Water-based silk-screen UV ink for intelligent card printing and preparation method of water-based silk-screen UV ink

By using water-based polyurethane, polyurethane modified acrylic copolymer, photoinitiator, defoaming agent and modified polyol in water-based silk-printing UV ink, the wear resistance, antibacterial and antioxidant properties of the ink are improved, and the wear resistance, antibacterial and antioxidant properties are solved. The lack of adaptability and wear resistance in smart card printing has achieved performance demands in the high-end market, and has reduced the use of organic solvents, meeting environmental protection requirements.

CN119081471APending Publication Date: 2024-12-06HUIZHOU DESIKUN CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411459659.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In smart card printing applications, existing water-based silk screen UV inks have poor printing adaptability and wear resistance, which cannot meet the market's high-end demand for gloss, color saturation, wear resistance, adhesion, antibacterial and oxidation resistance.

Method used

Using water-based polyurethane as the base resin, polyurethane-modified acrylic copolymer is introduced to improve adhesion and hardness, photoinitiators are used to promote UV curing, defoaming agents and aqueous thickening agents are added to ensure printing stability, and by modifying polyols and Modified chitosan improves antibacterial, antioxidant and mechanical properties.

Benefits of technology

The water-based silk-print UV ink for smart card printing has excellent wear resistance, adhesion, antibacteriality, oxidation resistance and a certain degree of heat resistance. The cured ink has strong adhesion fastness and high gloss, meeting the high-end market. Demand, while reducing VOCs emissions, achieving green and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005091510020000091
    Figure BDA0005091510020000091
  • Figure BDA0005091510020000101
    Figure BDA0005091510020000101
Patent Text Reader

Abstract

The invention relates to the technical field of printing ink, in particular to water-based silk-screen UV printing ink for intelligent card printing and a preparation method of the water-based silk-screen UV printing ink. The water-based screen printing UV ink for intelligent card printing is prepared from the following preparation raw materials in parts by mass: 80 to 90 parts of water-based polyurethane, 3 to 8 parts of polyurethane modified acrylic acid copolymer, 1 to 2 parts of photoinitiator, 1 to 2 parts of defoaming agent and 0.5 to 2 parts of water-based thickening agent. The water-based screen printing UV ink for intelligent card printing has the advantages of being environmentally friendly, high in performance, high in stability and the like, is very suitable for printing of high-end intelligent cards, and meets the requirements of the modern printing industry for environment-friendly and high-performance materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of ink technology, and in particular to a water-based screen printing UV ink for smart card printing and a preparation method thereof. Background Art

[0002] Water-based UV (ultraviolet light curing) ink is a new type of environmentally friendly ink that combines the advantages of water-based ink and UV ink. It not only has low VOC emissions, low environmental pollution, and low energy consumption, but also uses ultraviolet light source for curing, has a fast drying speed, and improves production efficiency.

[0003] With the strengthening of environmental protection policies at home and abroad, environmentally friendly, non-toxic, low-odor, easy-to-operate and safe water-based screen printing UV inks have become green products with real emission reduction and energy saving effects. However, the poor printing adaptability and wear resistance of water-based screen printing UV inks are the shortcomings of water-based screen printing UV inks, especially water-based screen printing UV inks used for smart card printing. At present, they cannot meet the high market demand in terms of gloss, color saturation, wear resistance, adhesion, antibacterial and antioxidant properties. Summary of the invention

[0004] The purpose of the present application is to provide a water-based screen printing UV ink for smart card printing and a preparation method thereof in view of the deficiencies in the current technology. The water-based screen printing UV ink for smart card printing prepared in the present application does not add organic solvents, greatly reduces VOCs emissions, is green and environmentally friendly, and has excellent wear resistance, adhesion, antibacterial, antioxidant and a certain degree of heat resistance, and excellent mechanical properties. The cured ink has strong adhesion and high gloss, which can meet the needs of the high-end market.

[0005] In the first aspect, the present application provides a water-based silk-screen UV ink for smart card printing, adopting the following technical scheme: a water-based silk-screen UV ink for smart card printing, comprising the following preparation raw materials, measured by mass: 80-90 parts of water-based polyurethane, 3-8 parts of polyurethane-modified acrylic copolymer, 1-2 parts of photoinitiator, 1-2 parts of defoaming agent, and 0.5-2 parts of water-based thickener.

[0006] By adopting the above technical solutions, water-based polyurethane: as a base resin, it provides good wear resistance, antibacterial properties and flexibility. The high content of water-based polyurethane ensures the basic performance of the ink. Polyurethane modified acrylic copolymer: by introducing epoxy resin and acrylate, the adhesion, hardness and wear resistance of the ink are improved. The structure of this copolymer helps to form a cross-linked network, enhancing the mechanical properties and durability of the ink. Photoinitiator: used to initiate UV curing reaction so that the ink can be quickly cured under ultraviolet light. The selection of photoinitiator is crucial to the curing speed of the ink and the physical properties after curing. Defoamer: helps to eliminate bubbles generated during the preparation of the ink to ensure that the surface of the printed product is smooth and defect-free. Water-based thickener: used to adjust the viscosity of the ink to meet different printing needs. Appropriate viscosity can ensure the stability and transferability of the ink during the printing process. In summary, the various components in the present application are carefully selected and proportioned to produce a synergistic effect with each other, so that the final water-based silk-screen UV ink for smart card printing has excellent wear resistance, adhesion, antibacterial properties, antioxidant properties and a certain degree of heat resistance, as well as good mechanical properties and high gloss after curing, meeting the needs of the high-end market.

[0007] Preferably, the waterborne polyurethane comprises the following raw materials, by mass: 9 parts of isophorone diisocyanate, 25 parts of modified polyol, 2.5 parts of dihydroxymethylbutyric acid, 2 parts of 1.4-butanediol, 1.3 parts of potassium hydroxide, 6 parts of N-methylpyrrolidone, 3 parts of acetone, 70 parts of water, and 0.08 parts of butyltin dilaurate.

[0008] Preferably, the method for preparing the modified polyol comprises the following steps: S31. In a three-necked flask equipped with a stirring device, 23.4 g of 3,5-di-tert-butyl-4-hydroxybenzaldehyde, 15 mL of piperidine and 100 mL of toluene were mixed, the temperature was raised to 57° C., and the mixture was stirred until the solid was completely dissolved. 11.5 g of diethylenetriamine was added dropwise. After the addition was completed, the mixture was kept warm for 6 h. After the reaction was completed, the mixture was naturally cooled and distilled under reduced pressure to obtain intermediate 1. S32, in a three-necked flask equipped with a stirring device, 31.9 g of intermediate 1, 9.1 g of thioglycolic acid, 20.6 g of dicyclohexylcarbodiimide and 110 mL of toluene were mixed and stirred evenly, and reacted for 4 h in a water bath at 53° C. After the reaction was completed, the mixture was filtered and the solvent was removed by distillation under reduced pressure to obtain intermediate 2; S33, add 158.1g of intermediate 2, 1.6g of azobisisobutyronitrile, and 250mL of N,N-dimethylformamide into a three-necked flask, stir and mix evenly, then dropwise add 34.4g of tetramethyltetravinylcyclotetrasiloxane, maintain the temperature of the system at 86°C, react for 7h, after the reaction is completed, first remove part of the solvent by rotary evaporation, and then purify by column chromatography (the eluent is a mixed solvent of ethyl acetate / toluene, the volume ratio of the two is 3:4), and remove the eluent by rotary evaporation to obtain intermediate 3; S34. At room temperature, under nitrogen protection, 191.2 g of intermediate 3, 88.1 g of 4-chloro-1-butanol, 63.5 g of potassium carbonate and 500 mL of N,N-dimethylformamide were stirred and mixed evenly in a three-necked flask. The reaction temperature was controlled to 71°C. After the reaction was kept warm for 7 hours, the temperature was further increased to 80°C and kept warm for 6 hours. After the reaction was completed, it was cooled to room temperature, distilled under reduced pressure, washed with anhydrous ethanol 3 times, and dried in vacuo to obtain a modified polyol.

[0009] By adopting the above technical scheme, the prepared modified polyol contains hindered phenol, quaternary ammonium salt, Schiff base and cyclic siloxane structure, wherein the hindered phenol structure has excellent antioxidant properties, can improve the antioxidant property of the polyurethane matrix, avoid adding additional antioxidants, and affect the homogeneity of the ink; in addition, the quaternary ammonium salt structure is introduced, and the quaternary ammonium salt is a broad-spectrum bactericide, which can dissociate into quaternary ammonium salt cations containing positive charges, and its N+ ions can be adsorbed onto the cell wall of negatively charged bacteria, destroy the cell membrane, and denature the protein, hindering the replication and reproduction of DNA, thereby improving the antibacterial property of the polyurethane matrix; moreover, the introduced Schiff base structure can react with The bacterial proteins and enzymes interact with each other, which hinders the synthesis of bacterial nucleotides and amino acids, and plays a synergistic role with quaternary ammonium ions, significantly improving the antibacterial properties of the polyurethane matrix; finally, the cyclic siloxane structure contains multiple Si-O bonds with high bond energy, which can improve the heat resistance of the polyurethane matrix to a certain extent; from the structure of the modified polyol itself, it is based on cyclic siloxane as the core, and there are -OH molecular chains with a dendritic structure distributed on the sides, so that the modified polyol can directly participate in the polymerization process with isocyanate and form a cross-linked polyurethane network structure, which not only improves the mechanical properties of the polyurethane matrix, but also makes the performance of the modified polyol more long-lasting and stable. In short, the prepared modified polyol can significantly enhance the antibacterial, antioxidant and certain degree of heat resistance of the ink, and can also cross-link with polyurethane to form a network structure, which not only improves the mechanical properties of the ink, but also ensures the long-term stability of the performance; Preferably, the method for preparing the waterborne polyurethane comprises the following steps: S41. Mix isophorone diisocyanate and modified polyol in a polymerization kettle according to their mass fractions, raise the temperature to 90° C. and stir in a constant temperature water bath for 3 hours, then add butyltin dilaurate and continue stirring for 50 minutes, then when the temperature of the reaction solution is reduced to 57° C., disperse dimethylolbutyric acid in N-methylpyrrolidone and add it to the polymerization kettle reaction solution, then raise the temperature to 75° C., react for 15 minutes, add half of acetone to adjust the viscosity, then raise the temperature to 93° C. and react for 2.3 hours to obtain a waterborne polyurethane prepolymer; S42. Lower the temperature of the waterborne polyurethane prepolymer to 32°C, slowly add 1.4-butanediol to the waterborne polyurethane prepolymer, and stir and shear at high speed for 2 hours. During the stirring process, add the remaining acetone in batches to adjust the viscosity. Add water dropwise to the reaction system in batches under high-speed stirring to fully mix the water and the waterborne polyurethane prepolymer, raise the temperature of the constant temperature water bath to 65°C, then add potassium hydroxide and slow down the rotation speed. Continue the reaction for 90 minutes before discharging the material to obtain a waterborne polyurethane.

[0010] By adopting the above technical solution and introducing modified polyols, the viscosity of waterborne polyurethane is reduced, the solid content of waterborne polyurethane is effectively increased, and the dispersibility and stability of waterborne polyurethane are improved. At the same time, the hindered phenol, quaternary ammonium salt, Schiff base and cyclic siloxane structure in the modified polyols give it excellent antioxidant and antibacterial properties, which can improve the mechanical properties of the polyurethane matrix and ensure the long-term stability of the performance.

[0011] Preferably, the preparation method of the polyurethane modified acrylic copolymer comprises the following steps: S51. Add 50.9 g of isophorone diisocyanate and 0.04 g of dibutyltin dilaurate to a four-necked flask equipped with a condenser, a stirring paddle, and a thermometer, and dropwise add 25 g of polyoxypropylene glycol with a molecular weight of 1000 while stirring. Keep the mixture at 75° C. for 3 h, and take a sample to determine the NCO group content during the reaction by a toluene-di-n-butylamine back titration method. S52, then cool to 60 ° C, dissolve 3.1g of dried dimethylol propionic acid in 10g of acetone, and add dropwise to the flask, stir and react for 2h, take samples to measure the NCO group content until it is close to the theoretical value of 2%, then heat to 80 ° C, add 5.3g of epoxy resin E-44, continue to react for 4h, and measure the acid value to be 118mgKOH / g; S53, finally cooling to 60°C, adding 10.7g of hydroxyethyl acrylate and 0.4g of p-hydroxyanisole to carry out end-capping reaction for 5h to obtain a polyurethane-modified acrylic copolymer.

[0012] By adopting the above technical scheme, the prepared polyurethane modified acrylic copolymer introduces epoxy resin and acrylate into the modification of polyurethane through polymerization, and adopts a dual curing system to further thermally cure the unreacted hydroxyl and isocyanate groups, and chemically bonds between polyurethane and epoxy resin and acrylate through graft copolymerization to obtain a copolymer with a cross-linked structure. The advantages of acrylate's excellent optical properties and weather resistance, epoxy resin's good chemical resistance and low curing shrinkage are combined with polyurethane's good elasticity and excellent mechanical properties, so that the synthesized copolymer combines the advantages of acrylate, epoxy resin and polyurethane, and significantly improves the heat resistance, good adhesion, wear resistance and stable performance of water-based screen printing UV ink.

[0013] Preferably, the photoinitiator is composed of ultraviolet photoinitiator IRGACURE819, ultraviolet photoinitiator IRGACURE907 and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 5:4:2. The ultraviolet photoinitiator IRGACURE819 and ultraviolet photoinitiator IRGACURE907 are both purchased from BASF, Germany.

[0014] By adopting the above technical scheme, the role of the photoinitiator in the water-based flexographic printing ink is to trigger the photoinitiated polymerization reaction, promote the polymerization and curing of the prepolymer in the ink, and realize the curing and drying of the ink. The photoinitiator is composed of ultraviolet light initiator IRGACURE819, ultraviolet light initiator IRGACURE907 and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and the mass ratio is 5:4:2. Ultraviolet light initiators IRGACURE819 and IRGACURE907 can be excited by ultraviolet light to produce free radicals, thereby initiating the polymerization reaction of the prepolymer. 2,4,6-Trimethylbenzoyl-diphenylphosphine oxide: This is a phosphorus-based photoinitiator with high photosensitivity and thermal stability. Under ultraviolet light irradiation, it can quickly decompose to produce phosphorus free radicals, thereby initiating the polymerization reaction of the monomer or prepolymer in the ink. Compared with other photoinitiators, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide has higher photosensitivity and thermal stability, and can achieve rapid curing of ink at lower light intensity. At the same time, it also has good solubility and compatibility, and can be fully mixed with other ingredients in the ink to improve the overall performance of the ink. Therefore, the synergistic effect of the photoinitiator in water-based flexographic printing ink is to achieve rapid curing and drying of the ink through the joint action of ultraviolet light initiator and synergist, reduce energy consumption and cost, thereby improving the adhesion, wear resistance and antibacterial properties of the ink, while maintaining high gloss on the surface of the ink.

[0015] Preferably, 2-3 parts of modified chitosan are also included.

[0016] Preferably, the preparation method of the modified chitosan is as follows: after adding 3g of 3,4-dihydroxyphenylpropionic acid to 465mL of a chitosan solution with a concentration of 0.72mol / mL and a pH value of 4.8, stirring at a speed of 330r / min for 50min to obtain a mixed solution; adding 7.5g of curcumin, 2.5g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 50mL of an aqueous solution of N-hydroxysulfosuccinimide with a concentration of 2.0mmol / mL to the mixed solution, mixing evenly, adjusting the pH value to 5.3, stirring and reacting at a speed of 490r / min for 11h to obtain a prefabricated chitosan solution; dialyzing the prefabricated chitosan solution in a hydrochloric acid buffer solution with a pH value of 4.9 for 52h, then dialyzing in a PBS buffer solution and deionized water for 3h respectively, and freeze-drying to obtain the modified chitosan.

[0017] By adopting the above technical scheme, the modified chitosan prepared improves the adhesion of water-based screen printing UV ink, provides anti-aging and anti-ultraviolet protection, makes the color of water-based screen printing UV ink more stable after exposure, and improves the glossiness and antibacterial performance of water-based screen printing UV ink.

[0018] Preferably, the defoaming agent is polydimethylsiloxane; and the aqueous thickener is carboxymethyl cellulose.

[0019] In a second aspect, the present application provides a method for preparing a water-based screen printing UV ink for smart card printing, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned water-based screen printing UV ink for smart card printing, comprising the following steps: The components except the photoinitiator were mixed and stirred evenly according to the weight fractions, and then the photoinitiator was added and stirred at a stirring speed of 3000 r / min for 30 minutes to obtain a water-based screen printing UV ink for smart card printing.

[0020] In summary, the beneficial technical effects of this application are: 1. Green and environmentally friendly: Since no organic solvents are added, VOCs emissions are greatly reduced, meeting environmental protection requirements.

[0021] 2. Excellent performance: It has excellent wear resistance, adhesion, antibacterial, antioxidant and a certain degree of heat resistance. These properties enable water-based screen printing UV ink to meet the needs of the high-end market.

[0022] 3. Good mechanical properties: The cured ink has strong adhesion and high gloss, which is mainly due to the introduction of modified polyols, which not only enhances the antibacterial, antioxidant and heat resistance of the ink, but also cross-links with polyurethane to form a network structure, thereby improving the mechanical properties of the ink.

[0023] 4. Improve adhesion: By adding modified chitosan, the adhesion of water-based screen printing UV ink is improved, while providing anti-aging and UV protection, making the color of water-based screen printing UV ink more stable after exposure and improving the gloss of water-based screen printing UV ink.

[0024] 5. Improved dispersibility and stability: The introduction of modified polyols reduces the viscosity of waterborne polyurethane, effectively increases the solid content of waterborne polyurethane, and improves the dispersibility and stability of waterborne polyurethane. At the same time, the introduction of modified chitosan water allows waterborne polyurethane to form a network structure while interacting with modified chitosan, thereby effectively controlling the molecular chain structure and cross-linking degree of waterborne polyurethane.

[0025] 6. Antibacterial and antioxidant properties: The modified polyols contain hindered phenols, quaternary ammonium salts, Schiff bases and cyclic siloxane structures, which can improve the antibacterial and antioxidant properties of the ink, avoid the need to add additional antioxidants or antibacterial agents, and maintain the homogeneity of the ink. DETAILED DESCRIPTION

[0026] The embodiments of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. The ultraviolet light initiator IRGACURE819 and the ultraviolet light initiator IRGACURE907 are both purchased from BASF, Germany.

[0027] In the following examples, preparation examples and comparative preparation examples, 1 part means 100 g.

[0028] Preparation Example 1 Preparation of modified polyol The preparation method of modified polyol comprises the following steps: S31. In a three-necked flask equipped with a stirring device, 23.4 g of 3,5-di-tert-butyl-4-hydroxybenzaldehyde, 15 mL of piperidine and 100 mL of toluene were mixed, the temperature was raised to 57° C., and the mixture was stirred until the solid was completely dissolved. 11.5 g of diethylenetriamine was added dropwise. After the addition was completed, the mixture was kept warm for 6 h. After the reaction was completed, the mixture was naturally cooled and distilled under reduced pressure to obtain intermediate 1. S32, in a three-necked flask equipped with a stirring device, 31.9 g of intermediate 1, 9.1 g of thioglycolic acid, 20.6 g of dicyclohexylcarbodiimide and 110 mL of toluene were mixed and stirred evenly, and reacted for 4 h in a water bath at 53° C. After the reaction was completed, the mixture was filtered and the solvent was removed by distillation under reduced pressure to obtain intermediate 2; S33, add 158.1g of intermediate 2, 1.6g of azobisisobutyronitrile, and 250mL of N,N-dimethylformamide into a three-necked flask, stir and mix evenly, then dropwise add 34.4g of tetramethyltetravinylcyclotetrasiloxane, maintain the temperature of the system at 86°C, react for 7h, after the reaction is completed, first remove part of the solvent by rotary evaporation, and then purify by column chromatography (the eluent is a mixed solvent of ethyl acetate / toluene, the volume ratio of the two is 3:4), and remove the eluent by rotary evaporation to obtain intermediate 3; S34. At room temperature, under nitrogen protection, 191.2 g of intermediate 3, 88.1 g of 4-chloro-1-butanol, 63.5 g of potassium carbonate and 500 mL of N,N-dimethylformamide were stirred and mixed evenly in a three-necked flask. The reaction temperature was controlled to 71°C. After the reaction was kept warm for 7 hours, the temperature was further increased to 80°C and kept warm for 6 hours. After the reaction was completed, it was cooled to room temperature, distilled under reduced pressure, washed with anhydrous ethanol 3 times, and dried in vacuo to obtain a modified polyol.

[0029] Preparation Example 2 Preparation of waterborne polyurethane The waterborne polyurethane comprises the following raw materials, measured by mass: 9 parts of isophorone diisocyanate, 25 parts of modified polyol, 2.5 parts of dihydroxymethylbutyric acid, 2 parts of 1.4-butanediol, 1.3 parts of potassium hydroxide, 6 parts of N-methylpyrrolidone, 3 parts of acetone, 70 parts of water, and 0.08 parts of butyltin dilaurate; the modified polyol is prepared in Preparation Example 1.

[0030] The preparation method of the waterborne polyurethane comprises the following steps: S41. Mix isophorone diisocyanate and modified polyol in a polymerization kettle according to their mass fractions, raise the temperature to 90° C. and stir in a constant temperature water bath for 3 hours, then add butyltin dilaurate and continue stirring for 50 minutes, then when the temperature of the reaction solution is reduced to 57° C., disperse dimethylolbutyric acid in N-methylpyrrolidone and add it to the polymerization kettle reaction solution, then raise the temperature to 75° C., react for 15 minutes, add half of acetone to adjust the viscosity, then raise the temperature to 93° C. and react for 2.3 hours to obtain a waterborne polyurethane prepolymer; S42. Lower the temperature of the waterborne polyurethane prepolymer to 32°C, slowly add 1.4-butanediol to the waterborne polyurethane prepolymer, and stir and shear at high speed for 2 hours. During the stirring process, add the remaining acetone in batches to adjust the viscosity. Add water dropwise to the reaction system in batches under high-speed stirring to fully mix the water and the waterborne polyurethane prepolymer, raise the temperature of the constant temperature water bath to 65°C, then add potassium hydroxide and slow down the rotation speed. Continue the reaction for 90 minutes before discharging the material to obtain a waterborne polyurethane.

[0031] Preparation Example 3 Preparation of polyurethane modified acrylic copolymer The preparation method of polyurethane modified acrylic copolymer comprises the following steps: S51. Add 50.9 g of isophorone diisocyanate and 0.04 g of dibutyltin dilaurate to a four-necked flask equipped with a condenser, a stirring paddle, and a thermometer, and dropwise add 25 g of polyoxypropylene glycol with a molecular weight of 1000 while stirring. Keep the mixture at 75° C. for 3 h, and take a sample to determine the NCO group content during the reaction by a toluene-di-n-butylamine back titration method. S52, then cool to 60 ° C, dissolve 3.1g of dried dimethylol propionic acid in 10g of acetone, and add dropwise to the flask, stir and react for 2h, take samples to measure the NCO group content until it is close to the theoretical value of 2%, then heat to 80 ° C, add 5.3g of epoxy resin E-44, continue to react for 4h, and measure the acid value to be 118mgKOH / g; S53, finally cooling to 60°C, adding 10.7g of hydroxyethyl acrylate and 0.4g of p-hydroxyanisole to carry out end-capping reaction for 5h to obtain a polyurethane-modified acrylic copolymer.

[0032] Preparation Example 4 Preparation of modified chitosan The preparation method of modified chitosan is as follows: after adding 3g of 3,4-dihydroxyphenylpropionic acid to 465mL of chitosan solution with a concentration of 0.72mol / mL and a pH value of 4.8, stirring at a speed of 330r / min for 50min to obtain a mixed solution; adding 7.5g of curcumin, 2.5g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 50mL of an aqueous solution of N-hydroxysulfosuccinimide with a concentration of 2.0mmol / mL to the mixed solution, mixing evenly, adjusting the pH value to 5.3, stirring and reacting at a speed of 490r / min for 11h to obtain a prefabricated chitosan solution; dialyzing the prefabricated chitosan solution in a hydrochloric acid buffer solution with a pH value of 4.9 for 52h, then dialyzing in a PBS buffer solution and deionized water for 3h respectively, and freeze-drying to obtain the modified chitosan.

[0033] Preparation of Comparative Example 1 Preparation of waterborne polyurethane The same as Preparation Example 2, except that an equal amount of polycarbonate diol is used instead of the modified polyol.

[0034] Example 1 A water-based silk-screen UV ink for smart card printing comprises the following raw materials, measured by weight: 80 parts of water-based polyurethane, 3 parts of polyurethane-modified acrylic copolymer, 1 part of photoinitiator, 1 part of polydimethylsiloxane, and 0.5 part of carboxymethyl cellulose, wherein the photoinitiator is composed of ultraviolet light initiator IRGACURE819, ultraviolet light initiator IRGACURE907, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a weight ratio of 5:4:2; the water-based polyurethane is prepared according to Preparation Example 2.

[0035] The method for preparing the above-mentioned water-based screen printing UV ink for smart card printing comprises the following steps: The components except the photoinitiator were mixed and stirred evenly according to the weight fractions, and then the photoinitiator was added and stirred at a stirring speed of 3000 r / min for 30 minutes to obtain a water-based screen printing UV ink for smart card printing.

[0036] Example 2 A water-based silk-screen UV ink for smart card printing comprises the following raw materials, measured by weight: 90 parts of water-based polyurethane, 8 parts of polyurethane-modified acrylic copolymer, 2 parts of photoinitiator, 2 parts of polydimethylsiloxane, and 2 parts of carboxymethyl cellulose. The photoinitiator consists of ultraviolet light initiator IRGACURE819, ultraviolet light initiator IRGACURE907, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a weight ratio of 5:4:2. The water-based polyurethane is prepared in Preparation Example 2.

[0037] The method for preparing the above-mentioned water-based screen printing UV ink for smart card printing comprises the following steps: The components except the photoinitiator were mixed and stirred evenly according to the weight fractions, and then the photoinitiator was added and stirred at a stirring speed of 3000 r / min for 30 minutes to obtain a water-based screen printing UV ink for smart card printing.

[0038] Example 3 A water-based silk-screen UV ink for smart card printing comprises the following raw materials, measured by weight: 85 parts of water-based polyurethane, 6 parts of polyurethane-modified acrylic copolymer, 1.5 parts of photoinitiator, 1.5 parts of polydimethylsiloxane, and 1.2 parts of carboxymethyl cellulose. The photoinitiator consists of ultraviolet light initiator IRGACURE819, ultraviolet light initiator IRGACURE907, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a weight ratio of 5:4:2. The water-based polyurethane is prepared as in Preparation Example 2.

[0039] The method for preparing the above-mentioned water-based screen printing UV ink for smart card printing comprises the following steps: The components except the photoinitiator were mixed and stirred evenly according to the weight fractions, and then the photoinitiator was added and stirred at a stirring speed of 3000 r / min for 30 minutes to obtain a water-based screen printing UV ink for smart card printing.

[0040] Example 4 A water-based silk-screen UV ink for smart card printing comprises the following raw materials by mass: 85 parts of water-based polyurethane, 6 parts of polyurethane-modified acrylic copolymer, 1.5 parts of photoinitiator, 1.5 parts of polydimethylsiloxane, 1.2 parts of carboxymethyl cellulose, and 2.5 parts of modified chitosan. The photoinitiator consists of ultraviolet light initiator IRGACURE819, ultraviolet light initiator IRGACURE907, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 5:4:2. The water-based polyurethane is prepared as in Preparation Example 2.

[0041] The method for preparing the above-mentioned water-based screen printing UV ink for smart card printing comprises the following steps: The components except the photoinitiator were mixed and stirred evenly according to the weight fractions, and then the photoinitiator was added and stirred at a stirring speed of 3000 r / min for 30 minutes to obtain a water-based screen printing UV ink for smart card printing.

[0042] Comparative Example 1 The same as Example 4, except that the waterborne polyurethane is prepared according to Comparative Example 1.

[0043] Comparative Example 2 The same as Example 3, except that the photoinitiator is ultraviolet photoinitiator IRGACURE819.

[0044] Comparative Example 3 The same as Example 3, except that the photoinitiator is ultraviolet photoinitiator IRGACURE907.

[0045] Comparative Example 4 The same as Example 3, except that the photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0046] Performance Testing The water-based screen printing UV inks for smart card printing prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were sampled and tested for the following performance using different testing methods according to different standards. The test results are shown in Table 1.

[0047] The adhesion fastness test method is tested in accordance with GB / T13217.7-2009; Glossiness: Test the glossiness of the sample according to the method specified in GB / T13217.2-2009 “Liquid Ink Color Gloss Method”; Adhesion: According to GB9286-1988, the coating film surface is tested by the 100-grid test, 0-5 levels, 5 is the worst; Abrasion resistance test: RCA test (i.e. paper tape friction test) is adopted, and it meets the requirements of 175g force, 300 continuous rotations of the paper tape, and the ink layer does not leak to the bottom, which is qualified.

[0048] Antibacterial performance and antibacterial durability: The national standard GB / T21866-2008 "Antibacterial performance determination method and antibacterial effect of antibacterial coatings (paint films)" is used to determine the antibacterial performance and antibacterial durability; Aging resistance: Apply the sample on a square plastic sheet with a side length of 2 cm. After UV curing, use the national standard GB / T1865-2009 "Artificial weathering and artificial radiation exposure of paints and varnishes to filtered xenon arc radiation" to age the sample for 400 hours, and observe whether the sample is powdered, peeled or faded; Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The water-based silk-screen UV ink for smart card printing prepared in Examples 1 to 4 does not add organic solvents, greatly reduces VOCs emissions, is green and environmentally friendly, and has excellent wear resistance, adhesion, antibacterial properties, antioxidant properties and a certain degree of heat resistance, and excellent mechanical properties. The cured ink has strong adhesion and high gloss, which can meet the needs of the high-end market.

[0049] 2) A comparative analysis of the performance of the water-based screen printing UV ink for smart card printing prepared in combination with Example 4 and Example 1-Example 3 shows that the addition of the modified chitosan prepared in the present application improves the adhesion of the water-based screen printing UV ink, provides anti-aging and UV protection, makes the color of the water-based screen printing UV ink more stable after exposure, and further improves the gloss and antibacterial properties of the water-based screen printing UV ink.

[0050] 3) The performance comparison analysis of the water-based screen printing UV ink for smart card printing prepared in Example 4 and Comparative Example 1 shows that the modified polyol prepared in the present application contains hindered phenol, quaternary ammonium salt, Schiff base and cyclic siloxane structure, wherein the hindered phenol structure has excellent antioxidant properties, can improve the antioxidant property of the polyurethane matrix, and avoid adding additional antioxidants to affect the homogeneity of the ink; in addition, the introduction of the quaternary ammonium salt structure, quaternary ammonium salt is a broad-spectrum bactericide that can dissociate a quaternary ammonium salt cation containing a positive charge, and its N +The ions can adsorb onto the cell walls of negatively charged bacteria, destroy the cell membrane, denature the protein, hinder the replication and reproduction of DNA, and improve the antibacterial properties of the polyurethane matrix; not only that, the introduced Schiff base structure can interact with bacterial proteins and enzymes, hinder the synthesis of bacterial nucleotides and amino acids, and play a synergistic role with quaternary ammonium ions, significantly improving the antibacterial properties of the polyurethane matrix; finally, the cyclic siloxane structure contains multiple Si-O bonds with high bond energy, which can improve the heat resistance of the polyurethane matrix to a certain extent; from the structure of the modified polyol itself, it is based on cyclic siloxane as the core, and there are -OH molecular chains with a dendritic structure distributed on the side, so that the modified polyol can directly participate in the polymerization process with isocyanate, and can form a cross-linked polyurethane network structure, which not only improves the mechanical properties of the polyurethane matrix, but also makes the performance of the modified polyol more long-lasting and stable.

[0051] 4) The performance comparison analysis of the water-based screen printing UV ink for smart card printing prepared in combination with Example 4 and Comparative Examples 2-4 shows that the photoinitiator is composed of ultraviolet light initiator IRGACURE819, ultraviolet light initiator IRGACURE907 and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 5:4:2. By utilizing their synergistic effect in water-based flexographic printing ink, the ultraviolet light initiator and the synergist work together to achieve rapid curing and drying of the ink, reduce energy consumption and cost, thereby improving the adhesion, wear resistance and antibacterial properties of the ink, while maintaining high gloss on the surface of the ink.

[0052] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A water-based screen printing UV ink for smart card printing, characterized in that: The preparation raw materials include the following by weight: 80-90 parts of waterborne polyurethane, 3-8 parts of polyurethane modified acrylic copolymer, 1-2 parts of photoinitiator, 1-2 parts of defoamer and 0.5-2 parts of waterborne thickener.

2. The water-based screen printing UV ink for smart card printing according to claim 1, characterized in that: The waterborne polyurethane comprises the following raw materials, calculated by weight: 9 parts of isophorone diisocyanate, 25 parts of modified polyol, 2.5 parts of dihydroxymethylbutyric acid, 2 parts of 1.4-butanediol, 1.3 parts of potassium hydroxide, 6 parts of N-methylpyrrolidone, 3 parts of acetone, 70 parts of water, and 0.08 parts of butyltin dilaurate.

3. The water-based screen printing UV ink for smart card printing according to claim 2, characterized in that: The preparation method of the modified polyol comprises the following steps: S31. In a three-necked flask equipped with a stirring device, 23.4 g of 3,5-di-tert-butyl-4-hydroxybenzaldehyde, 15 mL of piperidine and 100 mL of toluene were mixed, the temperature was raised to 57° C., and the mixture was stirred until the solid was completely dissolved. 11.5 g of diethylenetriamine was added dropwise. After the addition was completed, the mixture was kept warm for 6 h. After the reaction was completed, the mixture was naturally cooled and distilled under reduced pressure to obtain intermediate 1. S32, in a three-necked flask equipped with a stirring device, 31.9 g of intermediate 1, 9.1 g of thioglycolic acid, 20.6 g of dicyclohexylcarbodiimide and 110 mL of toluene were mixed and stirred evenly, and reacted for 4 h in a water bath at 53° C. After the reaction was completed, the mixture was filtered and the solvent was removed by distillation under reduced pressure to obtain intermediate 2; S33, add 158.1g of intermediate 2, 1.6g of azobisisobutyronitrile, and 250mL of N,N-dimethylformamide into a three-necked flask, stir and mix evenly, then dropwise add 34.4g of tetramethyltetravinylcyclotetrasiloxane, maintain the temperature of the system at 86°C, react for 7h, after the reaction is completed, first remove part of the solvent by rotary evaporation, and then purify by column chromatography (the eluent is a mixed solvent of ethyl acetate / toluene, the volume ratio of the two is 3:4), and remove the eluent by rotary evaporation to obtain intermediate 3; S34. At room temperature, 191.2 g of intermediate 3, 88.1 g of 4-chloro-1-butanol, 63.5 g of potassium carbonate and 500 mL of N,N-dimethylformamide were stirred and mixed in a three-necked flask under nitrogen protection. The reaction temperature was controlled to 71°C. After the reaction was kept warm for 7 hours, the temperature was further increased to 80°C and kept warm for 6 hours. After the reaction was completed, it was cooled to room temperature, distilled under reduced pressure, washed with anhydrous ethanol 3 times, and vacuum dried to obtain a modified polyol.

4. The water-based screen printing UV ink for smart card printing according to claim 1, characterized in that: The preparation method of the waterborne polyurethane comprises the following steps: S41. Mix isophorone diisocyanate and modified polyol in a polymerization kettle according to their mass fractions, raise the temperature to 90° C. and stir in a constant temperature water bath for 3 hours, then add butyltin dilaurate and continue stirring for 50 minutes, then when the temperature of the reaction solution is reduced to 57° C., disperse dimethylolbutyric acid in N-methylpyrrolidone and add it to the polymerization kettle reaction solution, then raise the temperature to 75° C., react for 15 minutes, add half of acetone to adjust the viscosity, then raise the temperature to 93° C. and react for 2.3 hours to obtain a waterborne polyurethane prepolymer; S42. Lower the temperature of the waterborne polyurethane prepolymer to 32°C, slowly add 1.4-butanediol to the waterborne polyurethane prepolymer, and stir and shear at high speed for 2 hours. During the stirring process, add the remaining acetone in batches to adjust the viscosity. Add water dropwise to the reaction system in batches under high-speed stirring to fully mix the water and the waterborne polyurethane prepolymer, raise the temperature of the constant temperature water bath to 65°C, then add potassium hydroxide and slow down the rotation speed. Continue the reaction for 90 minutes before discharging the material to obtain a waterborne polyurethane.

5. The water-based screen printing UV ink for smart card printing according to claim 1, characterized in that: The preparation method of the polyurethane modified acrylic copolymer comprises the following steps: S51. Add 50.9 g of isophorone diisocyanate and 0.04 g of dibutyltin dilaurate to a four-necked flask equipped with a condenser, a stirring paddle, and a thermometer, and dropwise add 25 g of polyoxypropylene glycol with a molecular weight of 1000 while stirring. Keep the mixture at 75° C. for 3 h, and take a sample to determine the NCO group content during the reaction by a toluene-di-n-butylamine back titration method. S52, then cool to 60 ° C, dissolve 3.1g of dried dimethylol propionic acid in 10g of acetone, and add dropwise to the flask, stir and react for 2h, take samples to measure the NCO group content until it is close to the theoretical value of 2%, then heat to 80 ° C, add 5.3g of epoxy resin E-44, continue to react for 4h, and measure the acid value to be 118mgKOH / g; S53, finally cooling to 60°C, adding 10.7g of hydroxyethyl acrylate and 0.4g of p-hydroxyanisole to carry out end-capping reaction for 5h to obtain a polyurethane-modified acrylic copolymer.

6. The water-based screen printing UV ink for smart card printing according to claim 1, characterized in that: The photoinitiator is composed of ultraviolet photoinitiator IRGACURE819, ultraviolet photoinitiator IRGACURE907 and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 5:4:

2.

7. The water-based screen printing UV ink for smart card printing according to claim 1, characterized in that: Also includes 2-3 parts of modified chitosan.

8. The water-based screen printing UV ink for smart card printing according to claim 7, characterized in that: The preparation method of the modified chitosan comprises the following steps: adding 3g of 3,4-dihydroxyphenylpropionic acid to 465mL of a chitosan solution having a concentration of 0.72mol / mL and a pH value of 4.8, stirring at a rotation speed of 330r / min for 50min to obtain a mixed solution; adding 7.5g of curcumin, 2.5g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 50mL of an aqueous solution of N-hydroxysulfosuccinimide having a concentration of 2.0mmol / mL to the mixed solution, mixing the mixture evenly, adjusting the pH value to 5.3, stirring at a rotation speed of 490r / min for reaction for 11h to obtain a prefabricated chitosan solution; dialyzing the prefabricated chitosan solution in a hydrochloric acid buffer solution having a pH value of 4.9 for 52h, then dialyzing in a PBS buffer solution and deionized water for 3h respectively, and freeze-drying the mixture to obtain the modified chitosan.

9. The water-based screen printing UV ink for smart card printing according to claim 1, characterized in that: The defoaming agent is polydimethylsiloxane; and the aqueous thickener is carboxymethyl cellulose.

10. A method for preparing a water-based screen printing UV ink for smart card printing according to any one of claims 1 to 9, characterized in that: The following steps are involved: The components except the photoinitiator were mixed and stirred evenly according to the weight fractions, and then the photoinitiator was added and stirred at a stirring speed of 3000 r / min for 30 minutes to obtain a water-based screen printing UV ink for smart card printing.

Citation Information

Patent Citations

  • Method for preparing photo-crosslinking polyurethane film

    CN106750059A

  • Modified urethane acrylate copolymer, photoresist and preparation method of photoresist

    CN106947053A

  • Environment-friendly acrylate modified waterborne polyurethane printing ink and preparation method thereof

    CN112029341A

  • Water-based UV ink-jet ink and preparation method thereof