Method for recovering tin from aluminum slag produced by tin refining
By using a complex system of low-melting point silicon calcium-iron ternary tin sludge and aluminum slag during the tin fire refining process, heating and reducing coal in batches for reduction and smelting, the problem of low tin recovery in aluminum slag is solved. Efficient and low-consumption tin recycling is achieved, simplifying the process flow and reducing unorganized emissions.
Patent Information
- Application Number
- CN202411211487.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
During the tin fire refining process, the aluminum slag is rich in valent metal tin and antimony, but because it produces the highly toxic gas hydrogen arsenide when it encounters water, it is necessary to be cautious when recycling, and the addition of auxiliary materials leads to a decrease in the recovery rate of tin metal.
The low-melting point silicon calcium iron ternary tin sludge and aluminum slag form a complex system. The reduction and smelting of reduced coal is heated in batches through electric furnaces and vacuum furnaces to reduce unorganized emissions and avoid the addition of silicon calcium iron slag-making agent. , directly recycle crude tin and aluminum-rich.
It realizes low-consumption and efficient recycling of tin in aluminum slag, improves the recovery rate of tin metal, reduces unorganized emissions, and simplifies the process flow.
Smart Images

Figure CN119082486A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tin smelting, and in particular relates to a method for recovering tin from aluminum slag produced by tin refining. Background Art
[0002] Mineral resources are non-renewable resources and are the foundation for human survival and development. With the development of the non-ferrous metal industry, natural mineral resources are constantly being consumed and reserves are shrinking step by step, making comprehensive recovery particularly important.
[0003] Generally, during the pyrometallurgical refining process of tin, aluminum particles are added to the molten tin liquid to remove impurities such as arsenic and antimony in the crude tin, and aluminum slag is produced. These aluminum slags are rich in valuable metals such as tin and antimony, and the comprehensive recovery of these valuable metals has good practical significance. However, aluminum slag has the characteristic of producing highly toxic gas arsenic when it comes into contact with water, so it is particularly important to be cautious when comprehensively recovering valuable metals in aluminum slag.
[0004] Aluminum slag is generally smelted in an electric furnace. Because aluminum slag contains a considerable amount of high-melting-point alumina, quartz, iron filings, stone powder and other auxiliary materials need to be added to the slag during the smelting process. These auxiliary materials will dissolve part of the tin in the process of slag formation, resulting in a decrease in the direct recovery rate of tin metal. Summary of the invention
[0005] In view of this, in view of the problems and shortcomings in the above-mentioned prior art, the present invention provides a method for recovering tin from aluminum slag produced by tin refining. The present invention can recover valuable metals in aluminum slag with low consumption and high efficiency.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A method for recovering tin from aluminum slag produced by tin refining, the specific steps of which are:
[0008] Step 1, preparation of raw and auxiliary materials: the raw material is aluminum slag produced during tin pyrometallurgical refining, and the auxiliary materials are tin smelting slag and reducing coal;
[0009] Step 2, putting the tin smelting slag from step 1 into an electric furnace and heating it to 1150-1250° C.;
[0010] Step 3, the aluminum slag and the reducing coal in step 1 are respectively put into the electric furnace with the hot tin smelting slag treated in step 2 in batches according to proportions for reduction smelting, so as to produce crude tin and aluminum-rich smelting slag;
[0011] Step 4: The crude tin obtained in step 3 is sent to a vacuum furnace to recover the tin, and the obtained aluminum-rich smelting slag is sent to a fuming furnace for treatment.
[0012] Optionally, the aluminum slag produced during the tin pyro-refining process in step 1 is produced by adding aluminum particles to the molten liquid crude tin during the crude tin pyro-refining process to remove impurities such as arsenic and antimony in the crude tin, and its chemical composition is 55-75% tin, 3-10% antimony, and 5-15% aluminum.
[0013] Optionally, the tin smelting slag in step 1 is smelting slag produced during the smelting process of tin concentrate, and its chemical composition is 4-10% tin, 15-25% iron oxide, 25-35% silicon dioxide, and 8-30% calcium oxide.
[0014] Optionally, the specific operation of adding the aluminum slag and the reducing coal into the electric furnace in batches according to a proportion in step 3 is as follows:
[0015] After adding 500-800kg of aluminum slag, add reducing coal at a ratio of 5-8% of the aluminum slag. The amount added should be two-thirds of the volume of the electric furnace. After the material pile in the furnace has dropped by two-thirds, continue to add aluminum slag and reducing coal in batches according to proportion. The total amount of aluminum slag added to each furnace is 12-15 tons.
[0016] Optionally, the chemical composition of the crude tin in step 4 is 80-90% tin, 3-8% antimony, 0.01-0.5% arsenic, and 0.01-1% lead.
[0017] Optionally, the chemical composition of the aluminum-rich smelting slag in step 5 is 2-8% tin, 10-25% iron oxide, 15-30% silicon dioxide, 5-25% calcium oxide, and 5-15% aluminum oxide.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention utilizes low melting point silicon-calcium-iron ternary system tin smelting slag and aluminum oxide in aluminum slag to form a complex system of aluminum-rich tin smelting slag.
[0020] (2) The present invention does not require the addition of silicon-calcium-iron slag-forming agents, and can effectively smelt aluminum slag to produce crude tin.
[0021] (3) The present invention is simple and efficient, and adopts a method of adding materials into the furnace in batches, which can effectively reduce the generation of unorganized emissions. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0023] Figure 1The present invention is a process flow chart of a method for recovering tin from aluminum slag produced by tin refining. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0026] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0027] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0028] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0029] The invention discloses a method for recovering tin from aluminum slag produced by tin refining.
[0030] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0031] Embodiment 1:
[0032] like Figure 1 As shown, a method for recovering tin from aluminum slag produced by tin refining, the specific process steps are as follows:
[0033] 1) 6 tons of tin smelting slag with a chemical composition of 5.8% tin, 26.1% silicon dioxide, 16.9% calcium oxide and 21.3% iron oxide are put into an electric furnace, and arc heating is started until the tin smelting slag is melted, and the temperature is 1150°C.
[0034] 2) 12 tons of aluminum slag with a chemical composition of 68.4% Sn, 5.2% Sb and 6.8% Al are prepared, and 600 kg of aluminum slag is added, followed by 30 kg of reducing coal, and 6 tons of aluminum slag is first added into the furnace for smelting.
[0035] After the material height in the furnace drops by two-thirds, 3t of aluminum slag is added into the furnace for smelting by adding 600kg of aluminum slag and then 30kg of reducing coal.
[0036] After the material height in the furnace has dropped by two-thirds, add 600kg of aluminum slag and then 30kg of reducing coal, and then add the remaining 3t of aluminum slag into the furnace for smelting.
[0037] 3) After smelting is completed, open the opening to release the crude tin and aluminum-rich smelting slag.
[0038] The smelting output was 8.47t of crude tin with a chemical composition of 89.2% tin and 7.1% antimony.
[0039] The smelting output was 7.13 tons of aluminum-rich smelting slag with a chemical composition of 6.5% tin, 19.6% silicon dioxide, 14.2% calcium oxide, 17.1% iron oxide and 11.4% aluminum oxide.
[0040] Embodiment 2:
[0041] like Figure 1 As shown, a method for recovering tin from aluminum slag produced by tin refining, the specific process steps are as follows:
[0042] 1) 6 tons of tin smelting slag with a chemical composition of 9.3% tin, 34.6% silicon dioxide, 28.8% calcium oxide and 20.6% iron oxide are put into an electric furnace, and arc heating is started until the tin smelting slag is melted, and the temperature is 1230°C.
[0043] 2) 12 tons of aluminum slag with a chemical composition of 55.8% tin, 3.6% Sb and 12.7% aluminum is prepared, and 600 kg of aluminum slag is added, followed by 36 kg of reducing coal, and 6 tons of aluminum slag is first added into the furnace for smelting.
[0044] After the material height in the furnace has dropped by two-thirds, 3t of aluminum slag is added into the furnace for smelting by adding 600kg of aluminum slag and then 36kg of reducing coal.
[0045] After the material height in the furnace has dropped by two-thirds, the remaining 3t of aluminum slag is added into the furnace for smelting by adding 600kg of aluminum slag and then 36kg of reducing coal.
[0046] 3) After smelting is completed, open the opening to release the crude tin and aluminum-rich smelting slag.
[0047] The smelting output was 6.63t of crude tin with a chemical composition of 92.6% tin and 6.4% antimony.
[0048] The smelting output was 7.66t of aluminum-rich smelting slag with a chemical composition of 5.8% tin, 25.7% silicon dioxide, 21.3% calcium oxide, 15.3% iron oxide and 19.1% aluminum oxide.
[0049] Embodiment 3:
[0050] like Figure 1 As shown, a method for recovering tin from aluminum slag produced by tin refining, the specific process steps are as follows:
[0051] 1) 6 tons of tin smelting slag with a chemical composition of 7.6% tin, 29.8% silicon dioxide, 19.4% calcium oxide and 18.9% iron oxide are put into an electric furnace, and arc heating is started until the tin smelting slag is melted, and the temperature is 1180°C.
[0052] 2) 12 tons of aluminum slag with a chemical composition of 62.3% tin, 8.7% Sb and 9.3% aluminum are prepared, and 600 kg of aluminum slag is added, followed by 47 kg of reducing coal, and 6 tons of aluminum slag is first added into the furnace for smelting.
[0053] After the material height in the furnace drops by two-thirds, 3t of aluminum slag is added into the furnace for smelting by adding 600kg of aluminum slag and then 47kg of reducing coal.
[0054] After the material height in the furnace has dropped by two-thirds, the remaining 3t of aluminum slag is added into the furnace for smelting by adding 600kg of aluminum slag and then 47kg of reducing coal.
[0055] 3) After smelting is completed, open the opening to release the crude tin and aluminum-rich smelting slag.
[0056] The smelting output was 7.79t of crude tin with a chemical composition of 93.1% tin and 12.8% antimony.
[0057] The smelting output was 8.21 tons of aluminum-rich smelting slag with a chemical composition of 3.2% tin, 19.6% silicon dioxide, 13.1% calcium oxide, 11.8% iron oxide, and 13.2% aluminum oxide.
[0058] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be construed as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without inventive work are also considered to fall within the scope of protection of the present invention.
[0059] Comparative Example 1
[0060] 6 tons of aluminum slag with a chemical composition of 63.6% tin, 6.3% Sb and 8.7% aluminum is added into the furnace by adding 600 kg of aluminum slag and then 47 kg of reducing coal.
[0061] 1 ton of quartz stone, 1 ton of iron ore and 0.8 ton of lime are mixed evenly and put into the furnace for arc smelting. The smelting temperature is controlled at 1200℃.
[0062] After smelting is completed, the opening is opened to release the crude tin and aluminum-rich smelting slag.
[0063] The smelting output was 3.6t of crude tin with a chemical composition of 92.3% tin and 11.9% antimony.
[0064] The smelting output was 4.86 tons of aluminum-rich smelting slag with a chemical composition of 6.3% tin, 22.7% silicon dioxide, 23.1% calcium oxide, 51.3% iron oxide and 11.2% aluminum oxide.
[0065] The comparative example shows that the processing volume is significantly reduced and the direct recovery rate of smelting is reduced.
[0066] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for recovering tin from aluminum slag produced by tin refining, characterized in that: The following steps are involved: Step 1, preparation of raw and auxiliary materials: the raw material is aluminum slag produced during tin pyrometallurgical refining, and the auxiliary materials are tin smelting slag and reducing coal; Step 2, putting the tin smelting slag from step 1 into an electric furnace and heating it to 1150-1250° C.; Step 3, the aluminum slag and the reducing coal in step 1 are respectively put into the electric furnace with the hot tin smelting slag treated in step 2 in batches according to proportions for reduction smelting, so as to produce crude tin and aluminum-rich smelting slag; Step 4: The crude tin obtained in step 3 is sent to a vacuum furnace to recover the tin, and the obtained aluminum-rich smelting slag is sent to a fuming furnace for treatment.
2. The method for recovering tin from aluminum slag produced by tin refining according to claim 1, characterized in that: The aluminum slag produced during the tin pyro-refining process in step 1 is produced by adding aluminum particles to the molten liquid crude tin during the crude tin pyro-refining process to remove impurities such as arsenic and antimony in the crude tin, and its chemical composition is 55-75% tin, 3-10% antimony, and 5-15% aluminum.
3. The method for recovering tin from aluminum slag produced by tin refining according to claim 1, characterized in that: The tin smelting slag in step 1 is smelting slag produced during the smelting process of tin concentrate, and its chemical composition is 4-10% tin, 15-25% iron oxide, 25-35% silicon dioxide, and 8-30% calcium oxide.
4. The method for recovering tin from aluminum slag produced by tin refining according to claim 1, characterized in that: The specific operation of adding aluminum slag and reducing coal into the electric furnace in batches according to proportion in step 3 is as follows: After adding 500-800kg of aluminum slag, add reducing coal at a ratio of 5-8% of the aluminum slag. The amount added should be two-thirds of the volume of the electric furnace. After the material pile in the furnace has dropped by two-thirds, continue to add aluminum slag and reducing coal in batches according to proportion. The total amount of aluminum slag added to each furnace is 12-15 tons.
5. The method for recovering tin from aluminum slag produced by tin refining according to claim 1, characterized in that: The chemical composition of the crude tin in step 4 is 80-90% tin, 3-8% antimony, 0.01-0.5% arsenic, and 0.01-1% lead.
6. The method for recovering tin from aluminum slag produced by tin refining according to claim 1, characterized in that: The chemical composition of the aluminum-rich smelting slag in step 5 is 2-8% tin, 10-25% iron oxide, 15-30% silicon dioxide, 5-25% calcium oxide, and 5-15% aluminum oxide.