Product, forming method thereof and shoe comprising product
A film-based molding method addresses foam product deficiencies by ensuring one-piece formation with no pores and adjustable thickness, enhancing comfort and durability without glue brushing, thus improving wear and weather resistance.
Patent Information
- Application Number
- CN202310654705.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
Foam products face issues such as surface pores, poor physical and mechanical properties, poor hydrolysis resistance, poor weather resistance, and poor stain resistance, with traditional vacuum film absorption methods limiting film thickness adjustment and leading to creases and debonding.
A molding method involving placing a film between a bottom mold and a middle frame, tensioning the film, and then applying a fluid material on the stretched film, followed by vacuum suction and curing to form a one-piece product with adjustable thickness and no pores, without the need for glue brushing.
The method achieves products with full coverage, no pores, adjustable thickness, high comfort, and improved wear and weather resistance, preventing creases and debonding, while maintaining low overall density.
Smart Images

Figure CN119078261A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of product production, and in particular relates to a product and a molding method thereof, and shoes comprising the same. Background Art
[0002] Due to its foaming characteristics, foam products are endowed with the characteristics of light weight, low density, high comfort and high efficiency and economy. They are widely used in various fields such as sole production, cushioning parts production, automobiles, sports and furniture. At present, foam products are generally formed by one-step molding, that is, the material is placed in the mold by pouring, extrusion and spraying, and then molded and demolded at a certain temperature. However, due to the low density of foam products, there are a large number of pores on the surface, poor physical and mechanical properties, poor hydrolysis resistance, poor weather resistance and poor stain resistance, and the defects are more obvious when the foaming density is too low. The most effective way to solve the technical defects of foam products is vacuum film absorption technology, that is, a mold with vacuum absorption function is used to clamp a layer of deformable film, fixed between the bottom mold and the middle frame, and then the film is sucked into the mold cavity to fit with the bottom film of the mold, and then the foaming material is placed in the mold cavity and the mold cover is laid down to buckle the fixing parts, demolding to obtain a complete film absorption molding product, and finally trimming.
[0003] The product prepared by the above method solves the problems of surface pores, poor hydrolysis resistance and weather resistance, but it also has performance defects such as poor stain resistance, easy wrinkling, poor wear resistance, etc. The film thickness is limited to a thin film and the thickness cannot be adjusted.
[0004] CN105666908A discloses a method for film-absorbing molding of a shoe sole. First, a traditional mold is changed into a mold capable of vacuum absorption, which has a special film-absorbing function. Then, the mold is heated to 45-60 degrees through a polyurethane production line, and a mold release agent is sprayed on the mold. Then, a bottom film is placed at the bottom of the mold. Then, a TPU film is hung on the middle frame of the mold, and the middle frame covers the bottom mold so that the TPU film is sandwiched between the bottom mold and the middle frame, and a fixing piece is applied. Then, the mold with the TPU film is heated to 110-160 degrees through an ultraviolet carbon fiber lampshade to make the TPU film reach a soft melting point. Then, the soft-melted TPU film is sucked into the mold cavity and fits with the bottom film of the mold bottom. Then, foamed polyurethane is poured into the mold cavity, and the upper cover of the mold is closed and two fixing pieces are buckled. The completed mold is passed through an oven provided with a polyurethane production line at a temperature of 80-100°C, and is taken out of the oven in 5-7 minutes. The mold is opened to take out the complete film-absorbing molding sole, and finally trimming is performed. The sole obtained by the molding method provided in this application only includes a polyurethane foam layer and a polyurethane film coated on the outer surface of the foam layer. In order to ensure the support of the shoe, the density of the foam layer is required to be relatively high, which reduces the comfort of the shoe to a certain extent. In addition, creases will appear on the film-absorbing area after wearing for a long time, affecting the appearance.
[0005] Therefore, it is necessary to develop a new molding method so that the molded products can take into account comfort, wear resistance, long-term use without creases and weather resistance. Summary of the invention
[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a product and a molding method thereof and shoes comprising the same. The molding method can achieve one-piece molding without the need for a glue brushing process, and the product obtained by the molding method has a fully glue-coated appearance and no pores. It also has the advantages of adjustable outer wall thickness, low overall density, high comfort, high wear resistance, no creases after long-term use, and not easy to debond.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for forming a product, the method comprising the following steps:
[0009] (1) Place the film on the bottom mold and fix it between the bottom mold and the middle frame;
[0010] (2) tightening the film fixed between the bottom mold and the middle frame;
[0011] (3) placing the outer skin material on the taut film, sucking the film, making the film concave toward the bottom mold, performing the first curing and molding, and demolding to obtain the product.
[0012] The molding method provided by the present invention includes three steps. First, a film is placed on a bottom mold and fixed between the bottom mold and a middle frame; then, the film fixed between the bottom mold and the middle frame is subjected to a tensioning treatment. The tensioning treatment ensures that the film fixed between the bottom mold and the middle frame is in a "wrinkle-free" state when suspended in the air, so that when the subsequent fluid material (outer skin material) is placed on it, it can be ensured that no bubbles are generated during the flow process, and the problem of uneven flow caused by wrinkles is avoided, so that the fluid can be spread on the film paper more quickly and evenly and ensure that there are no bubbles, thereby greatly improving the yield rate. Finally, the outer skin material is placed on the tight film and the film is sucked. Since the film is concave inward toward the bottom mold, The outer skin material will flow as the shape of the film changes, forming a thinner layer of outer skin material in the concave part of the film, and then solidifying and forming to obtain the product; the entire molding process is one-piece molding, and no glue brushing process is required, thereby effectively avoiding the risk of product debonding; at the same time, the molding method provided by the present invention can adjust the thickness of the outer skin through the amount and viscosity of the material, can adapt to different product shapes, and the overall product can be used for a long time without creases; in addition, according to the needs of different products, the molding method provided by the present invention can also place the liner material on the molded outer skin, and then solidify the liner material into shape. It is also one-piece molding, no glue brushing is required, and still has the advantage of avoiding debonding.
[0013] In summary, the products prepared by the molding method provided by the present invention break through the technical bottlenecks of traditional foam products such as pores, high density, poor weather resistance and hydrolysis resistance, and achieve one-piece molding, full coverage of the appearance, no pores, adjustable thickness, and low overall product density. It also effectively improves its weather resistance, wear resistance and hydrolysis resistance, and can be applied to the molding of a variety of products.
[0014] Preferably, the film is a deformable elastic film, further preferably any one of a thermoplastic organic film, a thermosetting organic film or a photocurable organic film, and further preferably any one of an ethylene-vinyl acetate copolymer film, a silicone film, a polyvinyl chloride film (PVC), a polyethylene film (PE), a rubber film, a thermoplastic polyurethane film or a thermosetting polyurethane film, or a combination of at least two thereof.
[0015] Preferably, before placing the film on the bottom mold in step (1), the step also includes heating the bottom mold to 45-85°C (for example, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 61°C, 64°C, 68°C, 74°C, 75°C, 77°C, 80°C, 81°C, 83°C or 84°C, etc.).
[0016] Preferably, after placing the film on the bottom mold in step (1), the step further includes coating a surface treatment agent on the surface of the film.
[0017] Preferably, the surface treatment agent includes a film anti-adhesive agent, the main function of which is to improve the peelability between the outer skin and the film.
[0018] Preferably, the film anti-adhesion agent includes any one of a water-based release agent, an oily release agent or a silicone oil auxiliary agent, or a combination of at least two of them.
[0019] Preferably, the tensioning treatment method in step (2) includes: applying pressure or baking the film fixed between the bottom mold and the middle frame.
[0020] Preferably, the pressure-applying method includes applying positive pressure to make the film half-bulge, or applying negative pressure to make the film half-sucked.
[0021] Preferably, the baking temperature is not less than 120°C, for example, 215°C, 210°C, 195°C, 185°C, 175°C, 16590°C, 155°C, 145°C, 135°C or 125°C, etc.
[0022] In the forming method provided by the present invention, if the film is made taut by applying pressure, the pressure applying method includes applying positive pressure or applying negative pressure, that is, using positive pressure or negative pressure to make the film bulge to form a semi-bulging state or concave to form a semi-suctioned state, the strength of the positive pressure or negative pressure should not be too large, and the film can be made taut without wrinkles. Too large a strength will cause the film to deform excessively in advance, and there will be a risk of rupture when the film is sucked later; if baking is adopted, it is preferably baked with a baking lamp ≥120°C (the baking lamp needs to keep a certain distance from the film, and the baking lamp needs to be moved continuously during the baking process to ensure that the film is evenly heated and will not cause the film paper to rupture due to excessive temperature). Baking mainly utilizes the thermal expansion of the air in the sealed space below the film and the thermal softening and deformation of the film to make the film taut.
[0023] Preferably, step (3) further includes the step of heating the stretched film to 70-120°C, for example, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C or 115°C, etc. before placing the outer skin material on the stretched film; the purpose of heating the film is to make the film reach a soft melting point, which is conducive to subsequent film absorption.
[0024] Preferably, the heating method comprises using an infrared carbon fiber lampshade to heat the stretched film.
[0025] Preferably, the method of placing the outer skin material on the taut film in step (3) comprises any one of casting, extrusion, spraying, brushing, scraping, blow molding or pressing, or a combination of at least two thereof.
[0026] Preferably, the outer skin material comprises any one of a thermosetting organic material, a photocurable organic material or a thermoplastic organic material, or a combination of at least two thereof.
[0027] Preferably, the melt viscosity of the outer skin material at 20-45° C. is 1000-5000 mPa·s, for example, 1500 mPa·s, 2000 mPa·s, 2500 mPa·s, 3000 mPa·s, 3500 mPa·s, 4000 mPa·s, 4500 mPa·s or 5000 mPa·s.
[0028] As a preferred technical solution of the present invention, when the viscosity of the outer skin material is within the above range, the outer skin material can obtain the best wall hanging effect. If the viscosity of the outer skin material is too high, the wall thickness of the outer skin material after molding will be too large, and the overall density of the product will be high; if the viscosity of the outer skin material is too low, the wall thickness of the outer skin will be too small or discontinuous, and the inner liner will not be well protected, affecting the comprehensive performance and appearance of the product.
[0029] Preferably, the density of the outer skin material is 0.8-1.5 g / cm 3 , for example 0.9g / cm 3 , 1g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 or 1.4 g / cm 3 wait.
[0030] Preferably, the vacuum degree of the film suction in step (3) is -0.1 to 0.05 MPa, such as 0 MPa, -0.02 MPa, -0.004 MPa, -0.005 MPa, -0.008 MPa or -0.009 MPa.
[0031] It should be noted that the vacuum degree mentioned in the present invention refers to the vacuum degree of the space formed between the film and the bottom mold.
[0032] As a preferred technical solution of the present invention, the present invention controls the vacuum degree of the film absorption process within the above-mentioned specific range. Within this range, the outer skin material can form the best wall hanging effect on the film wall. If the film absorption vacuum degree is too low, the wall hanging is not obvious, the wall thickness of the outer wall is small, and the comprehensive performance and appearance of the product are poor. If the film absorption vacuum degree is too high, the outer skin material hangs on the wall too much and the product density is high.
[0033] Preferably, the film suction method in step (3) specifically includes: extracting the air between the taut film and the bottom mold so that the film fits the bottom of the bottom mold.
[0034] Preferably, the method for extracting the air between the taut film and the bottom mold specifically includes: connecting at least two exhaust holes at the sharp corners of the texture of the bottom mold, each of the exhaust holes is connected to the vacuum system by air, and then starting the vacuum system to extract the air between the bottom mold and the film.
[0035] Preferably, step (3) further includes a dwelling step before the first solidification molding.
[0036] Preferably, the residence time is 0 to 5 minutes and is not equal to 0, for example, 1 minute, 2 minutes, 3 minutes or 4 minutes.
[0037] As a preferred technical solution of the present invention, a step of staying for 2 to 5 minutes is also included before the first curing molding to leave a certain flow time for the outer skin material, so that the outer skin material can form the best wall hanging effect on the film wall and ensure that the bottom outer skin material has good uniformity. If the residence time is too long, the wall hanging is not obvious, the wall thickness of the outer wall is small, the wear resistance and service life of the product are deteriorated, and the production efficiency is reduced; if the residence time is too short, the outer skin material hangs too much on the wall, the product density is high and the leveling uniformity is poor.
[0038] Preferably, the temperature of the first curing molding in step (3) is 45-85°C, for example, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 61°C, 64°C, 68°C, 74°C, 75°C, 77°C, 80°C, 81°C, 83°C or 84°C, etc.
[0039] Preferably, the time for the first curing molding in step (3) is 2 to 10 minutes, for example, 2.1 minutes, 2.4 minutes, 2.6 minutes, 2.8 minutes, 3 minutes, 3.2 minutes, 3.6 minutes, 4.0 minutes, 4.2 minutes, 4.5 minutes, 4.8 minutes, 6 minutes, 7 minutes, 8 minutes or 9 minutes.
[0040] Preferably, the step (3) specifically comprises: heating the taut film to 70-120° C., pouring the outer skin material on the taut film, sucking the film so that the film is attached to the bottom of the bottom mold, staying for 0-5 minutes, and then performing the first curing molding at 45-85° C. for 2-10 minutes to obtain a molded outer skin.
[0041] Preferably, after the first curing and molding in step (3), the step further includes placing an inner liner material on the molded outer skin and performing a second curing and molding step.
[0042] Preferably, after inserting the liner material, the step of closing the bottom mold is also included.
[0043] Preferably, the liner material includes any one of a thermosetting organic material, a photocurable organic material, a thermoplastic organic material or a rubber material, or a combination of at least two of them.
[0044] Preferably, the density of the liner material is 0.15-0.95 g / cm 3 , for example 0.2g / cm 3 , 0.25g / cm 3 , 0.3g / cm 3 , 0.35g / cm 3 , 0.4g / cm 3, 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 , 0.8g / cm 3 or 0.9g / cm 3 wait.
[0045] Preferably, the temperature of the second curing molding is 45-65°C, for example, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 61°C or 64°C, etc.
[0046] Preferably, the second curing molding time is 2 to 6 minutes, for example, 2.2 minutes, 2.4 minutes, 2.6 minutes, 2.8 minutes, 3 minutes, 3.2 minutes, 3.4 minutes, 3.6 minutes, 3.8 minutes, 4 minutes, 4.5 minutes, 5 minutes or 5.5 minutes.
[0047] Preferably, after step (3) is completed, the process also includes trimming and finishing the demoulded product, and packaging and warehousing the product after passing the inspection.
[0048] Preferably, the molding method comprises the following steps:
[0049] (1) heating the bottom mold to 45-85° C., placing the film on the bottom mold, fixing it between the bottom mold and the middle frame, and optionally applying a surface treatment agent on the surface of the film;
[0050] (2) Pressing or baking the film fixed between the bottom mold and the middle frame to tighten the film fixed between the bottom mold and the middle frame;
[0051] (3) heating the stretched film to 70-120° C., pouring the outer skin material on the stretched film, sucking the film, making the film concave inward toward the bottom mold and fitting with the bottom of the bottom mold, leaving it for 0-5 minutes, and then performing a first curing molding at 45-85° C. for 2-10 minutes to form the outer skin, pouring the liner material on the formed outer skin, closing the bottom mold, and performing a second curing molding at 45-65° C. for 2-6 minutes to obtain a formed liner, cooling, demolding, and optionally peeling off the film to obtain the product;
[0052] (4) Trim and tidy up the demoulding products, and pack and store them after passing the inspection.
[0053] In a second aspect, the present invention provides a product, which is prepared by the molding method described in the first aspect.
[0054] In a third aspect, the present invention provides a shoe, comprising the product according to the first aspect.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] The molding method provided by the present invention comprises placing a film on a bottom mold so that it is fixed between the bottom mold and the middle frame; performing a tightening treatment on the film fixed between the bottom mold and the middle frame; placing an outer skin material on the tightened film, sucking the film, making the film concave in the direction of the bottom mold, performing a first curing molding, and demolding to obtain the product; the molding method breaks through the technical bottlenecks of pores and high density of traditional foam products, and realizes one-piece molding, full rubber coating on the appearance, no pores, adjustable thickness, and low overall product density; in addition, the outer skin of the side of the product obtained by the molding method provided by the present invention is thinner, and the outer skin of the bottom is thicker. This structure can improve the overall performance of the product, and even when the density of the liner material is low, it still has high performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 A physical picture of the non-porous sole provided in Example 1;
[0058] Figure 2 A physical picture of a non-porous sole provided in Example 4;
[0059] Figure 3 A physical picture of the sole provided in Example 1;
[0060] Figure 4 A physical picture of the sole provided for Comparative Example 2;
[0061] Figure 5 This is a physical picture of the sole provided for Comparative Example 3. DETAILED DESCRIPTION
[0062] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0063] The test information involved in the specific implementation of the present invention is as follows:
[0064] Density: Test according to the test method provided in GB / T 533-2008;
[0065] Folding resistance: Tested in accordance with the test method provided in GB / T 3903.1-2008;
[0066] Yield rate: Prepare 100 parallel samples according to the molding method. If the samples do not have any problems such as air holding, dark bubbles, and inner liner leakage, they are good products. Yield rate = number of good products / 100×100%.
[0067] Example 1
[0068] A method for forming a non-porous sole specifically comprises the following steps:
[0069] (1) The bottom mold is heated to 55° C., a mold release agent (Silok 3236A2) is sprayed, a fully transparent thermoplastic polyurethane film (purchased from Huafeng Thermoplastic Polyurethane Co., Ltd., product number 3385A-1) is placed on the bottom mold, fixed between the bottom mold and the middle frame, and a surface treatment agent (purchased from Shanghai Maitu Co., Ltd., product number DC-193) is evenly coated on the film;
[0070] (2) applying positive pressure to the film fixed between the bottom mold and the middle frame, so that the film is half bulged and in a taut state;
[0071] (3) After the taut film is heated to 90° C. by irradiation with an infrared carbon fiber lampshade, a foamed polyurethane (purchased from Zhejiang Huafeng New Materials Co., Ltd., product number JF-I-6322T / JF-P-6333) is poured on the film, and the film is left for 0.5 min to allow the foamed polyurethane to cover the entire surface of the film. The film is sucked (the vacuum degree is -0.05 MPa) to fit the film to the bottom of the bottom mold, the bottom mold is closed, and then heat-molded at 60° C. for 3 min. The heat-molded sole is taken out to obtain the pore-free sole;
[0072] (4) Trim and arrange the soles without air holes, and pack them for storage after passing the inspection.
[0073] The non-porous sole obtained by the above-mentioned molding method is as follows Figure 1 As shown, from Figure 1 It can be seen that the surface of the non-porous sole obtained by the molding method provided in Example 1 is dense, non-porous, and the surface does not peel off. The density of the sole is 0.2g / cm 3 It has passed the -25℃ (5mm) punching and folding resistance test for 50,000 times. The probability of air holding and dark bubbles in the finished product is significantly reduced (the outer film used is transparent, so it can be seen that there are no dark bubbles). The continuous production yield is 98%, and there are no creases when worn.
[0074] Example 2
[0075] A method for forming a pore-free sole, which differs from Example 1 only in that step (2) is adjusted to apply negative pressure to a film fixed between a bottom mold and a middle frame so that the film is semi-concave and in a taut state, and other steps and parameters are the same as those in Example 1.
[0076] The surface of the non-porous sole obtained by the molding method provided in Example 2 is dense, non-porous, and does not peel off. The density of the sole is 0.23g / cm 3 It has passed the -25℃ (5mm) punching and folding resistance test for 50,000 times. The probability of air holding and dark bubbles in the finished product is significantly reduced, the continuous production yield rate is 96%, and there are no creases when wearing.
[0077] Example 3
[0078] A method for forming a pore-free sole, which differs from Example 1 only in that step (2) is adjusted to use a baking lamp at 125° C. to bake the film so that the film is in a taut state, and other steps and parameters are the same as those in Example 1.
[0079] The surface of the non-porous sole obtained by the molding method provided in Example 3 is dense, non-porous, and does not peel off. The density of the sole is 0.5g / cm 3 It has passed the -25℃ (5mm) punching and folding test for 50,000 times, and has no creases when worn. After baking, the film paper is softer and the texture is clearer after adsorption. The probability of air holding and dark bubbles in the finished product is significantly reduced. The continuous production yield rate is 97%, and there are no creases when worn.
[0080] Example 4
[0081] A sole forming method specifically comprises the following steps:
[0082] (1) The bottom mold is heated to 55° C., a mold release agent (Silok 3236A2) is sprayed, a thermoplastic polyurethane film (purchased from Huafeng Thermoplastic Polyurethane Co., Ltd., product number 3385A) is placed on the bottom mold, fixed between the bottom mold and the middle frame, and a treatment agent (purchased from Shanghai Maitu Co., Ltd., product number DC-193) is evenly coated on the film;
[0083] (2) applying positive pressure to the film fixed between the bottom mold and the middle frame, so that the film is half bulged and in a taut state;
[0084] (3) After the taut film is heated to 90° C. by irradiation with an infrared carbon fiber lampshade, thermosetting polyurethane (purchased from Huafeng New Materials Co., Ltd., product number JF-I-600 / JF-P-500, viscosity at 40° C. is poured on the film, and the film is sucked (vacuum degree is -0.05 MPa) to make the film fit with the bottom of the bottom mold, stay for 1 minute, and then perform the first heating molding at 60° C. for 3 minutes to obtain a molded outer skin;
[0085] (4) pouring foamed polyurethane (purchased from Huafeng New Materials Co., Ltd., product number JF-I-6322T / JF-P-6333) on the molded outer skin, closing the bottom mold, performing a second heating molding at 50° C. for 3 min to obtain a molded liner, cooling, demolding and tearing off the film to obtain the sole;
[0086] (5) Trim and tidy up the demoulding products, and pack and store them after passing the inspection.
[0087] The sole obtained by the above molding method is as follows Figure 2 As shown, from Figure 2 It can be seen that the sole surface obtained by the molding method provided in Example 4 is dense, has no pores, and does not peel off. The density of the sole outer skin is 1.14g / cm 3 The density of the liner is 0.33g / cm 3 It has passed the test of -25℃ (5mm) punching and folding resistance for 50,000 times. The outer liner evenly wraps the inner liner material, there is no leakage of the inner liner, the yield rate is 97%, and there are no creases when worn. This shows that when the mold is more complicated, the overall foaming effect of the molding method provided by the present invention is better, and the coating uniformity of the outer skin material is also better.
[0088] Example 5
[0089] A method for forming a sole, which differs from Example 4 only in that step (2) is adjusted to apply negative pressure to a film fixed between a bottom mold and a middle frame so that the film is semi-concave and in a taut state, and other steps and parameters are the same as those of Example 4.
[0090] The sole surface obtained by the molding method provided in Example 5 is dense, has no pores, and does not peel off. The density of the sole outer skin is 1.17g / cm 3 The density of the liner is 0.4g / cm 3 It has passed the -25℃ (5mm) punching and folding resistance test of 50,000 times. The outer liner evenly wraps the inner liner material, there is no leakage of the inner liner, the yield rate is 98%, and there are no creases when wearing.
[0091] Example 6
[0092] A method for forming a sole, which differs from Example 4 only in that step (2) is adjusted to use a baking lamp at 125° C. to bake the film so that the film is in a taut state, and the other steps and parameters are the same as those in Example 4.
[0093] The sole surface obtained by the molding method provided in Example 6 is dense, has no pores, and does not peel off. The density of the sole outer skin is 1.17g / cm 3 The density of the liner is 0.35g / cm 3It has passed the -25℃ (5mm) punching and folding resistance test of 50,000 times. The outer liner evenly wraps the inner liner material, there is no leakage of the inner liner, the yield rate is 97%, and there are no creases when wearing.
[0094] Example 7
[0095] A method for forming a bicycle saddle comprises the following steps:
[0096] (1) Heat the bottom mold to 55° C., spray a mold release agent (Silok 3236A2), place a thermoplastic polyurethane film (purchased from Huafeng Thermoplastic Polyurethane Co., Ltd., product number 3385A) on the bottom mold, and fix it between the bottom mold and the middle frame;
[0097] (2) applying positive pressure to the film fixed between the bottom mold and the middle frame, so that the film is half bulged and in a taut state;
[0098] (3) After the film is irradiated with an infrared carbon fiber lampshade to heat the film to 110° C., thermosetting polyurethane (Huafeng self-made material JF-I-600T / JF-P-500T, with a viscosity of 2800 mPa·s at 40° C.) is cast on the film, and the film is sucked (the vacuum degree is −0.08 MPa) to make the film fit the bottom of the bottom mold, stay for 1 minute, and then perform the first heating molding at 80° C. for 4 minutes to obtain the outer skin of the outer sole;
[0099] (4) casting and pouring foamed polyurethane (purchased from Huafeng New Materials Co., Ltd., product number JF-I-9818 / JF-P-4170) on the outer skin of the outer sole, closing the bottom mold, and performing a second heating molding at 60° C. for 4 minutes to obtain a midsole liner, and demolding to obtain the bicycle saddle product;
[0100] (5) trimming and arranging the demoulded bicycle saddle, and packing and storing it after passing the inspection.
[0101] The density of the outer skin of the bicycle saddle product obtained by the above molding method is 1.1g / cm 3 The density of the midsole liner is 0.32g / cm 3 The overall density is low, it is comfortable and soft, with no pores on the surface. The dense outer layer provides the product with excellent weather resistance, stain resistance and hydrolysis resistance, and the yield rate is 94%.
[0102] Example 8
[0103] A method for molding a sole, which differs from Example 1 only in that step (3) specifically comprises: after the taut film is heated to 90° C. by irradiation with an infrared carbon fiber lampshade, pouring foamed polyurethane (purchased from Zhejiang Huafeng New Materials Co., Ltd., product number JF-I-6322T / JF-P-6333) on the film, sucking the film to make the film fit with the bottom of the bottom mold, closing the bottom mold, and then heating and molding at 60° C. for 3 minutes, taking out the sole obtained by heating and molding, and obtaining the sole.
[0104] The pore-free sole obtained by the molding method provided in Example 8 passed the test of -25°C (5mm) perforation and folding resistance for 50,000 times, but because it absorbed the film without stopping, the foamed polyurethane was not evenly spread, and the foaming was not synchronized after absorption. The probability of defects such as air holding and dark bubbles in the finished product was greatly increased. The yield rate was 85%, and there were no creases when worn.
[0105] Comparative Example 1
[0106] A method for forming a sole, comprising the following steps:
[0107] (1) The bottom mold is heated to 55° C., a mold release agent (Silok 3236A2) is sprayed, an opaque thermoplastic polyurethane film (purchased from Huafeng Thermoplastic Polyurethane Co., Ltd., product number 3385A) is placed on the bottom mold, fixed between the bottom mold and the middle frame, and a surface treatment agent (purchased from Shanghai Maitu Co., Ltd., product number DC-193) is evenly coated on the film;
[0108] (2) After the film is heated to 90° C. by irradiation with an infrared carbon fiber lampshade, a foamed polyurethane (purchased from Zhejiang Huafeng New Materials Co., Ltd., product number JF-I-6322T / JF-P-6333) is poured on the film, and the film is left for 0.5 min to allow the foamed polyurethane to cover the entire surface of the film. The film is sucked (the vacuum degree is -0.05 MPa) to make the film fit the bottom of the bottom mold, the bottom mold is closed, and then heat-molded at 60° C. for 3 min, and the sole obtained by heat molding is taken out to obtain the sole;
[0109] (3) Trim and tidy up the soles, and pack and store them after passing inspection.
[0110] The sole obtained by the molding method provided in Comparative Example 1 is as follows Figure 3 As shown, its density is 0.2g / cm 3It has passed the -25℃ (5mm) punching and folding resistance test for 50,000 times, and has no creases when worn. However, since it has not been tightened, the foamed polyurethane is not evenly spread, resulting in asynchronous foaming after downward absorption. After multiple parallel proofing, the probability of some finished products having defects such as air holding and dark bubbles has greatly increased, and the yield rate is only 70%. However, since the thermoplastic polyurethane film used in its outer skin material is opaque, it is difficult to directly observe the dark bubbles from the picture alone.
[0111] Comparative Example 2
[0112] A method for forming a sole, which differs from Comparative Example 1 only in that a fully transparent polyurethane thermoplastic polyurethane film (purchased from Huafeng Thermoplastic Polyurethane Co., Ltd., product number 3385A-1) is used to replace the opaque thermoplastic polyurethane film in Comparative Example 1 as the outer material, and other materials and steps are the same as those in Comparative Example 1.
[0113] The sole obtained by the molding method provided in Comparative Example 2 is as follows Figure 4 As shown, from Figure 4 It can be clearly seen that the finished product obtained by the molding method provided in Comparative Example 2 has air holding and dark bubbles.
[0114] Comparative Example 3
[0115] A sole forming method specifically comprises the following steps:
[0116] (1) The bottom mold is heated to 55° C., a mold release agent (Silok 3236A2) is sprayed, a thermoplastic polyurethane film (purchased from Huafeng Thermoplastic Polyurethane Co., Ltd., product number 3385A) is placed on the bottom mold, fixed between the bottom mold and the middle frame, and a treatment agent (purchased from Shanghai Maitu Co., Ltd., product number DC-193) is evenly coated on the film;
[0117] (2) pouring thermosetting polyurethane (purchased from Huafeng New Materials Co., Ltd., product number JF-I-600 / JF-P-500, viscosity at 40°C is 3200 mPa·s) on the film, sucking the film (vacuum degree is -0.05 MPa) to make the film fit with the bottom of the bottom mold, leaving it for 1 minute, and then performing the first heating molding at 60°C for 3 minutes to obtain a molded outer skin;
[0118] (3) pouring foamed polyurethane (purchased from Huafeng New Materials Co., Ltd., product number JF-I-6322T / JF-P-6333) on the molded outer skin, closing the bottom mold, performing a second heating molding at 50° C. for 3 min to obtain a molded liner, cooling, demolding and tearing off the film to obtain the sole;
[0119] (4) Trim and tidy up the demoulding products, and pack and store them after passing the inspection.
[0120] The sole obtained by the molding method provided in Comparative Example 3 is as follows Figure 5 As shown, the density of the outer skin is 1.1 g / cm 3 The density of the liner is 0.32g / cm 3 It has passed the -25℃ (5mm) punching and folding resistance test of 50,000 times, and there are no creases when worn. However, after multiple parallel proofing, some finished products have uneven shells and missing materials, and the inner liner is exposed in some parts. The foaming uniformity is worse than that of the embodiment, the defective rate is high, and the good rate is only 72%.
[0121] The applicant declares that the present invention uses the above embodiments to illustrate a product and a molding method thereof and shoes containing the same, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for forming a product, characterized in that: The molding method comprises the following steps: (1) Place the film on the bottom mold and fix it between the bottom mold and the middle frame; (2) tightening the film fixed between the bottom mold and the middle frame; (3) placing the outer skin material on the taut film, sucking the film, making the film concave toward the bottom mold, performing the first curing and molding, and demolding to obtain the product.
2. The molding method according to claim 1, characterized in that: The film is a deformable elastic film, preferably any one of a thermoplastic organic film, a thermosetting organic film or a photocurable organic film, and more preferably any one of an ethylene-vinyl acetate copolymer film, a silicone film, a polyvinyl chloride film, a polyethylene film, a rubber film, a thermoplastic polyurethane film or a thermosetting polyurethane film, or a combination of at least two thereof; Preferably, before placing the film on the bottom mold in step (1), the step further includes heating the bottom mold to 45-85° C.; Preferably, after placing the film on the bottom mold in step (1), the step further includes coating a surface treatment agent on the surface of the film; Preferably, the surface treatment agent comprises a film anti-adhesive agent; Preferably, the film anti-adhesion agent includes any one of a water-based release agent, an oily release agent or a silicone oil auxiliary agent, or a combination of at least two of them.
3. The molding method according to claim 1 or 2, characterized in that: The method of tightening treatment in step (2) includes: applying pressure or baking the film fixed between the bottom mold and the middle frame; Preferably, the pressure application method includes applying positive pressure to make the film half bulge, or applying negative pressure to make the film half suck down; Preferably, the baking temperature is not less than 120°C.
4. The molding method according to any one of claims 1 to 3, characterized in that: Step (3) also includes heating the stretched film to 70-120° C. before placing the outer skin material on the stretched film; Preferably, the heating method comprises irradiating the stretched film with an infrared carbon fiber lampshade; Preferably, the method of inserting the outer skin material in step (3) comprises: any one or a combination of at least two of casting, extrusion, spraying, brushing, scraping, blow molding or pressing; Preferably, the outer skin material comprises any one or a combination of at least two of a thermosetting organic material, a photocurable organic material or a thermoplastic organic material; Preferably, the melt viscosity of the outer skin material at 20 to 45° C. is 1000 to 5000 mPa·s; Preferably, the density of the outer skin material is 0.8-1.5 g / cm 3 .
5. The molding method according to any one of claims 1 to 4, characterized in that: The vacuum degree of the film suction in step (3) is -0.1 to 0.05 MPa; Preferably, the film suction method in step (3) specifically includes: extracting the air between the tight film and the bottom mold so that the film fits the bottom of the bottom mold; Preferably, the method for extracting the air between the taut film and the bottom mold specifically includes: connecting at least two exhaust holes at the sharp corners of the texture of the bottom mold, each of the exhaust holes is connected to the vacuum system by air, and then starting the vacuum system to extract the air between the bottom mold and the film.
6. The molding method according to any one of claims 1 to 5, characterized in that: Step (3) also includes a stop step before the first curing and molding; Preferably, the dwell time is 0 to 5 minutes and is not equal to 0; Preferably, the temperature of the first curing molding in step (3) is 45-85°C; Preferably, the first curing time in step (3) is 2 to 10 minutes.
7. The molding method according to any one of claims 1 to 6, characterized in that: Step (3) after the first curing and molding, further includes placing an inner liner material on the molded outer skin and performing a second curing and molding step; Preferably, the liner material includes any one or a combination of at least two of a thermosetting organic material, a light-curing organic material, a thermoplastic organic material or a rubber material; Preferably, the density of the liner material is 0.15-0.95 g / cm 3 ; Preferably, the temperature of the second curing molding is 45-65°C; Preferably, the second curing molding time is 2 to 6 minutes.
8. The molding method according to claim 7, characterized in that: After step (3) is completed, the steps of trimming and finishing the demoulded product and packaging and warehousing the product after passing the inspection are also included; Preferably, the molding method comprises the following steps: (1) heating the bottom mold to 45-85° C., placing the film on the bottom mold, fixing it between the bottom mold and the middle frame, and optionally applying a surface treatment agent on the surface of the film; (2) applying pressure or baking the film fixed between the bottom mold and the middle frame to tighten the film fixed between the bottom mold and the middle frame; (3) pouring the outer skin material on the taut film, sucking the film, making the film concave inward toward the bottom mold and fitting with the bottom of the bottom mold, leaving it for 0 to 5 minutes, and then performing the first curing molding at 45 to 85° C. for 2 to 10 minutes to form the outer skin, pouring the liner material on the formed outer skin, closing the bottom mold, and performing the second curing molding at 45 to 65° C. for 2 to 6 minutes to obtain a formed liner, cooling, demolding, and optionally peeling off the film to obtain the product; (4) Trim and tidy up the demoulding products, and pack and store them after passing the inspection.
9. A product, characterized in that The product is prepared by the molding method according to any one of claims 1 to 8.
10. A shoe, characterized in that: The shoe comprises the article of claim 9.