or more and 150 g / equivalent or less. From the perspective of excellent heat resistance, a high epoxy equivalent is preferred. On the other hand, by lowering the melting point of the epoxy resin or lowering the viscosity, the filling property of the liquid composition becomes good, and the bonding property based on the filling is easily improved. From this perspective, a low epoxy equivalent is preferred.

[0258] The epoxy resin may be used alone or in combination of two or more in any combination and ratio. The epoxy equivalent in the case of mixing is defined as the equivalent of the mixture.

[0259] From the perspective of relatively increasing the content of inorganic fillers and the like and easily reducing the thermal expansion coefficient, it is preferred that the content of the epoxy resin in the liquid composition of the present invention is small. On the other hand, from the perspective of easily maintaining the excellent physical properties of the epoxy resin, it is preferred that the content of the epoxy resin is large. Specifically, it is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the composition. On the other hand, it is preferably 50% by mass or less, more preferably 25% by mass or less, and particularly preferably 15% by mass or less.

[0260] (Curing agent)

[0261] The liquid composition of the present invention preferably further comprises a curing agent. The curing agent is a substance that assists the crosslinking reaction between crosslinking groups of the epoxy resin.

[0262] The curing agent is not particularly limited, and generally, curing agents known as epoxy resin curing agents can be used. Examples include phenolic curing agents, aliphatic amines, polyether amines, alicyclic amines, amine curing agents such as aromatic amines, acid anhydride curing agents, amide curing agents, tertiary amines, imidazoles and their derivatives, organic phosphines, Salts, tetraphenyl boron salts, organic acid dihydrazides, halogenated boron amine complexes, polythiol curing agents, isocyanate curing agents, blocked isocyanate curing agents, dicyandiamide compounds, etc. From the viewpoint of imparting fluidity and rapid curing properties, the curing agent is preferably an acid anhydride curing agent.

[0263] Specific examples of the phenolic curing agent include bisphenol A, bisphenol F, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxydiphenyl ether, 1,4-bis(4-hydroxyphenoxy)benzene, 1,3-bis(4-hydroxyphenoxy)benzene, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, phenol novolac, bisphenol A novolac, o-cresol novolac, m-cresol novolac, p-cresol novolac, xylenol novolac, polyparahydroxystyrene, hydroquinone, resorcinol, catechol, and tert-butylcatechol. , tert-butylhydroquinone, fluoroglycinol, pyrogallol, tert-butylpyrogallol, allylated pyrogallol, polyallylated pyrogallol, 1,2,4-pyrogallol, 2,3,4-trihydroxybenzophenone, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,4-dihydroxynaphthalene, 2,5-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 2,8-dihydroxynaphthalene, allylated or polyallylated products of the above dihydroxynaphthalenes, allylated bisphenol A, allylated bisphenol F, allylated phenol novolac, allylated pyrogallol, etc.

[0264] Specific examples of amine curing agents include aliphatic amines such as ethylenediamine, 1,3-diaminopropane, 1,4-diaminopropane, hexamethylenediamine, 2,5-dimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylenetriamine, iminobispropylamine, bis(hexamethylene)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-hydroxyethylethylenediamine, and tetrakis(hydroxyethyl)ethylenediamine.

[0265] Examples of the polyetheramines include triethylene glycol diamine, tetraethylene glycol diamine, diethylene glycol bis(propylamine), polyoxypropylene diamine, and polyoxypropylene triamine.

[0266] Examples of the alicyclic amines include isophoronediamine, menthanediamine, N-aminoethylpiperazine, bis(4-amino-3-methyldicyclohexyl)methane, bis(aminomethyl)cyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, and norbornenediamine.

[0267] Examples of the aromatic amines include tetrachloro-p-phenylenediamine, m-phenylenediamine, p-phenylenediamine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, 2,4-diaminoanisole, 2,4-toluenediamine, 2,4-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, 2,4-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, m-aminophenol, m-aminobenzylamine, benzyldimethylamine, 2-dimethylaminomethylphenol, triethanolamine, methylbenzylamine, α-(m-aminophenyl)ethylamine, α-(p-aminophenyl)ethylamine, diaminodiethyldimethyldiphenylmethane, and α,α'-bis(4-aminophenyl)-p-diisopropylbenzene.

[0268] Specific examples of the acid anhydride curing agent include dodecenylsuccinic anhydride, polyadipic anhydride, polyazelaic anhydride, polysebacic anhydride, poly(ethyloctadecane dioic acid) anhydride, poly(phenylhexadecanedioic acid) anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, methylhumic anhydride, tetrahydrophthalic anhydride, trialkyltetrahydrophthalic anhydride, methylcyclohexene dicarboxylic anhydride, methylcyclohexene tetracarboxylic anhydride, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenone. Tetracarboxylic anhydride, ethylene glycol trimellitic dianhydride, chlorobridged anhydride, nadic anhydride, methyl nadic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexane-1,2-dicarboxylic anhydride, 3,4-dimethyl-6-(2-methyl-1-propenyl)-4-cyclohexene-1,2-dicarboxylic anhydride, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic anhydride, 1-methyldicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic anhydride, and the like.

[0269] Examples of the amide curing agent include dicyandiamide and polyamide resin.

[0270] Examples of the tertiary amine include 1,8-diazabicyclo(5,4,0)undecene-7, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol.

[0271] Examples of imidazole and its derivatives include 1-cyanoethyl-2-phenylimidazole, 2-phenylimidazole, 2-ethyl-4(5)-methylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole Trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins and the above imidazoles or polymer encapsulated imidazoles, etc.

[0272] Examples of the organic phosphine include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine. Salts such as tetraphenyl Tetraphenylborate, tetraphenyl Ethyl triphenyl borate, tetrabutyl Tetrabutyl borate and the like; examples of tetraphenyl borate include 2-ethyl-4-methylimidazolium tetraphenyl borate and N-methylmorpholine tetraphenyl borate.

[0273] These curing agents may be used alone or in combination of two or more in any ratio.

[0274] From the perspective of being less likely to cause the influence caused by the residue of unreacted epoxy groups and functional groups of the curing agent, when the curing agent is a phenolic curing agent, an amine curing agent, or an acid anhydride curing agent, it is preferred that the content of the curing agent when the liquid composition of the present invention contains the curing agent be in a range of 0.8 to 2.0 in terms of the equivalent ratio of the epoxy groups in the epoxy resin to the functional groups in the curing agent (functional groups in the curing agent / epoxy groups in the epoxy resin), and more preferably in a range of 0.8 to 1.5.

[0275] When the curing agent is an amide curing agent, a tertiary amine, imidazole and its derivatives, an organic phosphine, In the case of salts, tetraphenyl boron salts, organic acid dihydrazides, halogenated boron amine complexes, polythiol curing agents, isocyanate curing agents, blocked isocyanate curing agents, etc., preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the epoxy resin. On the other hand, preferably 20 parts by mass or less, more preferably 10 parts by mass or less.

[0276] In the case of a dicyandiamide compound, it is preferably used in an amount of 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, based on 100 parts by mass of the epoxy resin, while it is preferably used in an amount of 10 parts by mass or less, more preferably 6 parts by mass or less.

[0277] (Dispersant)

[0278] In order to improve the dispersibility of the inorganic filler, the liquid composition of the fourth embodiment of the present invention may contain a dispersant. The dispersant used in the liquid composition containing the resin and the filler is mainly used in the liquid composition containing the resin and the filler with large polarity differences, thereby improving the interface state of the two and improving the compatibility. As a result, it can show effects in reducing viscosity, improving the dispersibility of the filler, and preventing the filler from agglomerating and settling.

[0279] In the fourth embodiment, from the perspective of easily dispersing the inorganic filler in the liquid composition, the content of the dispersant is preferably high. On the other hand, from the perspective of not easily causing the increase in the thermal expansion coefficient caused by the phase separation of the inorganic filler and the epoxy resin, the content of the dispersant is preferably low. From the perspective of easily filling the liquid composition in a narrow space and easily achieving a low thermal expansion coefficient after curing, the content of the dispersant is preferably 0.1% by mass or more and 30% by mass or less, more preferably 0.1% by mass or more and 25% by mass or less, relative to the total amount of the liquid composition.

[0280] (Reactive diluent)

[0281] The liquid composition of the present invention may contain a reactive diluent. The reactive diluent is not particularly limited as long as it contains at least one monofunctional epoxy compound. A monofunctional epoxy compound is an epoxy compound having one epoxy group, and has been used as a reactive diluent to adjust the viscosity of epoxy resin compositions. Monofunctional epoxy compounds can be roughly divided into aliphatic monofunctional epoxy compounds and aromatic monofunctional epoxy compounds. From the viewpoint of viscosity, aromatic monofunctional epoxy compounds are preferred.

[0282] (Other additives)

[0283] In addition to the above, the liquid composition may appropriately contain other additives selected from coupling agents, UV protection agents, antioxidants, plasticizers, flame retardants, colorants, fluidity improvers, defoaming agents, ion trapping agents, and the like.

[0284] In addition, the liquid composition in the present embodiment is preferably a solvent-free type. By being set to a solvent-free type, it is possible to prevent the solvent from volatilizing and generating gaps when the liquid composition is heated and cured. It should be noted that solvent refers to a volatilizing component, and in this specification, it is a term that includes water and an organic solvent. The solvent-free liquid composition does not substantially contain a solvent, for example, relative to the total amount of the liquid composition, the content of the solvent is preferably less than 3% by mass, more preferably less than 1% by mass, and most preferably 0% by mass.

[0285] (Viscosity of liquid composition)

[0286] The liquid composition is a composition that has fluidity at room temperature (23°C). From the perspective of being easy to fill the composition even in a narrow space, the viscosity of the liquid composition of the fourth embodiment of the present invention is preferably low. On the other hand, from the perspective of preventing liquid sag from occurring when filling the composition, the viscosity of the liquid composition of the fourth embodiment of the present invention is preferably high. The viscosity of the liquid composition at 23°C is preferably 0.1 Pa·s or more, more preferably 1 Pa·s or more, further preferably 5 Pa·s or more, and particularly preferably 10 Pa·s or more. On the other hand, it is preferably 250 Pa·s or less, more preferably 200 Pa·s or less, further preferably 150 Pa·s or less, particularly preferably 60 Pa·s or less, and particularly preferably 30 Pa·s or less. In addition, the viscosity at 23°C is most preferably 1 Pa·s or more and 30 Pa·s or less.

[0287] The viscosity of the liquid composition can be measured in the same manner as the viscosity measurement method of the epoxy resin described above. The viscosity of the liquid composition used in the present invention at 23°C can be measured using a B-type rotational viscometer, which is one of the single cylinder rotational viscometer methods. The B-type rotational viscometer can be, for example, the B-type rotational viscometer described in the Examples.

[0288] (Average thermal expansion coefficient)

[0289] From the aspect that the epoxy resin composite material is not easily deformed by the surrounding temperature environment, heat generation, etc., it is preferred that the average thermal expansion coefficient (CTE1) of the liquid composition of the fourth embodiment of the present invention is low when it is made into a cured product. On the other hand, from the aspect that it is not easy to cause damage caused by the difference in the average thermal expansion of the surrounding components, it is preferred to be close to the average thermal expansion coefficient of the surrounding components. Therefore, when the liquid composition is used as a bottom filling material, etc. for the manufacture of semiconductor devices, it is preferably close to the average thermal expansion coefficient of the semiconductor substrate (for example, 3 to 4 ppm / K).

[0290] From the above viewpoints, the average thermal expansion coefficient (CTE1) when the liquid composition of the fourth embodiment of the present invention is made into a solidified product is preferably 0 ppm / K or more, more preferably 2 ppm / K or more, further preferably 4 ppm / K or more, and particularly preferably 10 ppm / K or more. On the other hand, it is preferably 200 ppm / K or less, further preferably 100 ppm / K or less, and particularly preferably 30 ppm / K or less.

[0291] It should be noted that, for the average thermal expansion coefficient of the cured product obtained by curing the liquid composition and the glass transition temperature (Tg) described later, it is sufficient to measure the average thermal expansion coefficient of the epoxy resin composite material (cured product) obtained by curing the liquid composition to a gel fraction of 80% or more. The average thermal expansion coefficient (CTE1) is determined as follows: According to JIS K7197 (2012), the temperature change of the change in sample length at 25 to 100°C is measured by the compression method using thermomechanical analysis, and the slope of the tangent is used to determine it. The specific measurement conditions of the average thermal expansion coefficient are described in the examples.

[0292] (Glass transition temperature)

[0293] The glass transition temperature (Tg) of the epoxy resin composite material obtained by making the liquid composition of the fourth embodiment of the present invention into a cured product is not particularly limited. For example, when the Tg as the bottom filling material is high, the part sealed with the bottom filling material has high bump protection at high temperature and excellent heat cycle resistance, so it is preferred (for example, with reference to Japanese Patent Publication No. 2017-110146). From such a viewpoint, the glass transition temperature (Tg) of the cured product when the liquid composition of the fourth embodiment is made into a cured product is preferably 50°C or more, more preferably 80°C or more.

[0294] In addition, when the glass transition temperature is 150°C or less, there is a tendency that the warpage at room temperature (23°C) is not easy to increase, so the glass transition temperature (Tg) is preferably 50 to 150°C, and more preferably 80 to 150°C. It should be noted that the glass transition temperature (Tg) can be measured by a thermomechanical analyzer (TMA). Specifically, it can be measured by the method described in the examples.

[0295] (Method for producing liquid composition)

[0296] The liquid composition of the fourth embodiment of the present invention can be generally obtained as follows: epoxy resin, inorganic filler, curing agent, dispersant, reactive diluent, and other additive components are mixed and kneaded using a vacuum mixer, mixing roll, planetary mixer, etc., and degassed as needed. As long as there is no particular problem in the reaction and the generation of precipitates, the order of mixing these components is arbitrary, and any two or more components of the constituent components can be mixed in advance, and then the remaining components can be mixed, or all the components can be mixed at once.

[0297] In addition, for example, by using zeolite having a particle size of 0.05 μm or more and less than 1 μm and an inorganic filler having a particle size of 1 μm or more and less than 50 μm as raw materials for manufacturing a liquid composition, the liquid composition can contain small-particle zeolite and large-particle inorganic filler produced by the above-mentioned method, and the liquid composition can also contain small-particle zeolite and large-particle inorganic filler produced by other methods.

[0298] <Epoxy resin composite materials>

[0299] The epoxy resin composite material of the fourth embodiment of the present invention can be obtained by curing the above-mentioned liquid composition. The epoxy resin composite material of the fourth embodiment is an epoxy resin composite material containing epoxy resin and inorganic filler, and the inorganic filler contains a zeolite (small particle size zeolite) with a particle size of 0.05 μm or more and less than 1 μm and an inorganic filler (large particle size inorganic filler) with a particle size of 1 μm or more and less than 50 μm. By making the epoxy resin composite material of the fourth embodiment contain small particle size zeolite and large particle size inorganic filler, the thermal expansion coefficient can be lowered and manufactured from a liquid composition with lower viscosity.

[0300] In the epoxy resin composite material of the fourth embodiment of the present invention, the epoxy resin and the inorganic filler are as described above. In addition, the epoxy resin composite material may also appropriately contain the components contained in the liquid composition in addition to the epoxy resin and the inorganic filler. Moreover, the content of each component in the epoxy resin composite material is as described above, except that the total amount of the epoxy resin composite material is used instead of the total amount of the liquid composition as a reference. In addition, the epoxy resin composite material is preferably cured to a gel fraction of 80% or more, preferably by a curing agent contained in the above-mentioned liquid composition.

[0301] From the same viewpoint as above, the preferred ranges of the average coefficient of thermal expansion (CTE1) and the glass transition temperature of the epoxy resin composite material in the fourth embodiment of the present invention are the same as the preferred ranges when the above-mentioned liquid composition is made into a cured product. In addition, the average coefficient of thermal expansion and the glass transition temperature can be measured by the above-mentioned measuring method for the epoxy resin composite material.

[0302] (Method for producing epoxy resin composite material)

[0303] The epoxy resin composite material can be obtained by curing the liquid composition. Curing is preferably performed by heating. As long as the epoxy resin composite material shows preferred performance, the manufacturing method of the epoxy resin composite material is not particularly limited and can be appropriately performed according to the composition of the liquid composition by utilizing a known method.

[0304] The epoxy resin composite material is preferably formed by filling the liquid composition into the gaps between components of various products such as electronic devices and then curing the components. Alternatively, the epoxy resin composite material can be formed by applying the liquid composition to components of various products and curing the components.

[0305] In addition, it is also possible to shape by curing the liquid composition in a desired shape, for example, under the state of being accommodated in a mold. In the manufacture of such a molded body, injection molding, injection compression molding, extrusion molding or compression molding can be utilized. In addition, the molding, i.e. curing of epoxy resin composite materials can be carried out under respective curing temperature conditions. In addition, epoxy resin composite materials can also be obtained by cutting the cured product of the liquid composition into a desired shape.

[0306] The heating temperature during thermal curing is also affected by the curing agent used, etc., and is not particularly limited, but is usually 30° C. or higher, preferably 50° C. or higher, more preferably 60° C. or higher, and further preferably 80° C. or higher. On the other hand, the heating temperature is usually 400° C. or lower, preferably 350° C. or lower, more preferably 300° C. or lower, and further preferably 250° C. or lower. When the curing temperature is within the above range, a high-quality resin composite material can be easily obtained in a short time.

[0307] [Fifth embodiment]

[0308] As a fifth embodiment, the present invention relates to an epoxy resin composite material containing zeolite as an inorganic filler and having a low average thermal expansion coefficient. The fifth embodiment of the present invention will be described below.

[0309] Specifically, the epoxy resin composite material of the fifth embodiment contains an epoxy resin and an inorganic filler, and the average thermal expansion coefficient of the epoxy resin composite material at 25 to 100° C. is 0 ppm / K or more and 200 ppm / K or less, and the inorganic filler contains zeolite. As described above, the average thermal expansion coefficient is more preferably 2 ppm / K or more, particularly preferably 4 ppm / K or more, and more preferably 100 ppm / K or less, particularly preferably 30 ppm / K or less.

[0310] In the fifth embodiment of the present invention, by making the inorganic filler contain zeolite, the average thermal expansion coefficient can be reduced as described above. From such a viewpoint, relative to the total amount of epoxy resin composite material, the content of zeolite in the fifth embodiment is preferably 20% by mass or more, more preferably 25% by mass or more, further preferably 30% by mass or more, more particularly preferably 40% by mass or more, and most preferably 45% by mass or more. In addition, from the viewpoint of suppressing the viscosity increase of the liquid composition used to obtain the epoxy resin composite material, the above content is preferably 90% by mass or less, more preferably 80% by mass or less, further preferably 75% by mass or less, and particularly preferably 70% by mass or less.

[0311] In addition, from the perspective of easily reducing the thermal expansion coefficient and further from the perspective of easily maintaining the excellent physical properties of the epoxy resin, the epoxy resin in the epoxy resin composite material of the fifth embodiment is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the epoxy resin composite material. On the other hand, it is preferably 50% by mass or less, more preferably 25% by mass or less, and particularly preferably 15% by mass or less.

[0312] In addition, in the fifth embodiment of the present invention, a liquid composition for obtaining the above-mentioned epoxy resin composite material is also provided. Specifically, the liquid composition of the fifth embodiment is a liquid composition containing an epoxy resin and an inorganic filler, and when the composition is made into a cured product with a gel fraction of 80% or more, the average thermal expansion coefficient at 25 to 100°C is 0 ppm / K or more and 200 ppm / K or less, and the above-mentioned inorganic filler contains zeolite. The determination method and preferred range of the average thermal expansion coefficient are the same as those of the above-mentioned epoxy resin composite material.

[0313] In addition, the viscosity of the liquid composition of the fifth embodiment at 23° C. is preferably 0.1 Pa·s or more and 250 Pa·s or less, and more preferably 1 Pa·s or more and 30 Pa·s or less. This can reduce the thermal expansion coefficient of the cured product and achieve low viscosity. The preferred range of the viscosity of the liquid composition at 23° C. is as described in the first embodiment above.

[0314] It should be noted that, in the fifth embodiment, the details other than the contents of the epoxy resin and zeolite are as described in the fourth embodiment. In addition, the inorganic filler of the fifth embodiment preferably includes small-diameter zeolite as described above, and the content of the small-diameter zeolite and other details are the same as those of the fourth embodiment, and the description thereof is omitted.

[0315] In addition, the inorganic filler may contain an inorganic filler other than zeolite. The details of the inorganic filler other than zeolite are the same as those of the fourth embodiment.

[0316] In addition, the liquid composition of the 5th embodiment is the same as the 4th embodiment, preferably contains a curing agent, and may contain a reactive diluent or other additives, etc., and these components are as described above. In addition, the liquid composition of the 5th embodiment is also preferably a solvent-free type, and its details are as described above.

[0317] In the fifth embodiment, the inorganic filler also preferably contains a small-diameter zeolite and a large-diameter inorganic filler, similarly to the fourth embodiment. The liquid composition or epoxy resin composite material in the fifth embodiment may contain a dispersant.

[0318] (use)

[0319] The composition and resin composite material of the present invention can be used in catalyst components, molecular sieve membrane components, optical components, hygroscopic components, food, building components, and components and packaging components of electronic devices, etc., wherein, it is preferably used in electronic devices. Therefore, as a preferred embodiment, the present invention provides an electronic device containing a resin composite material, and more preferably provides an electronic device containing an epoxy resin composite material.

[0320] An electronic device is a device having more than two electrodes and controlling the current flowing between these electrodes, the voltage generated by electricity, light, magnetism or chemical substances, or a device that generates light, electric field, and magnetic field by the applied voltage and current. Specifically, resistors, rectifiers (diodes), switching elements (transistors, thyristors), amplifier elements (transistors), memory elements, chemical sensors, etc., or devices obtained by combining or integrating these elements can be cited. In addition, photodiodes or photosensitive transistors that generate photocurrent, electroluminescent elements that emit light by applying an electric field, and optical elements such as photoelectric conversion elements or solar cells that generate electromotive force by light can also be cited. An electronic device is preferably a semiconductor device. A semiconductor device can have at least a semiconductor substrate, for example, a device having a semiconductor chip mounted on a substrate, a device having multiple layers of semiconductor chips and a semiconductor substrate stacked thereon, etc. can be cited.

[0321] The liquid composition of the present invention is preferably used as a liquid sealant. In this case, the epoxy resin composite material formed by curing the liquid composition can serve as a sealing material.

[0322] By filling the gap formed in the constituent members with the liquid sealant and then solidifying it, it can be used as a sealing material for filling the gap.

[0323] In addition, after applying the liquid sealant to various components, for example, another component is overlapped on the liquid sealant and then appropriately cured, so that it can be used as a sealing material to fill the gap between the components. In this case, the liquid sealant can be appropriately cured and B-staged before overlapping another component.

[0324] Among them, the liquid composition of the present invention is preferably used for filling in a gap and solidifying. That is, it is preferred to manufacture a sealing material by solidifying the liquid composition of the present invention after filling the gap. The liquid composition of the present invention is low in viscosity and can be filled in a narrow gap without generating voids.

[0325] Liquid composition of the present invention is preferably used as liquid sealant, and is particularly preferably used as bottom filling material. Bottom filling material is preferably used in the manufacture of electric devices, particularly semiconductor devices, and is preferably used in the purposes of filling the gap between substrate and semiconductor chip, between substrates, between semiconductor chips, etc. The substrate can use known substrates, and can use substrates made of organic materials such as epoxy resin substrates, phenolic resin substrates, etc. In addition, semiconductor chips can be formed by semiconductor substrates such as silicon substrates.

[0326] The liquid composition of the present invention has a low thermal expansion coefficient in its cured product, and by using it as an underfill material, the difference in thermal expansion coefficient of a semiconductor substrate etc. is reduced, thereby improving heat cycle resistance etc.

[0327] The underfill material is preferably filled in the gap between the substrate and the semiconductor chip in a laminated body having a semiconductor chip mounted on the substrate, and then cured by heating to be used as a sealing material for sealing the substrate and the chip. In this case, the semiconductor chip can be bonded to the surface of the substrate having a wiring pattern formed thereon via bumps, for example, by reflow soldering, before filling the underfill material.

[0328] The bottom filling material can be used in the manufacture of semiconductor devices using the pre-coating method. Specifically, on the surface of a semiconductor chip formed with a plurality of bumps, the bottom filling material is filled between the plurality of bumps to form a bottom filling layer. Here, the filled bottom filling material can be B-staged as needed. Then, the semiconductor chip formed with the bottom filling layer can be placed on the surface of the substrate in a manner such that the surface on the side formed with the bottom filling layer faces the substrate. Next, the bottom filling layer can be cured by heating and pressing, etc. to become a sealing material. In addition, the semiconductor chip can be bonded to the surface of the substrate formed with a wiring pattern via the bumps.

[0329] In addition, in the pre-coating method, an underfill material can be applied to the surface of the substrate on which the wiring pattern is formed to form an underfill layer. Here, the applied underfill layer can be B-staged as needed. Then, the semiconductor chip formed with the bumps can be placed on the substrate formed with the underfill layer in such a way that the surface of the side formed with the bumps faces the surface of the substrate formed with the underfill layer. Then, the underfill layer can be cured into a sealing material by heating and pressing, etc., and the semiconductor chip can be bonded to the surface of the substrate formed with the wiring pattern via the bumps.

[0330] It should be noted that, in the above description, an example of a bottom filling material being used as a sealing material for filling a gap between a substrate and a semiconductor chip is described, but the use of the bottom filling material is not particularly limited, and the gap between semiconductor chips can be filled, and the gap between substrates can also be filled. In addition, the substrate is not limited to a substrate made of an organic material, and can also be a semiconductor substrate, etc.

[0331] Example

[0332] Hereinafter, the present invention will be described in more detail using Examples, Comparative Examples, and Reference Examples. However, the present invention is not limited to the following Examples, Comparative Examples, and Reference Examples unless it departs from the gist of the present invention.

[0333] <Synthesis of Zeolite>

[0334] [Example 1]

[0335] (Manufacture of spherical zeolite (zeolite filler A))

[0336] Sodium hydroxide manufactured by Kishida Chemical, potassium hydroxide manufactured by Kishida Chemical, N,N,N-trimethyl-1-adamantanammonium hydroxide (TMAdaOH) manufactured by Sachem as a structure directing agent (SDA), "KYOWAAD 200S" manufactured by Kyowa Chemical Co., Ltd. as aluminum hydroxide, "Cataloid SI-30" manufactured by JGC Catalysts & Chemicals Co., Ltd. as silicon dioxide, and "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd. were added to the container in order. The composition (molar ratio) of the obtained mixture was SiO2:Al2O3:NaOH:KOH:TMAdaOH:H2O:KBM-403=1.0:0.033:0.07:0.06:0.07:20:0.025. After adding 2% by mass of CHA zeolite seed crystals relative to the amount of silica and mixing thoroughly, the resulting mixture was placed in a pressure-resistant container and subjected to hydrothermal synthesis in an oven at 160°C under stirring conditions for 48 hours. After suction filtration and washing, it was dried. The resulting powder was calcined at 600°C for 6 hours under air circulation to remove TMAdaOH as a structure directing agent (SDA) and obtain CHA aluminosilicate zeolite. The SEM photograph of the resulting zeolite is shown in Figure 1 . It is a zeolite in which the particle size of each particle is within the range of 0.1 μm or more and less than 1.0 μm, and the average primary particle size is 0.5 μm. It should be noted that the average primary particle size is set as the average value of the particle sizes of 50 randomly selected primary particles. It is a spherical particle with a Si / Al2 ratio of 26.1, a sphericity of 0.88, a roundness of 0.89, and a skeleton density of The counter cations are potassium, sodium, and proton-type. Table 1 shows the physical properties of the zeolite.

[0337] [Comparative Example 1]

[0338] (Manufacture of cubic zeolite (zeolite filler B))

[0339] Sodium hydroxide manufactured by Kishida Chemical, potassium hydroxide manufactured by Kishida Chemical, N,N,N-trimethyl-1-adamantanammonium hydroxide (TMAdaOH) manufactured by Sachem as a structure directing agent (SDA), "KYOWAAD 200S" manufactured by Kyowa Chemical Co., Ltd. as aluminum hydroxide, and "Cataloid SI-30" manufactured by JGC Catalysts & Chemicals Co., Ltd. as silica were added to the container in order. The composition (molar ratio) of the obtained mixture was SiO2:Al2O3:NaOH:KOH:TMAdaOH:H2O=1.0:0.033:0.07:0.06:0.07:20. After adding 2% by mass of seed crystals of CHA type zeolite relative to the amount of silica and mixing thoroughly, the obtained mixture was placed in a pressure-resistant container and subjected to hydrothermal synthesis in an oven at 160°C under stirring conditions for 48 hours. After filtration and washing, the mixture was dried. The obtained powder was calcined at 600°C for 6 hours under air circulation to remove TMAdaOH as a structure directing agent (SDA) and obtain CHA-type aluminosilicate zeolite. The SEM photograph of the obtained zeolite is shown in Figure 2 The particle size of each particle is within the range of 1.0 μm to 10 μm, and the average primary particle size is 0.5 μm. It should be noted that the average primary particle size is the average of the particle sizes of 50 randomly selected primary particles. The Si / Al2 ratio is 24.2, the sphericity is 0.60, the roundness is 0.79, and the skeleton density is The counter cations are potassium, sodium, and proton-type. Table 1 shows the physical properties of the zeolite.

[0340] [Table 1]

[0341] Silane coupling agent <![CDATA[Si / Al2 ratio]]> Average primary particle size Sphericity Roundness Example 1 have 26.1 0.5μm 0.88 0.89 Comparative Example 1 none 24.2 0.5μm 0.68 0.79

[0342] The results in Table 1 confirm that the zeolite of the first embodiment of the present invention can be produced by the production method of the present invention. On the other hand, compared with Comparative Example 1, it is known that a cubic zeolite with small sphericity and roundness can be produced by producing without using a silane coupling agent. Figure 2 As can be seen from the SEM image shown, the zeolite produced in Comparative Example 1 is cubic.

[0343] Next, examples of the composition and resin composite material of the present invention will be described.

[0344] <Combination ingredients>

[0345] The components used in the preparation of the liquid composition and the resin composite material are as follows.

[0346] <Inorganic filler>

[0347] As the zeolite fillers A and B, the zeolite fillers A and B produced in the above-mentioned Example 1 and Comparative Example 1 were used, respectively.

[0348] The inorganic fillers other than the zeolite fillers A and B are as follows.

[0349] Silica filler A: manufactured by Admatechs, trade name “FE920A-SQ” (average particle size 4 μm, true spherical silica filler)

[0350] <Epoxy resin>

[0351] Mitsubishi Chemical Corporation, trade name "jER630" (p-aminophenol type epoxy resin, epoxy equivalent: 97 g / equivalent)

[0352] <Polyimide powder>

[0353] Ube Industries, Ltd., trade name "UIP-R" (polyimide, average particle size: 7 μm, specific gravity 1.39)

[0354] <Curing Agent>

[0355] Acid anhydride curing agent: manufactured by Hitachi Chemical Co., Ltd., trade name "HN-2200" (methyltetrahydrophthalic anhydride, amine equivalent 83 g / equivalent)

[0356] (Physical Property Evaluation)

[0357] Physical property evaluation was performed as follows.

[0358] (Gel fraction)

[0359] The gel fraction of the resin composite material was measured according to the following procedure.

[0360] The resin composite material prepared under the curing conditions of 120°C and 2 hours after heat treatment at 80°C for 2 hours was cut into pieces within the range of 0.5 to 0.6 g and placed on a metal mesh. The metal mesh was left to stand for 24 hours while being immersed in acetone. Then, the metal mesh was taken out from the acetone and vacuum dried. The ratio of the weight of the resin composite material after being immersed in acetone to the weight before being immersed was taken as the gel fraction.

[0361] (Viscosity of liquid composition)

[0362] The viscosity of the liquid composition at 23° C. was measured using a B-type rotational viscometer. As the B-type rotational viscometer, a "LVDV-1Pri" manufactured by Brookfield, with a spindle of S64 or S63, was used when the viscosity was 0.1 to 100 Pa·s, and a "HBDV-E" manufactured by Brookfield, with a spindle of S-07 was used when the viscosity exceeded 100 Pa·s. It should be noted that the value measured at 20 rpm was taken as a representative value of the viscosity of each sample.

[0363] (Average coefficient of thermal expansion (CTE1) of epoxy resin and epoxy resin composites)

[0364] The average thermal expansion coefficient of the epoxy resin composite material obtained by curing the liquid composition to a gel fraction of 80% or more was measured by thermomechanical analysis according to JIS K7197 (2012). The measurement was performed by a compression method using a thermomechanical analyzer (device name: TMA SS7100, manufactured by SII Nano Technology).

[0365] Specifically, the epoxy resin composite material was cut into a size of φ6mm×10mm, and a temperature drop measurement was performed from 200°C to 20°C at 5°C / min using a thermomechanical analysis device by a compression method. The temperature change of the change in sample length at 25-100°C was measured, and the slope of the tangent was used as the average thermal expansion coefficient (CTE1).

[0366] (Average thermal expansion coefficient of polyimide resin and polyimide resin composite material (CTE1))

[0367] The average thermal expansion coefficient of the polyimide resin composite material obtained by curing to a gel fraction of 80% or more was measured by thermomechanical analysis according to the method of JIS K7197 (2012). The thermomechanical analyzer (device name: TMA SS7100, manufactured by SII Nano Technology) was used to measure the average thermal expansion coefficient by compression method. Specifically, the polyimide resin composite material was cut into a size of 10 mm in width, 6 mm in thickness, and 10 mm in height, and the temperature was lowered from 200°C to 20°C at 5°C / min using a thermomechanical analyzer by compression method, and the temperature change of the change in sample length at 25 to 100°C was measured, and the slope of the tangent was used as the average thermal expansion coefficient (CTE1).

[0368] (Glass transition temperature of epoxy resin composites)

[0369] The glass transition temperature (Tg) of the epoxy resin composite material obtained by curing the liquid composition to a gel fraction of 80% or more was measured by a thermomechanical analyzer (TMA). Specifically, the measurement was performed using the same device and conditions as the evaluation of the above-mentioned thermal expansion coefficient, and a graph with temperature as the X-axis and the linear expansion coefficient as the Y-axis was prepared. CTE'1 was determined based on the slope of the tangent line at 15 to 75°C of the graph, CTE'2 was determined based on the slope of the tangent line at 150 to 200°C, and the glass transition temperature Tg (°C) was determined based on the intersection of CTE'1 and CTE'2.

[0370] [Example 2]

[0371] 16 g of epoxy resin, 24 g of curing agent, and 60 g of zeolite filler A were weighed and mixed in a cup in a manner as shown in Table 2. Then, a vacuum mixer (manufactured by EME, "V-mini 300") was used to mix at 1500 rpm for 5 minutes to prepare a liquid composition. The viscosity of the liquid composition at 23°C was measured by a rotational viscometer. Then, it was injected into a molding mold, heated at 80°C for 2 hours, and then heated at 120°C for 2 hours to cure to a gel fraction of more than 80%, and then demolded to obtain an epoxy resin composite material.

[0372] [Comparative Example 2]

[0373] 16 g of epoxy resin, 24 g of curing agent, and 60 g of zeolite filler B were weighed and mixed in a cup to obtain the formulation shown in Table 2. A liquid composition and a resin composite material thereof were obtained in the same manner as in Example 2 except for the formulation ratio.

[0374] [Example 3]

[0375] 16 g of epoxy resin, 24 g of curing agent, 20 g of zeolite filler A, and 40 g of silica filler were weighed and mixed in a cup to obtain the formulation shown in Table 2. A liquid composition and a resin composite material thereof were obtained in the same manner as in Example 2 except for the formulation ratio.

[0376] [Comparative Example 3]

[0377] 16 g of epoxy resin, 24 g of curing agent, and 60 g of silica filler were weighed and mixed in a cup to obtain the formulation shown in Table 2. A liquid composition and a resin composite material thereof were obtained in the same manner as in Example 2 except for the formulation ratio.

[0378] [Comparative Example 4]

[0379] In Example 2, except that no zeolite filler was used, a liquid composition and a resin composite material thereof were obtained in the same manner as in Example 2.

[0380] The viscosity of each liquid composition in Examples 2 and 3 and Comparative Examples 2 to 4 was measured, and the average thermal expansion coefficient (CTE1) and glass transition temperature Tg of the epoxy resin composite material were measured.

[0381] [Table 2]

[0382]

[0383] The results of Examples 2 and 3 confirmed that the inclusion of the zeolite of the present invention can provide a liquid composition with a low viscosity and can reduce the thermal expansion coefficient of the resin composite material obtained by curing the liquid composition.

[0384] That is, it was confirmed that the inclusion of the zeolite of the present invention can provide a liquid composition with a low viscosity, and the thermal expansion coefficient of the resin composite material obtained by curing the liquid composition can be reduced.

[0385] In addition, it can be confirmed according to Example 3 that by using a small-diameter zeolite in combination with a large-diameter inorganic filler, the liquid composition has a low viscosity, and by curing it, an epoxy resin composite material with a low thermal expansion coefficient can be obtained. In contrast, the resin composite material of Comparative Example 2 contains fillers in the same amount, but its thermal expansion coefficient is high. That is, by using a small-diameter zeolite in combination with a large-diameter inorganic filler, a low-viscosity liquid composition can be obtained, and the thermal expansion coefficient of the resin composite material formed by curing the liquid composition can be reduced.

[0386] [Example 4]

[0387] 21 g of polyimide powder and 9 g of zeolite filler A prepared in Example 1 were weighed in a cup, mixed, and laid on a press mold. The mold was placed in a high-temperature vacuum press device (produced by Kitagawa Seiki Co., Ltd.), and pressurized at a press temperature of 390° C. and a press surface pressure of 8 MPa for 30 minutes, and then demolded to obtain a molded body with a length of 11 cm, a width of 2.5 cm, and a thickness of 6 mm.

[0388] [Example 5]

[0389] 21 g of the polyimide powder and 9 g of the silica filler were weighed in a cup, mixed, and spread on a press mold, and then a molded body was obtained in the same manner as in Example 4.

[0390] [Comparative Example 5]

[0391] A molded body was produced in the same manner as in Example 4, except that the zeolite filler A was not used, and the average thermal expansion coefficient thereof was measured. The results are shown in Table 3.

[0392] [Table 3]

[0393]

[0394] [Example 6] (Evaluation of injectability)

[0395] 2.4 g of epoxy resin, 3.6 g of curing agent, and 4 g of zeolite filler A were weighed and mixed in a cup in a manner as shown in Table 3. Then, a vacuum mixer (manufactured by EME, "V-mini300") was used to mix at 1500 rpm for 5 minutes to prepare a liquid composition. A gap of 6 μm was set on a glass plate, and a test piece with a glass plate fixed thereon was made to replace the semiconductor element. The test piece was placed on a heating plate set at 80°C. After confirming that the temperature of the glass plate reached 80°C, the prepared liquid composition was applied to one end of the glass plate, and the moving distance after a certain period of time was measured. This step was performed twice, and the average value of the measured values ​​was taken as the measured value of the moving distance.

[0396] In addition, when injecting into a narrow gap, when the particle size of the filler contained in the liquid composition is relatively large relative to the gap, sometimes the filler is left and only filled with resin. In this case, a part with more resin can be formed, so the change in the color of the liquid composition can be confirmed by naked eye observation. In this liquid resin composition, the zeolite filler is white and the resin part is transparent, so the part with more resin is close to transparent. In the case of the change in color, it can be judged that the filler cannot be filled into the gap, and in the case of no change in color, it can be judged that the filler filling into the gap has been carried out. Therefore, it was evaluated according to the following benchmark. The evaluation results are shown in Table 3.

[0397] ×: There is a color change.

[0398] ○: No color change.

[0399] [Comparative Example 6]

[0400] 2 g of epoxy resin, 3 g of curing agent, and 5 g of zeolite filler C (large particle size CHA) were weighed and mixed in a cup in a manner as shown in Table 3. Except for the mixing ratio, the same procedure as in Example 6 was carried out to obtain a liquid composition having the same viscosity as in Example 6, and the moving distance was measured. In addition, the color of the liquid composition filled in the gap was compared with the color of the liquid composition before filling to confirm whether there was a color change, and the filler filling in the gap was evaluated in the same manner as in Example 6. The evaluation results are shown in Table 3.

[0401] [Table 4]

[0402]

[0403] From the results in Table 4, it can be seen that the zeolite filler A having a small particle size has good injectability into narrow gaps.

[0404] It is expected that the miniaturization of devices and components constituting the devices will continue to advance in the future, and semiconductor chips are also expected to be miniaturized, thinned, and 3D stacked. It is believed that in such applications, it is necessary to install in a narrower gap of about 25μm or 10μm than the current narrow gap of about 50μm.

[0405] The small and spherical filler having high negative expansion characteristics as described in the present application can also cope with the above-mentioned uses.

[0406] Industrial Applicability

[0407] According to the present invention, a low-viscosity liquid composition can be provided. In addition, by solidifying the liquid composition, a resin composite material with a low thermal expansion coefficient can be provided. That is, according to the composition of the present invention, a sealing material with excellent injectability and excellent heat resistance can be obtained, which is particularly useful as a bottom filling material.

[0408] Furthermore, the resin composite material having a low thermal expansion coefficient of the present invention is also useful as a sealing material produced by press molding or the like.

Claims

1. A zeolite which is a spherical aluminosilicate having a particle size of 0.05 μm or more and less than 1.0 μm and having d6r as CBU.

2. The zeolite according to claim 1, which has a sphericity of 0.7 or more. The zeolite according to claim 2 , which is a CHA type zeolite. A composition comprising the zeolite according to claim 3 and a resin.

5. The composition according to claim 4, wherein The resin is at least one selected from epoxy resin and polyimide resin. The composition according to claim 5 , further comprising an inorganic filler having a particle size of 1.0 μm or more and 10 μm or less.

7. The composition according to claim 5, wherein The content of the zeolite according to claim 1 in the entire filler is 90 mass % or more.

8. The composition according to claim 5, wherein The content of the zeolite is 40 to 70% by mass, the resin is an epoxy resin, and the viscosity of the composition at 23° C. is greater than or equal to 0.1 Pa·s and less than or equal to 250 Pa·s.

9. A resin composite material, which is formed from the composition according to claim 5, wherein: The content of the zeolite is 40-70% by mass, the resin is an epoxy resin, and the average thermal expansion coefficient of the resin composite material at 25-100° C. is 10-30 ppm / K.

10. A liquid sealant formed from the composition according to claim 5. 11 . A sealing material formed from the resin composite material according to claim 9 . 12 . An electronic device comprising the resin composite material according to claim 9 .

13. A method for manufacturing a sealing material, the method comprising: A step of filling the gap with the composition according to claim 8 and then curing the gap.

14. A method for producing zeolite, the method comprising: The process of subjecting a raw material composition including a silicon atom raw material, a water-soluble aluminum atom raw material, an organic structure directing agent, a silane coupling agent and water to hydrothermal synthesis. 15 . The method for producing zeolite according to claim 14 , further comprising a calcining step.

Citation Information

Patent Citations

  • Under fill material for flip chip type semiconductor device, the flip chip type semiconductor device using the same and method for producing the device

    JP2007056070A

  • Adsorption heat pump, operation method for adsorption heat pump and vehicle air conditioner using adsorption heat pump

    JP2009097856A

  • Epoxy resin composition

    JP2017110146A