Preparation method of Fe3O4-PDMS photo-thermal response micro-cylinder surface with lubricating oil directional conveying function
Through the design of the photothermal response microcolumn surface of Fe3O4-PDMS, the use of bionic structure and laser processing technology, the remote and efficient transportation of lubricating oil is achieved, and the problem of oil-deficient lubrication caused by lubricating fluid in the spacecraft is solved, and the aerospace has been improved Life and reliability of device components.
Patent Information
- Application Number
- CN202411181927.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The moving parts of the spacecraft are creeping due to the influence of the temperature gradient of the lubricant in the space environment, resulting in oil lubrication on the friction interface, causing severe wear of mechanical components, reducing the working life of the spacecraft.
Fe3O4-PDMS photothermal response microcolumn surface design is adopted, and the remote, efficient and controllable transport of lubricating oil is achieved through the composite structure of bionic Nepenthes-rice leaf and laser processing, combined with silane coupling agent and nanoparticle modification. , replenish the oil-deficient area and improve the friction and side lubrication state.
It effectively alleviates the problem of lack of oil lubrication, reduces friction and wear of moving parts, improves the life and service reliability of space aircraft, and provides good droplet photothermal drive performance and wettability.
Smart Images

Figure CN119082729A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photothermal response surface design and preparation, and in particular relates to a method for preparing a Fe3O4-PDMS photothermal response microcolumn surface with directional lubricating oil delivery. Background Art
[0002] The moving parts of spacecraft generate a lot of heat in the friction pair area during movement. However, the space environment makes it difficult for this heat to dissipate, forming a sharp temperature gradient on the friction surface. The lubricant "creeps" from the high temperature to the low temperature area under the influence of the temperature gradient, causing the friction interface to be in an oil-starved lubrication state, resulting in severe wear of the moving parts, reducing the service life of mechanical parts, and even causing premature failure of the spacecraft. In order to solve the problem of oil-starved lubrication caused by the "creeping" of lubricants, realize the controllability of lubricant supply, enhance the remote control performance of the lubricant migration process to improve the lubrication performance of moving parts and reduce single point failures, it is of great significance for long-life spacecraft.
[0003] Responsive functional surfaces refer to surfaces whose physical / chemical properties change under the action of an external field, thus changing the surface wettability and achieving the effect of the functional surface on droplet driving. Common responsive functional surfaces include electrically responsive functional surfaces, magnetically responsive functional surfaces, optically responsive functional surfaces, thermally responsive functional surfaces, acoustically responsive functional surfaces, and mechanically stress responsive functional surfaces. Optically responsive functional surfaces have the characteristics of remote operation and flexible operation, and their response speed and stability are relatively good. Light is a flexible external field, and its size, shape, irradiation time, intensity, and process adjustability give it advantages in droplet operation. Droplet operation using light as the driving medium is suitable for remote operation, and the use of light to form an uneven temperature field can drive droplets to operate in real time. Photoresponsive materials are divided into three categories: organic responsive materials, inorganic responsive materials, and other responsive materials. Inorganic photoresponsive materials are mainly various photosensitive inorganic oxides, such as TiO2, V2O5, WO3, ZnO, Ga2O3, and SnO2. These materials can produce surface lattice defects under light, and water molecules invade the destroyed lattices, causing the wettability of the material to change. Inorganic photoresponsive materials have the advantages of low toxicity and good chemical / thermal stability. Organic photoresponsive materials contain photochromic functional groups, such as spiropyran, diarylethenes, and azobenzene, which have the ability to reversibly change molecular configuration under ultraviolet / visible light, which can cause changes in surface wettability. Photoresponsive organic materials have advantages in chemical modification and reaction diversity. The mechanism of action of other photoresponsive materials is to use the black color properties of the surface to convert more light absorption into thermal fields, such as Fe3O4, carbon black, MoS2, etc. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a Fe3O4-PDMS photothermal responsive microcolumn surface with directional lubricating oil delivery, which can realize the remote, efficient and controllable delivery of lubricating oil, replenish lubricating medium to the oil-deficient area in time, improve the lubrication state of the friction pair, avoid mechanical wear caused by oil deficiency, and improve the life and service reliability of spacecraft.
[0005] The technical solution adopted by the invention is a method for preparing a Fe3O4-PDMS photothermal response micro-column surface with directional lubricant delivery, which is specifically implemented in the following steps:
[0006] Step 1, designing a bionic Nepenthes-rice leaf composite structure;
[0007] Step 2: Laser processing of the bionic Nepenthes-rice leaf composite structure on the metal surface;
[0008] Step 3, Fe3O4-PDMS mixture preparation and coating;
[0009] Step 4: Preparation of micro-column structure;
[0010] Step 5, silane coupling agent treatment;
[0011] Step 6: Nanoparticle modification to obtain the Fe3O4-PDMS photothermal responsive microcolumn surface.
[0012] The present invention is also characterized in that:
[0013] Step 1 is implemented according to the following steps:
[0014] Step 1.1, the bionic Nepenthes-rice leaf composite structure is composed of a bionic Nepenthes "human" shaped structure and a bionic rice liquid linear structure. The composite structure is arranged centrally and symmetrically. The upper and lower structures are composed of a bionic Nepenthes "human" shaped track. The upper and lower parts are connected by a bionic rice leaf linear structure to form a composite structure for directional droplet transport.
[0015] Step 1.2, bionic rice leaf connection structure: the linear width Wd of the rice leaf is 20-80 μm, the linear spacing d is 0.1-0.5 mm, the linear track angle Dα is 0-5°, and the linear track length W1 is 1-3 mm;
[0016] Step 1.3, the width Wz of the bionic pitcher plant track is 0.5-2mm, the linear width b1 of a single bionic pitcher plant structure is 100-150μm, the distance b2 between two opposing single bionic pitcher plant structures is 50-200μm, the inclination angle Zα of a single bionic pitcher plant structure is 30-90°, multiple groups of bionic pitcher plant structures are arranged at equal intervals along the length direction, and the spacing h between two adjacent single bionic pitcher plant structures is 500-700μm.
[0017] Step 2 is implemented as follows:
[0018] Step 2.1, grinding the metal specimen to remove the surface oxide layer, the metal specimen is any one of titanium alloy, copper, steel, and aluminum alloy;
[0019] Step 2.2, the metal specimen obtained in step 2.1 is ultrasonically cleaned with anhydrous ethanol for 5-10 minutes to remove surface lipids and organic matter, and then the surface of the metal specimen is rinsed with deionized water to remove the anhydrous ethanol remaining on the surface, and the surface is dried for later use;
[0020] Step 2.3, place the metal specimen horizontally, mark the laser processing area on the surface of the specimen and start marking the bionic Nepenthes-rice leaf composite structure. The laser processing process is set to a laser power of 20-30 W, a laser frequency of 20-50 KHz, a pulse width of 100-300 ns, a processing speed of 50-100 mm / s, and a processing number of 1-3 times;
[0021] Step 2.4, the surface of the metal specimen marked with the bionic pitcher plant-rice leaf composite structure is polished again with 1000-2000# sandpaper to remove the burrs generated by the surface laser processing, and then the surface is polished. The surface of the metal specimen is rinsed with deionized water, and then ultrasonically cleaned in anhydrous ethanol for 5-10 minutes to remove residual metal debris and polishing abrasive particles on the surface of the specimen.
[0022] Step 3 is implemented as follows:
[0023] Step 3.1, mixing polydimethylsiloxane and curing agent at a mass ratio of 5:1-10:1 and stirring to obtain a PDMS mixture;
[0024] Step 3.2, mixing the Fe3O4 particles with the PDMS mixture obtained in step 3.1 at a mass ratio of 0.7:1-1:1, stirring the Fe3O4 particles and the PDMS mixture to obtain a Fe3O4-PDMS mixture, wherein the particle size of the Fe3O4 particles is one or more of microparticles with a particle size of 100 nm-10 μm;
[0025] Step 3.3, use a four-sided coating preparation device to evenly scrape the Fe3O4-PDMS mixture on the surface of the specimen, so that the interior of the bionic pitcher plant-rice leaf composite structure is filled with the Fe3O4-PDMS mixture, clean and wipe the Fe3O4-PDMS mixture in other areas of the surface, so that only the bionic pitcher plant-rice leaf composite structure is filled on the surface.
[0026] Step 4 is implemented according to the following steps:
[0027] Step 4.1, the fluorination liquid is prepared by mixing anhydrous ethanol and fluorosilane, the volume fraction of fluorosilane is 1%-5%, and the fluorosilane is one or more of trichlorotridecafluorooctylsilane, triethoxy-1H,1H,2H,2H-tridecafluorooctylsilane, and 1H,1H,2H,2H-perfluorodecyltriethoxysilane;
[0028] Step 4.2, placing the glass slide in the fluoride solution of step 4.1, and soaking it for 5-10 minutes to complete the low surface energy treatment;
[0029] Step 4.3, using copper foil as a gasket, the glass slide treated with low surface energy in step 4.2 is supported on the surface of the test piece obtained in step 3, and the thickness of the copper foil gasket is 100-400 μm;
[0030] Step 4.4, place the structure obtained in step 4.3 horizontally on the surface of a magnet, let it stand for 1-5 minutes, and obtain a micro-column structure under the guidance of a magnetic field. The magnet is any one of the brands N37, N42, and N52;
[0031] Step 4.5: Place the microcolumn structure sample and the magnet in step 4.4 in a forced air drying oven for curing at a temperature of 70-100°C for 1-3 hours to complete the curing of the Fe3O4-PDMS microcolumn surface.
[0032] Step 5 is implemented according to the following steps:
[0033] Step 5.1, preparing a KH-550 ethanol solution by mixing a KH-550 silane coupling agent and anhydrous ethanol, wherein the mass ratio of the KH-550 silane coupling agent is 1%-5%;
[0034] Step 5.2, soaking the Fe3O4-PDMS micro-column surface specimen obtained in step 4.5 in the KH-550 ethanol solution obtained in step 5.1 at a temperature of 20-25°C for 1-5 minutes;
[0035] Step 5.3: Incubate the surface specimen obtained in step 5.2 in a temperature environment of 20-25°C for 10-20 hours to complete the silane coupling agent treatment.
[0036] Step 6 is implemented according to the following steps:
[0037] Step 6.1, forming a nanoparticle modification solution by mixing SiO2 nanoparticles and anhydrous ethanol, wherein the mass fraction of SiO2 nanoparticles is 1%-5%, and the particle size of SiO2 nanoparticles is 10-50nm. After mixing SiO2 nanoparticles and anhydrous ethanol, the temperature is set to 40-60°C, and magnetic stirring is performed at a speed of 200-400r / min for 5-10min to complete the preparation of the nanoparticle modification solution;
[0038] Step 6.2, placing the test piece treated with the silane coupling agent in step 5 horizontally in the nanoparticle modification solution, soaking for 1-5 minutes, taking it out and letting it stand for 10-20 minutes;
[0039] Step 6.3, placing the specimen obtained in step 6.2 horizontally in the nanoparticle modification solution again, soaking for 1-5 minutes, taking it out and letting it stand for 1-2 hours, to obtain a Fe3O4-PDMS photothermal responsive micro-column surface with directional transport of lubricating oil;
[0040] Step 6.4, infiltrating the surface of the specimen obtained in step 6.3 with lubricating oil, wherein the infiltration amount of the lubricating oil is 200-400 μL, and the lubricating oil is one or more of PAO2, PAO4, and PFPE lubricating oil, to obtain a Fe3O4-PDMS photothermal responsive microcolumn surface with directional transport of water-based droplets.
[0041] The beneficial effect of the present invention is that photothermal responsive lubricant delivery is an efficient delivery method for long-distance droplet delivery. The present invention can obtain good droplet photothermal driving performance and wettability after treatment on various metal surfaces, can effectively alleviate the problem of oil-deficient lubrication through lubricant replenishment, and can drive the lubricant oil to move to the friction area through photothermal drive, thereby reducing the friction and wear of moving parts, and improving the design life of the workpiece, which has good social and economic value. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic diagram of the bionic Nepenthes-rice leaf composite structure designed by the present invention and various parameters;
[0043] Figure 2 This is a SEM image of a local area on the surface of the bionic Nepenthes-rice leaf composite structure of the present invention;
[0044] Figure 3 It is the process of the droplets of the present invention being self-driven in a directional manner on the surface of the bionic Nepenthes-rice leaf composite structure;
[0045] Figure 4 This is a SEM picture of the PDMS-Fe3O4 micro-column structure of the present invention filled in the bionic Nepenthes-rice leaf composite structure. DETAILED DESCRIPTION
[0046] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0047] The method for preparing the surface of a Fe3O4-PDMS photothermal response microcolumn with directional lubricant delivery of the present invention is specifically implemented according to the following steps:
[0048] Step 1, designing a bionic Nepenthes-rice leaf composite structure;
[0049] Combination Figure 1 , Figure 2 , Figure 3 , step 1 is implemented according to the following steps:
[0050] Step 1.1, the bionic Nepenthes-rice leaf composite structure is composed of a bionic Nepenthes "human" shaped structure and a bionic rice liquid linear structure. The composite structure is arranged centrally and symmetrically. The upper and lower structures are composed of a bionic Nepenthes "human" shaped track. The upper and lower parts are connected by a bionic rice leaf linear structure to form a composite structure for directional droplet transport.
[0051] Step 1.2: Bionic rice leaf connection structure Rice leaf linear width W d is 20-80 μm, the linear spacing d is 0.1-0.5 mm, the linear track angle Dα is 0-5°, and the linear track length W1 is 1-3 mm;
[0052] Step 1.3, the width Wz of the bionic pitcher plant track is 0.5-2mm, the linear width b1 of a single bionic pitcher plant structure is 100-150μm, the distance b2 between two opposing single bionic pitcher plant structures is 50-200μm, the inclination angle Zα of a single bionic pitcher plant structure is 30-90°, multiple groups of bionic pitcher plant structures are arranged at equal intervals along the length direction, and the spacing h between two adjacent single bionic pitcher plant structures is 500-700μm.
[0053] Step 2: Laser processing of the bionic Nepenthes-rice leaf composite structure on the metal surface;
[0054] Step 2 is implemented as follows:
[0055] Step 2.1, grinding the metal specimen to remove the surface oxide layer, the metal specimen is any one of titanium alloy, copper, steel, and aluminum alloy;
[0056] Step 2.2, the metal specimen obtained in step 2.1 is ultrasonically cleaned with anhydrous ethanol for 5-10 minutes to remove surface lipids and organic matter, and then the surface of the metal specimen is rinsed with deionized water to remove the anhydrous ethanol remaining on the surface, and the surface is dried for later use;
[0057] Step 2.3, place the metal specimen horizontally, mark the laser processing area on the surface of the specimen and start marking the bionic Nepenthes-rice leaf composite structure. The laser processing process is set to a laser power of 20-30 W, a laser frequency of 20-50 KHz, a pulse width of 100-300 ns, a processing speed of 50-100 mm / s, and a processing number of 1-3 times;
[0058] Step 2.4, the surface of the metal specimen marked with the bionic pitcher plant-rice leaf composite structure is polished again with 1000-2000# sandpaper to remove the burrs generated by the surface laser processing, and then the surface is polished. The surface of the metal specimen is rinsed with deionized water, and then ultrasonically cleaned in anhydrous ethanol for 5-10 minutes to remove residual metal debris and polishing abrasive particles on the surface of the specimen.
[0059] Step 3, Fe3O4-PDMS mixture preparation and coating;
[0060] Step 3 is implemented as follows:
[0061] Step 3.1, mixing polydimethylsiloxane and curing agent at a mass ratio of 5:1-10:1 and stirring to obtain a PDMS mixture;
[0062] Step 3.2, mixing the Fe3O4 particles with the PDMS mixture obtained in step 3.1 at a mass ratio of 0.7:1-1:1, stirring the Fe3O4 particles and the PDMS mixture to obtain a Fe3O4-PDMS mixture, wherein the particle size of the Fe3O4 particles is one or more of microparticles with a particle size of 100 nm-10 μm;
[0063] Step 3.3, evenly scrape the Fe3O4-PDMS mixture on the surface of the specimen so that the interior of the bionic pitcher plant-rice leaf composite structure is filled with the Fe3O4-PDMS mixture, clean and wipe the Fe3O4-PDMS mixture in other areas of the surface so that only the bionic pitcher plant-rice leaf composite structure is filled on the surface.
[0064] Combination Figure 4 , step 4, preparation of micro-column structure;
[0065] Step 4 is implemented according to the following steps:
[0066] Step 4.1, the fluorination liquid is prepared by mixing anhydrous ethanol and fluorosilane, the volume fraction of fluorosilane is 1%-5%, and the fluorosilane is one or more of trichlorotridecafluorooctylsilane, triethoxy-1H,1H,2H,2H-tridecafluorooctylsilane, and 1H,1H,2H,2H-perfluorodecyltriethoxysilane;
[0067] Step 4.2, placing the glass slide in the fluoride solution of step 4.1, and soaking it for 5-10 minutes to complete the low surface energy treatment;
[0068] Step 4.3, using copper foil as a gasket, the glass slide treated with low surface energy in step 4.2 is supported on the surface of the test piece obtained in step 3, and the thickness of the copper foil gasket is 100-400 μm;
[0069] Step 4.4, place the structure obtained in step 4.3 horizontally on the surface of a magnet, let it stand for 1-5 minutes, and obtain a micro-column structure under the guidance of a magnetic field. The magnet is any one of the brands N37, N42, and N52;
[0070] Step 4.5: Place the microcolumn structure sample and the magnet in step 4.4 in a forced air drying oven for curing at a temperature of 70-100°C for 1-3 hours to complete the curing of the Fe3O4-PDMS microcolumn surface.
[0071] Step 5, silane coupling agent treatment;
[0072] Step 5 is implemented according to the following steps:
[0073] Step 5.1, preparing a KH-550 ethanol solution by mixing a KH-550 silane coupling agent and anhydrous ethanol, wherein the mass ratio of the KH-550 silane coupling agent is 1%-5%;
[0074] Step 5.2, soaking the Fe3O4-PDMS micro-column surface specimen obtained in step 4.5 in the KH-550 ethanol solution obtained in step 5.1 at a temperature of 20-25°C for 1-5 minutes;
[0075] Step 5.3: Incubate the surface specimen obtained in step 5.2 in a temperature environment of 20-25°C for 10-20 hours to complete the silane coupling agent treatment.
[0076] Step 6: Nanoparticle modification to obtain the Fe3O4-PDMS photothermal responsive microcolumn surface.
[0077] Step 6 is implemented according to the following steps:
[0078] Step 6.1, forming a nanoparticle modification solution by mixing SiO2 nanoparticles and anhydrous ethanol, wherein the mass fraction of SiO2 nanoparticles is 1%-5%, and the particle size of SiO2 nanoparticles is 10-50nm. After mixing SiO2 nanoparticles and anhydrous ethanol, the temperature is set to 40-60°C, and magnetic stirring is performed at a speed of 200-400r / min for 5-10min to complete the preparation of the nanoparticle modification solution;
[0079] Step 6.2, placing the test piece treated with the silane coupling agent in step 5 horizontally in the nanoparticle modification solution, soaking for 1-5 minutes, taking it out and letting it stand for 10-20 minutes;
[0080] Step 6.3, placing the specimen obtained in step 6.2 horizontally in the nanoparticle modification solution again, soaking for 1-5 minutes, taking it out and letting it stand for 1-2 hours, to obtain a Fe3O4-PDMS photothermal responsive micro-column surface with directional transport of lubricating oil;
[0081] Step 6.4, infiltrating the surface of the specimen obtained in step 6.3 with lubricating oil, wherein the infiltration amount of the lubricating oil is 200-400 μL, and the lubricating oil is one or more of PAO2, PAO4, and PFPE lubricating oil, to obtain a Fe3O4-PDMS photothermal responsive microcolumn surface with directional transport of water-based droplets.
[0082] Example 1
[0083] The method for preparing the surface of a Fe3O4-PDMS photothermal response microcolumn with directional lubricant delivery of the present invention is specifically implemented according to the following steps:
[0084] Step 1, designing a bionic Nepenthes-rice leaf composite structure;
[0085] Step 2: Laser processing of the bionic Nepenthes-rice leaf composite structure on the metal surface;
[0086] Step 3, Fe3O4-PDMS mixture preparation and coating;
[0087] Step 4: Preparation of micro-column structure;
[0088] Step 5, silane coupling agent treatment;
[0089] Step 6: Nanoparticle modification to obtain the Fe3O4-PDMS photothermal responsive microcolumn surface.
[0090] Example 2
[0091] The Fe3O4-PDMS photothermal response micro-column surface is prepared by selecting a Ti6Al4V specimen, and a Φ30×5 (mm) titanium alloy specimen is selected. A specific embodiment of a Fe3O4-PDMS photothermal response micro-column surface with directional delivery of lubricating oil.
[0092] Step 1, designing a bionic Nepenthes-rice leaf composite structure;
[0093] Step 1 is implemented according to the following steps:
[0094] Step 1.1, the bionic Nepenthes-rice leaf composite structure is composed of the bionic Nepenthes "human" shaped structure and the bionic rice liquid linear structure. The composite structure is arranged centrally and symmetrically, the upper and lower structures are composed of the bionic Nepenthes "human" shaped track, and the upper and lower parts are connected by the bionic rice leaf linear structure to form a composite structure that can be used for directional droplet transport;
[0095] Step 1.2, bionic rice leaf connection structure: the linear width Wd of the rice leaf is 20 μm, the linear spacing d is 0.15 mm, the linear track angle Dα is 5°, and the linear track length W1 is 3 mm;
[0096] Step 1.3, the bionic pitcher plant track width Wz is 1 mm, the linear width b1 of a single bionic pitcher plant structure is 100 μm, the center spacing b2 is 100 μm, the inclination angle Zα is 30°, and multiple groups of bionic pitcher plant structures are arranged at equal intervals along the length direction, and the arrangement spacing h is 500 μm.
[0097] Step 2: Laser processing of the bionic Nepenthes-rice leaf composite structure on the titanium alloy surface;
[0098] Step 2 is implemented as follows:
[0099] Step 2.1, grinding the titanium alloy specimen to remove the surface oxide layer;
[0100] Step 2.2, the test piece obtained in step 2.1 is ultrasonically cleaned with anhydrous ethanol for 5 minutes to remove surface lipids and organic matter, and the surface of the test piece is rinsed with deionized water to remove the anhydrous ethanol remaining on the surface, and the surface is dried for later use;
[0101] Step 2.3, place the specimen horizontally, mark the laser processing area on the specimen surface and start marking the bionic Nepenthes-rice leaf composite structure. The laser processing process is set to a laser power of 20 W, a laser frequency of 20 KHz, a pulse width of 300 ns, a processing speed of 50 mm / s, and a processing number of 3 times;
[0102] Step 2.4, the surface of the specimen marked with the bionic pitcher plant-rice leaf composite structure was polished again with 1000# sandpaper to remove the burrs generated by the surface laser processing, and then the surface was polished. The surface of the specimen was rinsed with deionized water, and then ultrasonically cleaned in anhydrous ethanol for 5 minutes to remove residual metal debris and polishing abrasive particles on the surface of the specimen.
[0103] Step 3, Fe3O4-PDMS mixture preparation and coating;
[0104] Step 3 is implemented as follows:
[0105] Step 3.1, mixing polydimethylsiloxane and curing agent at a mass ratio of 10:1 and stirring to obtain a PDMS mixture;
[0106] Step 3.2, mixing the Fe3O4 particles and the PDMS mixture obtained in step 3.1 at a mass ratio of 1:1, and stirring the Fe3O4 particles and the PDMS mixture to obtain a Fe3O4-PDMS mixture, wherein the particle size of the Fe3O4 particles is one or more of microparticles with a particle size of 100 nm-10 μm;
[0107] Step 3.3, use a four-sided coating preparation device to evenly scrape the Fe3O4-PDMS mixture on the surface of the specimen, so that the interior of the bionic pitcher plant-rice leaf composite structure is filled with the Fe3O4-PDMS mixture, clean and wipe the Fe3O4-PDMS mixture in other areas of the surface, so that only the bionic pitcher plant-rice leaf composite structure is filled on the surface.
[0108] Step 4: Preparation of micro-column structure
[0109] Step 4 is implemented according to the following steps:
[0110] Step 4.1, the fluorinated liquid component is prepared by mixing anhydrous ethanol and fluorosilane, the volume fraction of the fluorosilane is 1%, and the fluorosilane is trichlorotridecafluorooctylsilane;
[0111] Step 4.2, place the glass slide in the fluoride solution and soak it for 5 minutes to complete the low surface energy treatment;
[0112] Step 4.3, using copper foil as a gasket, the glass slide treated with low surface energy in step 4.2 is supported on the surface of the test piece obtained in step 3.3, and the thickness of the copper foil gasket is 100 μm;
[0113] Step 4.4, place the structure obtained in step 4.3 horizontally on the surface of the magnet, let it stand for 1 minute, and obtain a micro-column structure under the guidance of the magnetic field. The magnet is brand N52;
[0114] Step 4.5: Place the microcolumn structure sample and the magnet in step 4.4 in a forced air drying oven for curing at a temperature of 70°C for 3 hours to complete the curing of the Fe3O4-PDMS microcolumn surface.
[0115] Step 5, silane coupling agent treatment;
[0116] Step 5 is implemented according to the following steps:
[0117] Step 5.1, the KH-550 ethanol solution is composed of KH-550 silane coupling agent and anhydrous ethanol, and the mass ratio of the KH-550 silane coupling agent is 1%;
[0118] Step 5.2, immerse the Fe3O4-PDMS micro-column surface specimen obtained in step 4.5 in KH-550 ethanol solution at a temperature of 20°C for 5 minutes;
[0119] Step 5.3: Incubate the surface obtained in step 5.2 in a temperature environment of 20-25° C. for 10-20 hours to complete the silane coupling agent treatment.
[0120] Step 6: Nanoparticle modification to obtain the Fe3O4-PDMS photothermal responsive microcolumn surface.
[0121] Step 6 is implemented according to the following steps:
[0122] Step 6.1, the nanoparticle modification solution is composed of SiO2 nanoparticles and anhydrous ethanol, the mass fraction of SiO2 nanoparticles is 1%, and the particle size of SiO2 nanoparticles is 10nm. After the SiO2 nanoparticles and anhydrous ethanol are mixed, the temperature is set to 40-60°C, and the magnetic stirring is performed at a speed of 200r / min for 5min to complete the preparation of the nanoparticle modification solution;
[0123] Step 6.2, placing the test piece treated with the silane coupling agent in step 5.3 horizontally in the nanoparticle modification solution, soaking for 1 minute, taking it out and letting it stand for 10 minutes;
[0124] Step 6.3, placing the specimen obtained in step 6.2 horizontally in the nanoparticle modification solution, soaking for 5 minutes, taking it out and letting it stand for 1 hour, to obtain a Fe3O4-PDMS photothermal responsive micro-column surface with directional transport of lubricating oil;
[0125] Step 6.4, soaking the surface of the specimen obtained in step 6.3 with 200 μL of lubricating oil, wherein the lubricating oil is PFPE lubricating oil, to obtain a Fe3O4-PDMS photothermal responsive micro-column surface with directional transport of water-based droplets.
[0126] Example 3
[0127] The Fe3O4-PDMS photothermal response micro-column surface is prepared by selecting Ti6Al4V as the specimen and selecting a copper specimen of Φ30×5 (mm). A specific embodiment of the Fe3O4-PDMS photothermal response micro-column surface with directional delivery of lubricating oil.
[0128] Step 1, designing a bionic Nepenthes-rice leaf composite structure;
[0129] Step 1 is implemented according to the following steps:
[0130] Step 1.1, the bionic Nepenthes-rice leaf composite structure is composed of the bionic Nepenthes "human" shaped structure and the bionic rice liquid linear structure. The composite structure is arranged centrally and symmetrically, the upper and lower structures are composed of the bionic Nepenthes "human" shaped track, and the upper and lower parts are connected by the bionic rice leaf linear structure to form a composite structure that can be used for directional droplet transport;
[0131] Step 1.2, bionic rice leaf connection structure: the linear width Wd of the rice leaf is 80 μm, the linear spacing d is 0.5 mm, the linear track angle Dα is 5°, and the linear track length W1 is 3 mm;
[0132] Step 1.3, the bionic pitcher plant track width Wz is 2 mm, the linear width b1 of a single bionic pitcher plant structure is 150 μm, the center spacing b2 is 200 μm, the inclination angle Zα is 90°, and multiple groups of bionic pitcher plant structures are arranged at equal intervals along the length direction, and the arrangement spacing h is 700 μm.
[0133] Step 2: Laser processing of the copper surface to form a bionic Nepenthes-rice leaf composite structure;
[0134] Step 2 is implemented as follows:
[0135] Step 2.1, grinding the metal specimen to remove the surface oxide layer, the metal specimen is one of titanium alloy, copper, steel, and aluminum alloy;
[0136] Step 2.2, the test piece obtained in step 2.1 is ultrasonically cleaned with anhydrous ethanol for 10 minutes to remove surface lipids and organic matter, and the surface of the test piece is rinsed with deionized water to remove the anhydrous ethanol remaining on the surface, and the surface is dried for standby use;
[0137] Step 2.3, place the specimen horizontally, mark the laser processing area on the surface of the specimen and start marking the bionic Nepenthes-rice leaf composite structure. The laser processing process is set to a laser power of 20 W, a laser frequency of 20 KHz, a pulse width of 100 ns, a processing speed of 50 mm / s, and a processing number of 1 time;
[0138] Step 2.4, the surface of the specimen marked with the bionic pitcher plant-rice leaf composite structure was polished again with 2000# sandpaper to remove the burrs generated by the surface laser processing, and then the surface was polished. The surface of the specimen was rinsed with deionized water, and then ultrasonically cleaned in anhydrous ethanol for 5 minutes to remove residual metal debris and polishing abrasive particles on the surface of the specimen.
[0139] Step 3, Fe3O4-PDMS mixture preparation and coating;
[0140] Step 3 is implemented as follows:
[0141] Step 3.1, mixing polydimethylsiloxane and curing agent at a mass ratio of 5:1 and stirring to obtain a PDMS mixture;
[0142] Step 3.2, mixing the Fe3O4 particles and the PDMS mixture obtained in step 3.1 at a mass ratio of 0.7:1, and stirring the Fe3O4 particles and the PDMS mixture to obtain a Fe3O4-PDMS mixture, wherein the particle size of the Fe3O4 particles is one or more of microparticles with a particle size of 1 μm;
[0143] Step 3.3, use a four-sided coating preparation device to evenly scrape the Fe3O4-PDMS mixture on the surface of the specimen, so that the interior of the bionic pitcher plant-rice leaf composite structure is filled with the Fe3O4-PDMS mixture, clean and wipe the Fe3O4-PDMS mixture in other areas of the surface, so that only the bionic pitcher plant-rice leaf composite structure is filled on the surface.
[0144] Step 4: Preparation of micro-column structure
[0145] Step 4 is implemented according to the following steps:
[0146] Step 4.1, the fluorination liquid component is prepared by mixing anhydrous ethanol and fluorosilane, the volume fraction of fluorosilane is 1%, and the fluorosilane is 1H,1H,2H,2H-perfluorodecyltriethoxysilane;
[0147] Step 4.2, place the glass slide in the fluoride solution and soak it for 10 minutes to complete the low surface energy treatment;
[0148] Step 4.3, using copper foil as a gasket, the glass slide treated with low surface energy in step 4.2 is supported on the surface of the test piece obtained in step 3.3, and the thickness of the copper foil gasket is 400 μm;
[0149] Step 4.4, place the structure obtained in step 4.3 horizontally on the surface of the magnet, let it stand for 5 minutes, and obtain a micro-column structure under the guidance of the magnetic field. The magnet is grade N42;
[0150] Step 4.5: Place the microcolumn structure sample and the magnet prepared in step 4.4 in a forced air drying oven for curing at a temperature of 100° C. for 1 h to complete the curing of the Fe3O4-PDMS microcolumn surface.
[0151] Step 5, silane coupling agent treatment;
[0152] Step 5 is implemented according to the following steps:
[0153] Step 5.1, the KH-550 ethanol solution is composed of KH-550 silane coupling agent and anhydrous ethanol, and the mass ratio of the KH-550 silane coupling agent is 1%;
[0154] Step 5.2, immerse the Fe3O4-PDMS micro-column surface specimen obtained in step 4.5 in KH-550 ethanol solution at a temperature of 25°C for 5 minutes;
[0155] Step 5.3: Incubate the surface obtained in step 5.2 in a 25°C temperature environment for 10 hours to complete the silane coupling agent treatment.
[0156] Step 6: Nanoparticle modification to obtain the Fe3O4-PDMS photothermal responsive microcolumn surface.
[0157] Step 6 is implemented according to the following steps:
[0158] Step 6.1, the nanoparticle modification solution is composed of SiO2 nanoparticles and anhydrous ethanol, the mass fraction of SiO2 nanoparticles is 5%, and the particle size of SiO2 nanoparticles is 50nm. After the SiO2 nanoparticles and anhydrous ethanol are mixed, the temperature is set to 60°C, and the magnetic stirring is performed at a speed of 400r / min for 10min to complete the preparation of the nanoparticle modification solution;
[0159] Step 6.2, placing the test piece treated with the silane coupling agent in step 5.3 horizontally in the nanoparticle modification solution, soaking for 5 minutes, taking it out and letting it stand for 20 minutes;
[0160] Step 6.3, placing the specimen obtained in step 6.2 horizontally in the nanoparticle modification solution, soaking for 5 minutes, taking it out and letting it stand for 2 hours, to obtain a Fe3O4-PDMS photothermal responsive micro-column surface with directional transport of lubricating oil;
[0161] Step 6.4, soaking the surface of the specimen obtained in step 6.3 with 400 μL of lubricating oil, wherein the lubricating oil is PAO2 lubricating oil, to obtain a Fe3O4-PDMS photothermal responsive micro-column surface with directional transport of water-based droplets.
Claims
1. A method for preparing a Fe3O4-PDMS photothermal response microcolumn surface with directional lubricant delivery, characterized in that: Follow the steps below to implement it: Step 1, designing a bionic Nepenthes-rice leaf composite structure; Step 2: Laser processing of the bionic Nepenthes-rice leaf composite structure on the metal surface; Step 3, Fe3O4-PDMS mixture preparation and coating; Step 4: Preparation of micro-column structure; Step 5, silane coupling agent treatment; Step 6: Nanoparticle modification to obtain the Fe3O4-PDMS photothermal responsive microcolumn surface.
2. The method for preparing the surface of Fe3O4-PDMS photothermal responsive microcolumn with directional lubricant delivery according to claim 1, characterized in that: The step 1 is specifically implemented according to the following steps: Step 1.1, the bionic Nepenthes-rice leaf composite structure is composed of a bionic Nepenthes "human" shaped structure and a bionic rice liquid linear structure. The composite structure is arranged centrally and symmetrically. The upper and lower structures are composed of a bionic Nepenthes "human" shaped track. The upper and lower parts are connected by a bionic rice leaf linear structure to form a composite structure for directional droplet transport. Step 1.2, bionic rice leaf connection structure: the linear width Wd of the rice leaf is 20-80 μm, the linear spacing d is 0.1-0.5 mm, the linear track angle Dα is 0-5°, and the linear track length W1 is 1-3 mm; Step 1.3, the width Wz of the bionic pitcher plant track is 0.5-2mm, the linear width b1 of a single bionic pitcher plant structure is 100-150μm, the distance b2 between two opposing single bionic pitcher plant structures is 50-200μm, the inclination angle Zα of a single bionic pitcher plant structure is 30-90°, multiple groups of bionic pitcher plant structures are arranged at equal intervals along the length direction, and the spacing h between two adjacent single bionic pitcher plant structures is 500-700μm.
3. The method for preparing the surface of Fe3O4-PDMS photothermal response micro-column with directional lubricant delivery according to claim 2, characterized in that: The step 2 is specifically implemented according to the following steps: Step 2.1, grinding the metal specimen to remove the surface oxide layer, the metal specimen is any one of titanium alloy, copper, steel, and aluminum alloy; Step 2.2, the metal specimen obtained in step 2.1 is ultrasonically cleaned with anhydrous ethanol for 5-10 minutes to remove surface lipids and organic matter, and then the surface of the metal specimen is rinsed with deionized water to remove the anhydrous ethanol remaining on the surface, and the surface is dried for later use; Step 2.3, place the metal specimen horizontally, mark the laser processing area on the surface of the specimen and start marking the bionic Nepenthes-rice leaf composite structure. The laser processing process is set to a laser power of 20-30 W, a laser frequency of 20-50 KHz, a pulse width of 100-300 ns, a processing speed of 50-100 mm / s, and a processing number of 1-3 times; Step 2.4, the surface of the metal specimen marked with the bionic pitcher plant-rice leaf composite structure is polished again with 1000-2000# sandpaper to remove the burrs generated by the surface laser processing, and then the surface is polished. The surface of the metal specimen is rinsed with deionized water, and then ultrasonically cleaned in anhydrous ethanol for 5-10 minutes to remove residual metal debris and polishing abrasive particles on the surface of the specimen.
4. The method for preparing the Fe3O4-PDMS photothermal response micro-column surface with directional lubricant delivery according to claim 3, characterized in that: The step 3 is specifically implemented according to the following steps: Step 3.1, mixing polydimethylsiloxane and curing agent at a mass ratio of 5:1-10:1 and stirring to obtain a PDMS mixture; Step 3.2, mixing the Fe3O4 particles with the PDMS mixture obtained in step 3.1 at a mass ratio of 0.7:1-1:1, stirring the Fe3O4 particles and the PDMS mixture to obtain a Fe3O4-PDMS mixture, wherein the particle size of the Fe3O4 particles is one or more of microparticles with a particle size of 100 nm-10 μm; Step 3.3, evenly scrape the Fe3O4-PDMS mixture on the surface of the specimen so that the interior of the bionic pitcher plant-rice leaf composite structure is filled with the Fe3O4-PDMS mixture, clean and wipe the Fe3O4-PDMS mixture in other areas of the surface so that only the bionic pitcher plant-rice leaf composite structure is filled on the surface.
5. The method for preparing the surface of Fe3O4-PDMS photothermal response micro-column with directional lubricant delivery according to claim 4, characterized in that: The step 4 is specifically implemented according to the following steps: Step 4.1, the fluorination liquid is prepared by mixing anhydrous ethanol and fluorosilane, the volume fraction of fluorosilane is 1%-5%, and the fluorosilane is one or more of trichlorotridecafluorooctylsilane, triethoxy-1H,1H,2H,2H-tridecafluorooctylsilane, and 1H,1H,2H,2H-perfluorodecyltriethoxysilane; Step 4.2, placing the glass slide in the fluoride solution of step 4.1, and soaking it for 5-10 minutes to complete the low surface energy treatment; Step 4.3, using copper foil as a gasket, the glass slide treated with low surface energy in step 4.2 is supported on the surface of the test piece obtained in step 3, and the thickness of the copper foil gasket is 100-400 μm; Step 4.4, place the structure obtained in step 4.3 horizontally on the surface of a magnet, let it stand for 1-5 minutes, and obtain a micro-column structure under the guidance of a magnetic field. The magnet is any one of the brands N37, N42, and N52; Step 4.5: Place the microcolumn structure sample and the magnet in step 4.4 in a forced air drying oven for curing at a temperature of 70-100°C for 1-3 hours to complete the curing of the Fe3O4-PDMS microcolumn surface.
6. The method for preparing the surface of Fe3O4-PDMS photothermal response micro-column with directional lubricant delivery according to claim 5, characterized in that: The step 5 is specifically implemented according to the following steps: Step 5.1, preparing a KH-550 ethanol solution by mixing a KH-550 silane coupling agent and anhydrous ethanol, wherein the mass ratio of the KH-550 silane coupling agent is 1%-5%; Step 5.2, soaking the Fe3O4-PDMS micro-column surface specimen obtained in step 4.5 in the KH-550 ethanol solution obtained in step 5.1 at a temperature of 20-25°C for 1-5 minutes; Step 5.3: Incubate the surface specimen obtained in step 5.2 in a temperature environment of 20-25°C for 10-20 hours to complete the silane coupling agent treatment.
7. The method for preparing the surface of Fe3O4-PDMS photothermal response micro-column with directional lubricant delivery according to claim 6, characterized in that: The step 6 is specifically implemented according to the following steps: Step 6.1, forming a nanoparticle modification solution by mixing SiO2 nanoparticles and anhydrous ethanol, wherein the mass fraction of SiO2 nanoparticles is 1%-5%, and the particle size of SiO2 nanoparticles is 10-50nm. After mixing SiO2 nanoparticles and anhydrous ethanol, the temperature is set to 40-60°C, and magnetic stirring is performed at a speed of 200-400r / min for 5-10min to complete the preparation of the nanoparticle modification solution; Step 6.2, placing the test piece treated with the silane coupling agent in step 5 horizontally in the nanoparticle modification solution, soaking for 1-5 minutes, taking it out and letting it stand for 10-20 minutes; Step 6.3, placing the specimen obtained in step 6.2 horizontally in the nanoparticle modification solution again, soaking for 1-5 minutes, taking it out and letting it stand for 1-2 hours, to obtain a Fe3O4-PDMS photothermal responsive micro-column surface with directional transport of lubricating oil; Step 6.4, infiltrating the surface of the specimen obtained in step 6.3 with lubricating oil, wherein the infiltration amount of the lubricating oil is 200-400 μL, and the lubricating oil is one or more of PAO2, PAO4, and PFPE lubricating oil, to obtain a Fe3O4-PDMS photothermal responsive microcolumn surface with directional transport of water-based droplets.
Citation Information
Patent Citations
Anisotropic micro-nano surface based on energy adjusted femtosecond laser bionic processing
CN106167247A
Method for preparing pitcher plant imitated super-lubricative surface by using flame spraying technology
CN107761039A
Preparation method of photo-responsive superhydrophobic / super-lubricous conversion coating
CN109438747A
Preparation method of super-hydrophobic high-oleophobic surface of common nepenthes-like structure
CN112174087A
Preparation method and application of bionic common nepenthes two-dimensional functional material
CN112280083A