Polydopamine modified natural fiber cloth and prepared epoxy resin composite material
By forming a modified coating with covalent bonds and epoxy resin on the surface of natural fibers, the poor compatibility of natural fibers and polymer materials is solved, and the problem of poor compatibility of natural fibers and polymer materials is improved. The mechanical properties and production efficiency of composite materials have been realized, and environmentally friendly industrial applications are achieved.
Patent Information
- Application Number
- CN202411256215.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The surface of natural fibers contains a large amount of colloids and hydroxyl groups, which is easy to absorb water, and has poor compatibility with polymer material matrix, resulting in a decline in the mechanical properties of composite materials. The existing modification methods are long and affecting industrial production efficiency.
Horseradish peroxidase is used as the catalyst, hydrogen peroxide aqueous solution is the oxidant, dopamine hydrochloride is the monomer, water is the reaction medium, and sodium hydroxide aqueous solution is the pH regulator. Under the catalytic action of horseradish peroxidase The modification process takes less than 30 minutes to form a polydopamine-modified natural fiber cloth, and the amino group and epoxy resin are covalently bonded to improve the interface binding force.
It significantly shortens the modification time, improves production efficiency, and enhances the mechanical properties of composite materials. Natural fibers can be completely degraded and have no pollution to the environment. Modified water can be recycled. All substances are non-toxic and harmless.
Smart Images

Figure CN119083179A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of continuous fiber reinforced polymer composite materials, in particular to a polydopamine modified natural fiber cloth and an epoxy resin composite material prepared therefrom. Background Art
[0002] Natural fibers have excellent mechanical properties, biodegradability, and cause almost no environmental pollution. At present, various natural fibers such as flax, ramie, hemp, jute and sisal fibers have been widely used in the research of strengthening and toughening polymer composites. Compared with glass fibers, natural fibers are light in weight, and the composite materials reinforced by them are lighter. Moreover, natural fibers come from nature, and the energy consumed in producing natural fibers is far less than that of glass fibers and synthetic fibers. Therefore, strengthening and toughening polymer materials with natural fibers is gaining more and more attention. However, the surface of natural fibers contains a large amount of colloid and hydroxyl groups, which are highly polar and easy to absorb water. They have poor compatibility with the polymer matrix, resulting in a decrease in the mechanical properties of the composite materials.
[0003] Dopamine, or DA for short, is a naturally occurring substance that exists in the bodies of humans and other animals. It has good biocompatibility and is not prone to cause immune responses or toxic effects. Dopamine has attracted much attention because it has excellent adhesion properties and can form strong adhesion on many surfaces, similar to the role of some biological adhesives in organisms. It has the ability to self-assemble and can form a dense dopamine film on the surface through interactions such as hydrogen bonds and van der Waals forces. Therefore, dopamine is widely believed to have the potential to be a biomimetic adhesive. Dopamine has the ability to adhere because it undergoes self-oxidation reaction under the action of oxygen to generate dopamine quinone, which can then undergo cyclization reaction through Michael addition, so that it can only be coated on the surface of the object to form a protective layer through chemical bonds and non-chemical bonds. Dong et al. used AccelrysMaterial Studio software and COMPASS force field to construct a full-atom model of the dopamine-modified aramid fiber surface. The adhesion mechanism of polydopamine aggregated with 21 typical molecular structures on the aramid fiber surface was analyzed. MD simulation results show that the polydopamine nanofilm forms a clear and smooth interface with the aramid fiber surface. In a small interface area, polydopamine has a high atomic density, which is conducive to the formation of non-covalent bonds between polydopamine and the aramid surface. At present, there have been studies on the use of dopamine to modify fibers, but there has been no research on the use of dopamine to modify natural fiber cloth, and most of the current modification methods are through self-oxidation, which takes a long time (usually more than 24 hours), which is not conducive to improving industrial production efficiency. Summary of the invention
[0004] The object of the present invention is to provide a polydopamine modified natural fiber cloth and epoxy resin composite material prepared therefrom, which is characterized in that natural fiber cloth is used as raw material, horseradish peroxidase is used as catalyst, hydrogen peroxide aqueous solution is used as oxidant, dopamine hydrochloride is used as monomer, water is used as reaction medium, and sodium hydroxide aqueous solution is used as pH regulator. Under the catalytic action of horseradish peroxidase, the whole modification process takes less than 30 minutes, which can greatly improve production efficiency. Since dopamine is rich in amino groups, the amino groups in the modified coating can be combined with epoxy resin in the form of covalent bonds, thereby improving the interfacial bonding force between natural fiber cloth and epoxy resin and enhancing the mechanical properties of the composite material, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a polydopamine modified natural fiber cloth is as follows: Take the natural fiber cloth and soak it in water containing dopamine hydrochloride, add (0.1~5) mol / L NaOH solution, adjust the pH to 6~8, add horseradish peroxidase, and add a (5~10)% volume content of hydrogen peroxide aqueous solution at a stirring speed of 20~100rmp / min using a syringe pump. The whole process lasts for 15~20min, and the reaction is continued for 3~5min. The cloth is taken out and dried and rolled at 30~80℃ to obtain a polydopamine modified natural fiber cloth.
[0006] The natural fiber cloth is at least one of sisal fiber cloth, jute fiber cloth, linen fiber cloth and ramie fiber cloth, and the moisture content of the natural fiber cloth after drying is less than 0.05%; The mass ratio of natural fiber cloth to dopamine hydrochloride is 100:(1-20); The mass ratio of horseradish peroxidase to dopamine hydrochloride is 1:(500-5000); The volume content of hydrogen peroxide in the hydrogen peroxide aqueous solution is 5-10%, and the mass ratio of dopamine hydrochloride to hydrogen peroxide is 1:(0.18-0.25).
[0007] A method for preparing an epoxy resin composite material is as follows: Weigh the epoxy resin and the curing agent, mix them, mature them for 2 to 5 hours, and then evenly apply them on the surface of the polydopamine-modified natural fiber cloth. Curing them at 60 to 90° C. for 15 to 30 minutes to obtain a prepreg. A single layer of prepreg or at least two layers of prepreg are stacked, and hot pressed at 110 to 130° C. for 5 to 10 minutes to obtain an epoxy resin composite material.
[0008] The mass ratio of epoxy resin to curing agent is 100:(10~50); The epoxy resin is epoxy E51 or hydrogenated epoxy E51. Further, the epoxy resin is set to be epoxy E51.
[0009] The curing agent is an alicyclic amine or an aromatic amine curing agent, and further, the curing agent is set to be isophorone diamine.
[0010] Compared with the prior art, the beneficial effects achieved by the present invention are: (1) Using horseradish peroxidase as a catalyst greatly shortens the modification time and improves production efficiency.
[0011] (2) Natural fiber cloth is completely degradable and has no pollution to the environment.
[0012] (3) Natural fiber cloth is inexpensive, widely available, and requires little energy to produce.
[0013] (4) Modified water can be recycled at least 10 times, and all substances used are non-toxic and harmless, and do not pollute the environment.
[0014] (5) Dopamine-modified coatings are rich in amino groups and can be combined with epoxy resin through chemical bonds. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 Schematic diagram of the preparation of PDA / ramie fiber cloth composite material; Figure 2 The flax fiber cloth strips and the polydopamine-modified flax fiber cloth strips obtained in Examples 1, 2, and 3 are actual pictures; Figure 3 This is the infrared spectrum of linen fiber cloth; Figure 4 This is the infrared spectrum of the modified flax fiber cloth obtained in Example 1. DETAILED DESCRIPTION
[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] In the experiment, linen fiber cloth, sisal fiber cloth, jute fiber cloth, and ramie fiber cloth were all purchased from Xinjiang Tiantai Fiber Co., Ltd. The fiber diameters were between 5 and 120 μm, with an average diameter of 43 μm.
[0018] See also Figure 1-4 And Table 1-2, the present invention provides a technical solution: Example 1: Weigh 100g of flax fiber cloth and add it to 1L of aqueous solution containing 5g of dopamine hydrochloride, add 26.3mL of 1mol / L NaOH aqueous solution, adjust the pH to 7, add 2mg of horseradish peroxidase, stir at 50rmp / min, set the injection pump feeding speed to 1.2mL / min, and add 21.5g of 5% hydrogen peroxide aqueous solution. After the hydrogen peroxide aqueous solution is completely added, continue stirring for 3min, take it out, and heat it at 60 o The polydopamine modified flax fiber cloth was obtained by drying under C conditions and rolling.
[0019] Example 2: Weigh 100g of flax fiber cloth and add it to 1L of aqueous solution containing 10g of dopamine hydrochloride, add 52.6mL of 1mol / L NaOH aqueous solution, adjust the pH to 7. Add 4mg of horseradish peroxidase, stir at 50rmp / min, set the injection pump feeding speed to 2.4mL / min, and add 43.0g of 5% hydrogen peroxide aqueous solution. After the hydrogen peroxide aqueous solution is completely added, continue stirring for 3min, take it out, and heat it at 60 o The polydopamine modified flax fiber cloth was obtained by drying under C conditions and rolling.
[0020] Example 3: Weigh 100g of flax fiber cloth and add it to 1L of aqueous solution containing 15g of dopamine hydrochloride, add 78.9mL of 1mol / L NaOH aqueous solution, adjust the pH to 7. Add 6mg of horseradish peroxidase, stir at 50rmp / min, set the injection pump feeding speed to 3.6mL / min, and add 64.5g of 5% hydrogen peroxide aqueous solution. After the hydrogen peroxide aqueous solution is completely added, continue stirring for 3min, take it out, and heat it at 60 o The polydopamine modified flax fiber cloth was obtained by drying under C conditions and rolling.
[0021] Example 4: Weigh 100g of flax fiber cloth and add it to 1L of aqueous solution containing 20g of dopamine hydrochloride, add 105.2mL of 1mol / L NaOH aqueous solution, adjust the pH to 7. Add 8mg of horseradish peroxidase, stir at 50rmp / min, set the injection pump feeding speed to 4.8mL / min, and add 86.0g of 5% hydrogen peroxide aqueous solution. After the hydrogen peroxide aqueous solution is completely added, continue stirring for 3min, take it out, and heat it at 60 o The polydopamine modified flax fiber cloth was obtained by drying under C conditions and rolling.
[0022] Example 5: Take the polydopamine-modified flax fiber cloth prepared in Examples 1-4 and perform the following treatment: Weigh 100g of epoxy E51 and 20g of isophorone diamine into a 500mL beaker, stir and ripen at 100rmp / min for 3h, and then use a glue machine to evenly coat the surface of polydopamine modified flax fiber cloth. o After curing in an oven at 120 °C for 20 min, the prepreg was obtained. Three layers of prepreg were stacked and placed in a 120 °C oven. o C press was hot pressed for 5 minutes to obtain sample 1, sample 2, sample 3 and sample 4.
[0023] Embodiment 6: Based on Embodiment 3, the following treatment is performed: Weigh 100g of epoxy E51 and 10g of isophorone diamine into a 500mL beaker, stir and ripen at 100rmp / min for 3h, and then use a glue machine to evenly coat the surface of polydopamine-modified flax fiber cloth. o After curing in an oven at 120 °C for 20 min, the prepreg was obtained. Three layers of prepreg were stacked and placed in a 120 °C oven. o C press for 5 min to obtain sample 5.
[0024] Embodiment 7: Based on Embodiment 3, the following treatment is performed: Weigh 100g of epoxy E51 and 30g of isophorone diamine into a 500mL beaker, stir and ripen at 100rmp / min for 3h, and then use a glue machine to evenly coat the surface of polydopamine-modified flax fiber cloth. o After curing in an oven at 120 °C for 20 min, the prepreg was obtained. Three layers of prepreg were stacked and placed in a 120 °C oven. o C press for 5 min to obtain sample 6.
[0025] Embodiment 8: Based on Embodiment 3, the following treatment is performed: Weigh 100g of epoxy E51 and 40g of isophorone diamine into a 500mL beaker, stir at 100rmp / min for 3h, and then apply them evenly on the surface of polydopamine modified flax fiber cloth using a glue machine. o After curing in an oven at 120 °C for 20 min, take out the prepreg, stack 3 layers of prepreg and put them into the oven at 120 °C. o C press for 5 min to obtain sample 7.
[0026] Embodiment 9: Based on Embodiment 3, the following treatment is performed: Weigh 100g of epoxy E51 and 50g of isophorone diamine into a 500mL beaker, stir and ripen at 100rmp / min for 3h, and then use a glue machine to evenly coat the surface of polydopamine modified flax fiber cloth. o After curing in an oven at 120 °C for 20 min, take out the prepreg, stack 3 layers of prepreg and put them into the oven at 120 °C. oC press for 5 min to obtain sample 8.
[0027] Example 10: (1) Weigh 100 g of sisal fiber cloth and add it to 1 L of aqueous solution containing 15 g of dopamine hydrochloride, add 78.9 mL of 1 mol / L NaOH aqueous solution, and adjust the pH to 7. Add 6 mg of horseradish peroxidase, stir at 50 rpm, set the injection pump feeding speed to 3.6 mL / min, and add 64.5 g of 5% hydrogen peroxide aqueous solution. After the hydrogen peroxide aqueous solution is completely added, continue stirring for 3 min, take out the polydopamine-modified sisal fiber cloth, and simmer at 60 o C, and rolled up to obtain a polydopamine modified sisal fiber cloth.
[0028] (2) Weigh 100g of epoxy E51 and 20g of isophorone diamine into a 500mL beaker, stir and mature at 100rmp / min for 3h, and then use a glue coating machine to evenly coat the surface of the polydopamine-modified sisal fiber cloth obtained in step (1) at 80 o After curing in an oven at 120 °C for 20 min, take out the prepreg and stack three layers of prepreg. o C press for 5 min to obtain sample 9.
[0029] Example 11: (1) Weigh 100 g of jute fiber cloth and add it to 1 L of aqueous solution containing 15 g of dopamine hydrochloride, add 78.9 mL of 1 mol / L NaOH aqueous solution, and adjust the pH to 7. Add 6 mg of horseradish peroxidase, stir at 50 rpm, set the injection pump feeding speed to 3.6 mL / min, and add 64.5 g of 5% hydrogen peroxide aqueous solution. After the hydrogen peroxide aqueous solution is completely added, continue stirring for 3 min, take it out, and heat it at 60 o C, and rolled up to obtain polydopamine modified jute fiber cloth.
[0030] (2) Weigh 100g of epoxy E51 and 20g of isophorone diamine into a 500mL beaker, stir and mature at 100rmp / min for 3h, and then use a glue coating machine to evenly coat the surface of the polydopamine-modified jute fiber cloth obtained in step (1) at 80 o After curing in an oven at 120 °C for 20 min, take out the prepreg and stack three layers of prepreg. o C press for 5 min to obtain sample 10.
[0031] Example 12: (1) Weigh 100 g of ramie fiber cloth and add it to 1 L of aqueous solution containing 15 g of dopamine hydrochloride, add 78.9 mL of 1 mol / L NaOH aqueous solution, and adjust the pH to 7. Add 6 mg of horseradish peroxidase, stir at 50 rpm, set the injection pump feeding speed to 3.6 mL / min, and add 64.5 g of 5% hydrogen peroxide aqueous solution. After the hydrogen peroxide aqueous solution is completely added, continue stirring for 3 min, take it out, and stir at 60 o The fiber was dried under C conditions and rolled up to obtain polydopamine modified ramie fiber cloth.
[0032] Weigh 100g of epoxy E51 and 20g of isophorone diamine into a 500mL beaker, stir and mature at 100rmp / min for 3h, and then use a glue machine to evenly coat the surface of the polydopamine-modified ramie fiber cloth obtained in step (1) at 80 o After curing in an oven at 120 °C for 20 min, take out the prepreg and stack three layers of prepreg. o C press for 5 min to obtain sample 11.
[0033] In summary, the amounts of some raw materials required for samples 1-11 are tabulated, as shown in Table 1: Table 1 Types and usage of natural fiber cloth Dopamine hydrochloride Horseradish peroxidase 5% Hydrogen Peroxide Solution Epoxy E51 Isophorone diamine Sample 1 Flax 100g 5g 2mg 21.5g 100g 20g Sample 2 Flax 100g 10g 4mg 43.0g 100g 20g Sample 3 Flax 100g 15g 6mg 64.5g 100g 20g Sample 4 Flax 100g 20g 8mg 86.0g 100g 20g Sample 5 Flax 100g 15g 6mg 64.5g 100g 10g Sample 6 Flax 100g 15g 6mg 64.5g 100g 30g Sample 7 Flax 100g 15g 6mg 64.5g 100g 40g Sample 8 Flax 100g 15g 6mg 64.5g 100g 50g Sample 9 Sisal 100g 15g 6mg 64.5g 100g 20g Sample 10 Jute 100g 15g 6mg 64.5g 100g 20g Sample 11 Ramie 100g 15g 6mg 64.5g 100g 20g Detection test: (1) Infrared testing is performed in the following manner: Nicolet 6700, ATR mode, test range 4000~400cm -1 .
[0034] (2) The performance of polydopamine-modified natural fiber cloth and its epoxy resin composite material was studied in the following manner: A universal material testing machine of Xiamen Easy Test Instrument Co., Ltd., model: STS100KN, was used to cut samples and conduct tensile tests in accordance with ASTMD638 standard, with a tensile speed of 50 mm / min.
[0035] The universal material testing machine was used to cut samples and perform bending tests according to ASTM D790. Notched impact test specimens were prepared according to GB / T1843 and tested using an Izod impact testing machine according to ASTM D-256.
[0036] The main properties of the polydopamine modified natural fiber cloth reinforced epoxy resin composite material prepared according to the above example are shown in Table 2.
[0037] Table 2 Tensile strength (MPa) Tensile modulus (GPa) Bending strength (MPa) Flexural modulus (GPa) <![CDATA[Impact strength (kJ / m 2 )]]> Sample 1 193 8.11 319 9.06 35.91 Sample 2 253 9.46 398 9.80 46.93 Sample 3 289 9.93 413 10.19 55.63 Sample 4 291 9.85 409 10.08 55.88 Sample 5 269 9.16 365 9.33 59.99 Sample 6 293 10.19 406 10.55 43.61 Sample 7 270 9.51 392 9.95 51.62 Sample 8 209 8.39 361 9.29 39.91 Sample 9 265 9.86 418 10.23 55.93 Sample 10 295 10.05 406 10.06 54.38 Sample 11 289 9.81 426 10.39 53.89 Conclusion: For samples 1-4 obtained in Examples 1-5, the proportions of dopamine, enzyme, and hydrogen peroxide were increased in sequence, and sample 3 had better comprehensive mechanical properties than the other three samples; Examples 6-9 were based on Example 3, and the influence of the content of the curing agent on the mechanical properties of the composite material was studied when other factors remained unchanged; Examples 10-12 were based on Example 3, and the influence of the type of natural fiber cloth on the mechanical properties of the composite material was studied when other factors remained unchanged; Figure 2 The physical pictures of the untreated flax fiber strips and the polydopamine modified flax fiber cloths prepared in Examples 1, 2 and 3 are shown in FIG. Figure 2 It can be seen that the surface of the modified linen strips is brown, which is the color of polydopamine. The higher the proportion of dopamine used in the modification, the darker the color of the surface of the linen fiber strips. Figure 4 is the infrared spectrum of the modified flax fiber cloth obtained in Example 1, compared with Figure 3 Infrared spectrum of linen fiber cloth, we can find that: at 1619cm -1 、1506cm -1 、1054cm -1 The new signal peak at 1281cm -1 and 1107cm -1 The new signal peaks appearing at are the asymmetric and symmetric vibration absorption peaks of the COC bond; these results indicate that a polydopamine coating is formed on the surface of the flax fiber cloth.
[0038] The working principle of the present invention is as follows: under the catalytic action of horseradish peroxidase, the aqueous solution of hydrogen peroxide can oxidize the phenolic hydroxyl group in dopamine to generate phenoloxy free radicals, the phenoloxy free radicals can resonate with the benzene ring to continue to form carbon free radicals, various free radicals can react to form CO or CC bonds, and then form a polydopamine coating on the surface of the natural fiber cloth through covalent bonds and non-covalent bonds. The amino group in the polydopamine coating can react with the epoxy group in the epoxy resin to generate a CN bond, and the formation of chemical bonds improves the interface bonding ability between the fiber and the epoxy resin.
[0039] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0040] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a polydopamine-modified natural fiber cloth, characterized in that: The preparation method is as follows: Take the natural fiber cloth and soak it in water containing dopamine hydrochloride, adjust the pH to 6-8, add horseradish peroxidase, add hydrogen peroxide aqueous solution under stirring conditions, continue to react for 3-5 minutes, take it out, dry and roll it at 30-80°C to obtain polydopamine modified natural fiber cloth.
2. The method for preparing a polydopamine modified natural fiber cloth according to claim 1, characterized in that: The natural fiber cloth is at least one of sisal fiber cloth, jute fiber cloth, linen fiber cloth and ramie fiber cloth, and the moisture content of the natural fiber cloth after drying is less than 0.05%.
3. The method for preparing a polydopamine modified natural fiber cloth according to claim 1, characterized in that: The mass ratio of natural fiber cloth to dopamine hydrochloride is 100:(1-20).
4. The method for preparing a polydopamine modified natural fiber cloth according to claim 1, characterized in that: The mass ratio of horseradish peroxidase to dopamine hydrochloride is 1:(500~5000).
5. The method for preparing a polydopamine modified natural fiber cloth according to claim 1, characterized in that: The hydrogen peroxide aqueous solution is added at a uniform speed using a syringe pump, the stirring speed is 20-100 rpm, and the whole process lasts for 15-20 min; the volume content of hydrogen peroxide in the hydrogen peroxide aqueous solution is 5-10%, and the mass ratio of dopamine hydrochloride to hydrogen peroxide is 1:(0.18-0.25).
6. A method for preparing an epoxy resin composite material, characterized in that: The preparation method is as follows: Weigh an epoxy resin and a curing agent, mix them, mature them for 2 to 5 hours, and then evenly apply them on the surface of the polydopamine-modified natural fiber cloth described in any one of claims 1 to 5, and cure them at 60 to 90° C. for 15 to 30 minutes to obtain a prepreg. A single layer of prepreg or at least two layers of prepreg are stacked, and hot pressed at 110 to 130° C. for 5 to 10 minutes to obtain an epoxy resin composite material.
7. The method for preparing an epoxy resin composite material according to claim 6, characterized in that: The mass ratio of epoxy resin and curing agent is 100:(10~50).
8. The method for preparing an epoxy resin composite material according to claim 6, characterized in that: The epoxy resin is epoxy E51 or hydrogenated epoxy E51.
9. The method for preparing an epoxy resin composite material according to claim 6, characterized in that: The curing agent is an alicyclic amine or aromatic amine curing agent.
Citation Information
Patent Citations
Preparation method of surface-treated natural fiber fabric reinforced resin-based laminated composite material
CN110774614A
Super-hydrophobic and antibacterial natural cellulose fabric and preparation method thereof
CN112900102A
Hyaluronic acid / tannic acid / carbon microsphere injectable hydrogel for promoting wound healing and preparation method of hyaluronic acid / tannic acid / carbon microsphere injectable hydrogel
CN118045224A
Surface-modified aramid fiber and preparation method therefor
US20210222358A1