Flexible substrate, flexible solar cell device and preparation method thereof
By forming a fluorinated graphene-doped thermal smooth layer on the paper-based substrate, the problems of environmental pollution and working stability of flexible solar cells are solved, and efficient thermal conductivity and performance improvements are achieved.
Patent Information
- Application Number
- CN202310669009.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
The flexible substrates of existing flexible solar cells have a high pollution to the environment, low operating performance of the device, and are prone to overheating, resulting in poor working stability.
A paper-based substrate is used and a thermally conductive smoothing layer is formed on its surface, which is made of biodegradable materials doped with fluorinated graphene, including furandicarboxylic acid-based polyester and fluorinated graphene, fluorinated graphene The degree of fluorination of ene is C/F=1, and the doping mass percentage is 40% to 90% by weight.
The green degradability of flexible solar cells is realized, the surface roughness of paper-based substrate is reduced, the thermal conductivity is improved, the working performance and stability of the device is improved, and environmental pollution and the risk of short circuit between the anode and cathode layers is avoided. .
Smart Images

Figure CN119095459A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of flexible devices, and more specifically, to a flexible substrate, a method for preparing a flexible substrate, and a flexible solar cell device. Background Art
[0002] A solar cell is a clean energy device that directly converts light energy into electrical energy through the photoelectric effect or the photochemical effect. Currently, the commonly used solar cells on the market are silicon solar cells, which have a high conversion efficiency, but have problems such as complex processes, high costs, and high energy consumption in the production process. Therefore, flexible solar cells are considered to be the main application direction of solar cells at present due to their light texture, flexibility, low cost, and large-area preparation characteristics.
[0003] Existing flexible solar cells usually use difficult-to-degrade plastic substrates as flexible substrates. After the battery is discarded, the plastic substrate causes environmental pollution. At the same time, the surface roughness of this flexible substrate can easily affect the performance of optoelectronic devices. Conventional solutions usually use an organic smoothing layer to improve the surface roughness of the flexible substrate. Due to its own insulation properties and difficult-to-degrade properties, in the process of flexible solar cells converting solar energy into electrical energy, the excessive accumulation of heat affects the working stability of the battery. At the same time, the organic smoothing layer will cause environmental pollution after the battery is discarded. Summary of the invention
[0004] The technical problem to be solved by the embodiments of the present application is that the flexible substrate of the existing flexible solar cell has a great pollution to the environment, the device has low working performance, and is prone to overheating, resulting in poor working stability.
[0005] In order to solve the above technical problems, the present application provides a flexible substrate, which adopts the following technical solution:
[0006] Paper-based substrate;
[0007] A thermally conductive smoothing layer is disposed on the paper-based substrate, wherein the thermally conductive smoothing layer comprises a biodegradable material doped with fluorinated graphene.
[0008] Furthermore, the degree of fluorination of the fluorinated graphene is C / F=1.
[0009] Furthermore, the mass percentage of the fluorinated graphene doping is 40wt% to 90wt%.
[0010] Further, the biodegradable material includes furan dihydroxy acid polyester (FDCA) and polyhydroxy fatty acid (PHA);
[0011] Optionally, the furan dihydroxy acid-based polyester includes polyfuran dicarboxylic acid diethanol ester (PEF), p-xylene dimer (PCF), and high-toughness furan copolyester (PECF);
[0012] Optionally, the polyhydroxyalkanoic acid includes polylactic acid (PLA), polyglycolic acid (PGA), polyhydroxyhexanoate (PHHx), polyhydroxyvalerate (PHV), polyhydroxyoctanoate (PHO), polybutylene glycol succinate (PBS).
[0013] Furthermore, the paper-based substrate is selected from at least one of stone paper, printing paper, filter paper, coated paper, sulfuric acid paper, photographic paper, copy paper, glossy paper, art adhesive paper, and graphite paper.
[0014] In order to solve the above technical problems, the present application also provides a method for preparing a flexible substrate, which adopts the following technical solution:
[0015] A method for preparing a flexible substrate, used for preparing the above-mentioned flexible substrate, comprises the following steps:
[0016] providing a paper-based substrate;
[0017] placing a thermally conductive smoothing layer solution on the paper-based substrate to form a thermally conductive smoothing layer;
[0018] Wherein, the thermally conductive smoothing layer solution comprises a biodegradable material doped with fluorinated graphene.
[0019] Furthermore, the thermally conductive smoothing layer solution is prepared by the following steps:
[0020] Adding graphite fluoride to a hexafluoroisopropanol solution to form a mixed solution, subjecting the solution to ultrasonic treatment, and then subjecting the solution to centrifugal treatment, removing the precipitate, and obtaining a thermal conductor, wherein the degree of fluorination of the thermal conductor is C / F=1;
[0021] Adding biodegradable materials to the thermal conductor to form a mixed solution, and performing ultrasonic treatment to form a thermally conductive smooth layer solution, wherein the mass percentage of the thermal conductor doped is 40wt% to 90wt%;
[0022] Wherein, the biodegradable material includes an energetic dicarboxylic acid-based polyester and a polyhydroxyalkanoic acid (PHA);
[0023] Optionally, the furan dicarboxylic acid-based polyester includes polyethylene furandicarboxylate (PEF), p-xylene dimer (PCF), and high-toughness furan copolyester (PECF);
[0024] Optionally, the polyhydroxyalkanoic acid includes polylactic acid (PLA), polyglycolic acid (PGA), polyhydroxyhexanoate (PHHx), polyhydroxyvalerate (PHV), polyhydroxyoctanoate (PHO), and polybutylene glycol succinate (PBS).
[0025] Furthermore, before adding the biodegradable material into the thermal conductive agent to form a mixed solution, the following steps are also included:
[0026] The thermal conductor is concentrated, and then the biodegradable material is added to the concentrated thermal conductor to form a mixed solution.
[0027] In order to solve the above technical problems, the embodiment of the present application further provides a flexible solar cell device, which adopts the following technical solution:
[0028] A flexible solar cell device, comprising:
[0029] A flexible substrate, wherein the flexible substrate is the above-mentioned flexible substrate, or is prepared by the above-mentioned method for preparing the flexible substrate;
[0030] The optoelectronic device assembly layer is arranged on the thermally conductive smooth layer of the flexible substrate.
[0031] Furthermore, the optoelectronic device combination layer includes:
[0032] An anode layer and a cathode layer are arranged opposite to each other;
[0033] a photoactive layer disposed between the anode layer and the cathode layer;
[0034] An electron transport layer, disposed between the photoactive layer and the cathode layer;
[0035] A hole transport layer, which is disposed between the photoactive layer and the anode layer;
[0036] And / or, the material of the anode layer and the cathode layer is selected from at least one of a metal material, a carbon material and a metal oxide, wherein the metal material is selected from at least one of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material is selected from at least one of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes a doped or undoped metal oxide, including at least one of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, and the composite electrode includes at least one of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2;
[0037] And / or, the material of the electron transport layer is selected from oxides, fullerenes and their derivatives, graphene and its derivatives, low work function metals, polyfluorene derivatives such as, conjugated polyelectrolytes, NDI derivatives, perylene diimide (PDI) derivatives, naphthalene diimide-like molecules NDIO, star-shaped conjugated small molecule electrolyte interface materials TzPyBr, black scale (BP), Mxenes, metal oxides, doped metal oxides, II-VI semiconductor materials, III-V semiconductor materials and I-III-VI semiconductor materials, the low work function metal is selected from at least one of Ca and Ba; the polyfluorene derivative is selected from at least one of PFN and PFNBr; the NDI derivative is selected from PDNI-F3 N, PDNI-F3N-Br; the metal oxide is selected from at least one of ZnO, TiO2, SnO2; the perylene diimide (PDI) derivative is selected from at least one of PDIN, PDINO, PDINN; the metal oxide in the doped metal oxide is selected from at least one of ZnO, TiO2, SnO2, the doping element is selected from at least one of Al, Mg, Li, In, Ga, the II-VI semiconductor material is selected from at least one of ZnS, ZnSe, CdS; the III-V semiconductor material is selected from at least one of InP and GaP; the I-III-VI semiconductor material is selected from at least one of CuInS and CuGaS;
[0038] And / or, the material of the photoactive layer is selected from at least one of an organic photovoltaic material, a perovskite photovoltaic material or a dye-sensitized photovoltaic material;
[0039] And / or, the material of the hole transport layer is selected from Spiro-OMeTAD, PEDOT:PSS, PTAA, P3HT, CuSCN, molybdenum oxide, graphene oxide (GO), CuI, 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-bis(3 -methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), polyaniline, polypyrrole , poly(p-phenylene vinylene), poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] and poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, poly(N-vinylcarbazole) and its Derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine, spiro NPB, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO.
[0040] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0041] The present application uses a paper-based substrate as a flexible substrate and a furan dicarboxylic acid-based polyester material as the main material of a thermally conductive smooth layer, so that the flexible solar cell device has green and degradable properties and avoids pollution to the environment; a thermally conductive smooth layer is formed on the surface of the paper-based substrate to reduce the surface roughness of the paper-based substrate, so as to facilitate the preparation of subsequent photovoltaic device combination layers and improve the performance of the device; in addition, the thermally conductive smooth layer has good water and oxygen barrier properties, which can prevent water and oxygen from corroding the device and improve the stability of the device; by doping a thermal conductive agent in the furan dicarboxylic acid-based polyester material, the thermal conductivity of the device is improved and the working stability of the device is improved;
[0042] The present application forms a thermally conductive smoothing layer on a paper-based substrate to reduce the surface roughness of the paper-based substrate and improve the thermal conductivity, thereby improving the working performance and working stability of the flexible solar cell device. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the scheme of the present application, a brief introduction is given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0044] Figure 1 is a schematic structural diagram of a flexible substrate according to an embodiment of the present application;
[0045] Figure 2 is a schematic structural diagram of a flexible solar cell device according to an embodiment of the present application;
[0046] Figure 3 is a flow chart of a method for preparing a flexible substrate according to an embodiment of the present application;
[0047] Figure 4 is a flow chart of a method for preparing a flexible solar cell device according to an embodiment of the present application;
[0048] Figure 5 for Figure 4 A flowchart of a specific implementation of step S20;
[0049] Figure 6 for Figure 4 A flowchart of a specific implementation of step S30.
[0050] Reference numerals:
[0051] 1. Paper-based substrate; 2. Thermally conductive smoothing layer; 3. Photoelectric device assembly layer; 31. Cathode layer; 32. Electron transport layer; 33. Photoactive layer; 34. Hole transport layer; 35. Anode layer. DETAILED DESCRIPTION
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.
[0053] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0054] For examples of the flexible substrate of this application, please refer to Figure 1 As shown, the present application provides a flexible substrate, including: a paper-based substrate 1 and a thermally conductive smoothing layer 2 .
[0055] A thermally conductive smoothing layer is disposed on the paper-based substrate, and the thermally conductive smoothing layer includes a biodegradable material doped with fluorinated graphene. In the present embodiment, the film thickness of the thermally conductive smoothing layer 2 is 5 μm to 500 μm to adapt to paper-based substrates 1 with different surface roughnesses to reduce the surface roughness of the paper-based substrate 1.
[0056] In this embodiment, the film thickness of the thermally conductive smoothing layer 2 can be 5 μm, 10 μm, 20 μm, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, etc.
[0057] The flexible solar cell device provided in the embodiment of the present application adopts a paper-based substrate 1 as a flexible substrate, and adopts a furan dicarboxylic acid-based polyester material as the main component of the thermally conductive smooth layer 2, so that the flexible solar cell device has a degradable characteristic and avoids polluting the environment. By arranging the thermally conductive smooth layer 2 on the paper-based substrate 1, the sharp protrusions on the paper-based substrate 1 are filled with the thermally conductive smooth layer 2, thereby reducing the surface roughness of the paper-based substrate 1, so as to avoid the situation in which the anode layer is directly in contact with the cathode layer after the protrusions on the surface of the paper-based substrate cause the anode layer to be arched during the subsequent preparation process of the photovoltaic device combination layer 3, thereby avoiding the risk of short circuit between the anode layer and the cathode layer, so as to improve the performance of the flexible solar cell device.
[0058] In this embodiment, the fluorinated graphene has a fluorination degree of C / F=1, that is, perfluorinated graphene.
[0059] In the embodiment of the present application, fluorinated graphene is used as a thermal conductor. Compared with graphite and graphene materials, the selection of fluorinated graphene can not only make the thermally conductive smooth layer 2 have good thermal conductivity, but also have good insulation, so as to avoid short circuit of the anode layer or cathode layer of the photovoltaic device combination layer 3; in some embodiments, the thermal conductivity of fluorinated graphene decreases with the increase of the fluorination degree of graphene, but when the fluorination degree of fluorinated graphene reaches C / F=1, the thermal conductivity of fluorinated graphene will increase to 35% of graphene. With the increase of fluorination degree, fluorinated graphene will be transformed from a conductor to an insulator. When the fluorination degree reaches C / F=1, the conductivity of fluorinated graphene reaches a minimum value and the thermal conductivity reaches a maximum value. Therefore, compared with non-perfluorinated graphene, the use of perfluorinated graphene as a thermal conductor in this embodiment improves the thermal conductivity and electrical insulation of the thermally conductive smooth layer 2, thereby improving the working performance of the flexible solar cell device.
[0060] In some embodiments, the mass percentage of the fluorinated graphene doping is 40wt% to 90wt%, for example, 40wt%, 50wt%, 60wt%, 70wt%, 80wt%, 90wt%. In this embodiment, 20ml of a layered fluorinated graphene suspension with a concentration of 45mg / ml was added with 1g of PEF material, and ultrasonic treatment was performed for 30min to prepare a fluorinated graphene with a doping mass percentage of 90wt%.
[0061] Combined with the setting of the flexible solar cell device, the thermally conductive smooth layer 2 of this embodiment can obtain a larger thermal conductivity and resistivity. When the optoelectronic device combination layer is set on the thermally conductive smooth layer 2, a short circuit between the anode layer and the cathode layer is avoided, and heat can be quickly transferred from the thermally conductive smooth layer 2, thereby improving the working performance of the flexible solar cell device and extending the service life of the flexible solar cell device.
[0062] In some embodiments, the biodegradable material includes furan dicarboxylic acid-based polyester and polyhydroxy fatty acid (PHA). The thermally conductive smoothing layer 2 may be selected from at least one of polyethylene furan dicarboxylate (PEF), p-xylene dimer (PCF), and high-toughness furan copolyester (PECF). Optionally, the polyhydroxy fatty acid includes polylactic acid (PLA), polyhydroxyacetic acid (PGA), polyhydroxycaproate (PHHx), polyhydroxyvalerate (PHV), polyhydroxyoctanoate (PHO), and polybutylene glycol succinate (PBS). In this embodiment, the biodegradable material in the thermally conductive smoothing layer is selected from the furan dicarboxylic acid-based polyester material and is made of PEF material. The use of PEF material can achieve the function of reducing the roughness of the paper-based substrate 1. In addition, the PEF material is a bio-based material composed of 100% renewable forestry and agricultural waste raw materials, so it can be degraded by recycling or incineration, thereby improving the degradable characteristics of the flexible solar cell device and avoiding the pollution of the environment by the discarded flexible solar cell device.
[0063] In some embodiments, the paper-based substrate 1 is selected from at least one of stone paper, printing paper, filter paper, coated paper, sulfuric acid paper, photographic paper, copy paper, glossy paper, art adhesive paper, and graphite paper. In this embodiment, the paper-based substrate 1 is glossy paper.
[0064] The embodiment of the present application adopts a paper-based substrate 1 as a flexible substrate. Due to the degradable nature of the paper-based substrate 1 itself, it can be degraded by recycling or incineration, thereby improving the degradable characteristics of the flexible solar cell device and avoiding environmental pollution caused by discarded flexible solar cell devices. In addition, the use of the paper-based substrate 1 also has the advantages of simplifying the production process, being compatible with large-scale production and reducing production costs. In this embodiment, the paper-based substrate 1 uses glossy paper, which has a better surface fineness, a lower surface roughness, and is not prone to wrinkles, so that the thermal conductive smoothing layer 2 and the optoelectronic device combination layer 3 are arranged on the paper-based substrate 1, thereby improving the working stability of the device and reducing production costs.
[0065] Embodiment of the method for preparing the flexible device of the present application
[0066] See also Figure 3 As shown, the present application provides a method for preparing a flexible device, comprising the following steps:
[0067] Step S1, providing a paper-based substrate.
[0068] In some embodiments, the paper substrate is selected from at least one of stone paper, printing paper, filter paper, coated paper, sulfuric acid paper, photographic paper, copy paper, glossy paper, art adhesive paper, and graphite paper. In this embodiment, the paper-based substrate is glossy paper.
[0069] Step S2, disposing a thermally conductive smoothing layer solution on the paper-based substrate to form a thermally conductive smoothing layer; wherein the thermally conductive smoothing layer solution comprises a biodegradable material doped with fluorinated graphene.
[0070] In some embodiments, the thermally conductive smoothing layer solution is prepared by the following steps:
[0071] Graphite fluoride is added to a hexafluoroisopropanol solution to form a mixed solution, and ultrasonic treatment is performed, followed by centrifugal treatment. After the precipitate is removed, a thermal conductor is obtained, wherein the degree of fluorination of the thermal conductor is C / F=1.
[0072] In this embodiment, the fluorinated graphite is commercially available graphite fluoride powder, which is added to a hexafluoroisopropanol solution to form a mixed solution, and then subjected to ultrasonic treatment for at least 24 hours to exfoliate the fluorinated graphite dissolved in the hexafluoroisopropanol solution into layered fluorinated graphene.
[0073] In this embodiment, the mixed solution after the ultrasonic treatment is centrifuged at a rotation speed of 3000 rpm for 10 minutes to remove the unexfoliated graphite fluoride precipitate to form a layered graphene fluoride suspension.
[0074] In this embodiment, the thermal conductor obtained in step S203 is further processed, and the filtered layered fluorinated graphene suspension is concentrated to form a concentrated thermal conductor. Specifically, the mixed solution is ultrasonically treated while maintaining an ambient temperature of above 60°C, so that the concentration of the layered fluorinated graphene suspension is concentrated to 45 mg / ml, and the degree of fluorination of the layered fluorinated graphene suspension is C / F=1.
[0075] The layered fluorinated graphene suspension is concentrated so that a thermally conductive smoothing layer solution with a high doping ratio can be obtained after subsequent mixing.
[0076] The biodegradable material is added into the thermal conductive agent to form a mixed solution, and ultrasonic treatment is performed to form a thermal conductive smoothing layer solution.
[0077] In some embodiments, the mass percentage of the thermal conductor doped is 40 wt % to 90 wt %.
[0078] The biodegradable materials include furan dicarboxylic acid-based polyesters and polyhydroxyalkanoic acids (PHA).
[0079] Optionally, the furan dicarboxylic acid-based polyester includes polyethylene furandicarboxylate (PEF), paraxylene dimer (PCF), and high-tenacity furan copolyester (PECF).
[0080] Optionally, the polyhydroxyalkanoic acid includes polylactic acid (PLA), polyglycolic acid (PGA), polyhydroxyhexanoate (PHHx), polyhydroxyvalerate (PHV), polyhydroxyoctanoate (PHO), and polybutylene glycol succinate (PBS).
[0081] In this embodiment, 20 ml of the above-mentioned layered fluorinated graphene suspension with a concentration of 45 mg / ml is taken as a thermal conductor, 1 g of PEF material is added to the thermal conductor, and ultrasonic treatment is performed for more than 30 minutes to form a PEF solution doped with fluorinated graphene, wherein the doping mass percentage of the fluorinated graphene is 90 wt%.
[0082] The method for preparing a flexible device provided in the embodiment of the present application can reduce the surface roughness of the paper-based substrate and improve the thermal conductivity by preparing a thermally conductive smooth layer on the paper-based substrate, thereby improving the working performance and working stability of the flexible solar cell device and facilitating the subsequent further preparation of flexible solar cells.
[0083] Embodiments of the flexible solar cell device of the present application
[0084] See also Figure 2 As shown, the present application provides a flexible solar cell device, comprising: a paper-based substrate 1, a thermally conductive smoothing layer 2, and a photovoltaic device combination layer 3.
[0085] The thermally conductive smoothing layer 2 is arranged on the paper-based substrate 1, and the thermally conductive smoothing layer 2 includes a biodegradable material doped with fluorinated graphene. In the present embodiment, the film thickness of the thermally conductive smoothing layer 2 is 5 μm to 500 μm to adapt to the paper-based substrates 1 with different surface roughnesses, so as to reduce the surface roughness of the paper-based substrate 1. Due to the protrusions on the upper surface of the paper-based substrate 1, the anode layer in the optoelectronic combination device layer protrudes upward and directly contacts the cathode layer, thereby causing a short circuit. Therefore, in the present embodiment, the thermally conductive smoothing layer 2 is arranged on the surface of the paper-based substrate to avoid direct contact between the anode layer and the cathode layer, thereby avoiding a short circuit between the anode and the cathode, thereby improving the performance of the optoelectronic device combination layer 3.
[0086] In this embodiment, the film thickness of the thermally conductive smoothing layer 2 can be 5 μm, 10 μm, 20 μm, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, etc.
[0087] The photovoltaic device assembly layer 3 is arranged on the thermally conductive smooth layer 2, and the photovoltaic device assembly layer 3 is used to convert solar energy into electrical energy.
[0088] The flexible solar cell device provided in the embodiment of the present application adopts a paper-based substrate 1 as a flexible substrate, and adopts a furan dicarboxylic acid-based polyester material as the main component of the thermally conductive smooth layer 2, so that the flexible solar cell device has a degradable characteristic and avoids polluting the environment. Due to the high surface roughness of the paper-based substrate 1, the anode layer located on the paper-based substrate 1 is arched due to the protrusions on the surface of the paper-based substrate, and the arched anode layer is in direct contact with the cathode layer, thereby causing a short circuit between the anode layer and the cathode layer. In this embodiment, a thermally conductive smooth layer 2 is arranged on the paper-based substrate 1, and the sharp protrusions on the paper-based substrate 1 are filled with the thermally conductive smooth layer 2, thereby reducing the surface roughness of the paper-based substrate 1, so as to avoid the arching of the anode layer and the direct contact with the cathode layer in the subsequent preparation process of the photovoltaic device combination layer 3, thereby avoiding the risk of short circuit between the anode layer and the cathode layer, and improving the performance of the flexible solar cell device. In addition, by doping fluorinated graphene into the biodegradable material, not only the water and oxygen barrier property of the thermally conductive smooth layer 2 is improved, but also the thermally conductive smooth layer 2 has thermal conductivity. In the process of the flexible solar cell device converting solar energy into electrical energy, heat can be transferred to avoid excessive heat accumulation caused by exposure, thereby improving the working performance and working stability of the flexible solar cell device and extending the service life of the flexible solar cell device.
[0089] In some embodiments, the optoelectronic device assembly layer 3 is formed on the thermally conductive smoothing layer 2, and includes:
[0090] An anode layer 35 and a cathode layer 31 are arranged opposite to each other;
[0091] A photoactive layer 33 disposed between the anode layer 35 and the cathode layer 31;
[0092] An electron transport layer 32, which is disposed between the photoactive layer 33 and the cathode layer 31;
[0093] The hole transport layer 34 is disposed between the photoactive layer 33 and the anode layer 35 .
[0094] In this embodiment, the flexible solar cell device is an inverted cell device, and the photoelectric device combination layer 3 includes: a cathode layer 31, an anode layer 35, and an electron transport layer 32, a photoactive layer 33 and a hole transport layer 34 stacked from bottom to top between the anode layer 35 and the cathode layer 31. In other embodiments, the flexible solar cell device can also be an upright cell device, and the photoelectric device combination layer 3 includes: an anode layer 35, a cathode layer 31, and a hole transport layer 34, a photoactive layer 33 and an electron transport layer 32 stacked from bottom to top between the anode layer 35 and the cathode layer 31.
[0095] In this embodiment, the cathode layer 31 has a film thickness of 10 nm to 500 nm, for example, 10 nm, 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.
[0096] In this embodiment, the film thickness of the electron transport layer 32 is 1 nm to 500 nm, for example, 1 nm, 5 nm, 10 nm, 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.
[0097] In this embodiment, the film thickness of the photoactive layer 33 is 20 nm to 2000 nm, for example, 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.
[0098] In this embodiment, the hole transport layer 34 has a film thickness of 10 nm to 500 nm, for example, 10 nm, 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.
[0099] In this embodiment, the anode layer 35 has a film thickness of 10 nm to 500 nm, for example, 10 nm, 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.
[0100] By setting a photoactive layer 33 between the electron transport layer 32 and the hole transport layer 34, when the flexible solar cell device is irradiated by sunlight, the light is incident on the photoactive layer 33, and the electrons and holes are excited in the photoactive layer 33. When the electrons in the photoactive layer 33 move, the electrons and holes are separated. Therefore, the carriers generated by light are separated into electrons and holes and move toward the electron transport layer 32 and the hole transport layer 34 respectively, generating electricity, thereby realizing the conversion of solar energy into light energy; the heat generated by sunlight irradiating the flexible solar cell device is transferred through the thermally conductive smoothing layer 2 to avoid the heat being concentrated in the optoelectronic device combination layer 3.
[0101] In some embodiments, the material of the anode layer 35 and the cathode layer 31 is selected from at least one of a metal material, a carbon material and a metal oxide, wherein the metal material is selected from at least one of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material is selected from at least one of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes doped or undoped metal oxides, including at least one of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, and the composite electrode includes at least one of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2.
[0102] In some embodiments, the material of the electron transport layer 32 is selected from oxides, fullerenes and their derivatives, graphene and its derivatives, low work function metals, polyfluorene derivatives such as, conjugated polyelectrolytes, NDI derivatives, perylene diimide (PDI) derivatives, naphthalene diimide-like molecules NDIO, star-shaped conjugated small molecule electrolyte interface materials TzPyBr, black scale (BP), Mxenes, metal oxides, doped metal oxides, II-VI semiconductor materials, III-V semiconductor materials and I-III-VI semiconductor materials. At least one of the low work function metal is selected from at least one of Ca and Ba; the polyfluorene derivative is selected from at least one of PFN and PFNBr; the NDI derivative is selected from PDNI -F3N, PDNI-F3N-Br; the metal oxide is selected from at least one of ZnO, TiO2, SnO2; the perylene diimide (PDI) derivative is selected from at least one of PDIN, PDINO, PDINN; the metal oxide in the doped metal oxide is selected from at least one of ZnO, TiO2, SnO2, the doping element is selected from at least one of Al, Mg, Li, In, Ga, the II-VI group semiconductor material is selected from at least one of ZnS, ZnSe, CdS; the III-V group semiconductor material is selected from at least one of InP, GaP; the I-III-VI group semiconductor material is selected from at least one of CuInS, CuGaS.
[0103] In some embodiments, the material of the photoactive layer 33 is selected from at least one of an organic photovoltaic material, a perovskite photovoltaic material, or a dye-sensitized photovoltaic material. In this embodiment, the photoactive layer 33 uses an organic photovoltaic material, which is composed of a junction structure of an electron donor and an electron acceptor material. When light is incident on the photoactive layer 33, electrons and holes are excited in the electron donor, and separation of electrons and holes occurs when the electrons move to the electron acceptor. Therefore, the carriers generated by light are separated into electrons-holes, and then generate electricity when they move to an external circuit.
[0104] In some embodiments, the material of the hole transport layer 34 is selected from Spiro-OMeTAD, PEDOT:PSS, PTAA, P3HT, CuSCN, molybdenum oxide, graphene oxide (GO), CuI, 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N '-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), polyaniline, Polypyrrole, poly(p-phenylene vinylene), poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] and poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraaryl benzidine, PEDOT:PSS and its derivatives, poly(N-vinyl carbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine, spiro NPB, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO.
[0105] Embodiment of the method for preparing the flexible solar cell device of the present application
[0106] See also Figure 4 As shown, the present application provides a method for preparing a flexible solar cell device, which is used to prepare the flexible solar cell device as described above, comprising the following steps:
[0107] Step S10, providing a paper-based substrate.
[0108] In some embodiments, the paper substrate is selected from at least one of stone paper, printing paper, filter paper, coated paper, sulfuric acid paper, photographic paper, copy paper, glossy paper, art adhesive paper, and graphite paper. In this embodiment, the paper-based substrate is glossy paper.
[0109] Step S20, disposing a thermally conductive smoothing layer solution on the paper-based substrate to form a thermally conductive smoothing layer.
[0110] See also Figure 5 As shown, in some embodiments, the thermally conductive smoothing layer solution is prepared by the following steps:
[0111] Step S201, adding graphite fluoride into a hexafluoroisopropanol solution to form a mixed solution, and performing ultrasonic treatment.
[0112] In this embodiment, the fluorinated graphite is commercially available graphite fluoride powder, which is added to a hexafluoroisopropanol solution to form a mixed solution, and then subjected to ultrasonic treatment for at least 24 hours to exfoliate the fluorinated graphite dissolved in the hexafluoroisopropanol solution into layered fluorinated graphene.
[0113] Step S202, centrifuging the mixed solution after the ultrasonic treatment.
[0114] In this embodiment, the mixed solution after the ultrasonic treatment is centrifuged at a rotation speed of 3000 rpm for 10 minutes to remove the unexfoliated graphite fluoride precipitate to form a layered graphene fluoride suspension.
[0115] Step S203, filtering the mixed solution after the centrifugal treatment to remove the precipitate to obtain a thermal conductor.
[0116] In this embodiment, the thermal conductor obtained in step S203 is further processed, and the layered fluorinated graphene suspension obtained after filtering and precipitation is concentrated to form a concentrated thermal conductor. Specifically, the mixed solution is ultrasonically treated while maintaining the ambient temperature above 60°C, so that the concentration of the layered fluorinated graphene suspension is concentrated to 45 mg / ml, and the degree of fluorination of the layered fluorinated graphene suspension is C / F=1.
[0117] The layered fluorinated graphene suspension is concentrated so that a thermally conductive smoothing layer solution with a high doping ratio can be obtained after subsequent mixing.
[0118] Step S204: adding the biodegradable material into the thermal conductive agent to form a mixed solution, and performing ultrasonic treatment to form a thermal conductive smoothing layer solution.
[0119] In this embodiment, 20 ml of the above-mentioned layered fluorinated graphene suspension with a concentration of 45 mg / ml is taken as a thermal conductor, 1 g of PEF material is added to the thermal conductor, and ultrasonic treatment is performed for more than 30 minutes to form a PEF solution doped with fluorinated graphene, wherein the doping mass percentage of the fluorinated graphene is 90 wt%.
[0120] Please review Figure 4 As shown, in step S30, a photoelectric device assembly layer is formed on the thermally conductive smoothing layer.
[0121] See also Figure 6 As shown, in some embodiments, the flexible solar cell device is an inverted device, and the step S30 forms a photovoltaic device combination layer on the thermally conductive smooth layer, specifically comprising the following steps:
[0122] Step S301, forming a cathode layer on the thermally conductive smooth layer.
[0123] In this embodiment, the cathode layer adopts a PEDOT:PSS (PH1000) solution, wherein the PEDOT:PSS (PH1000) solution is modified by adding DMSO with a volume ratio of 5 vol%, and filtering with a polytetrafluoroethylene filter with a specification of 0.45 μm. The cathode layer is formed on the thermally conductive smoothing layer by a solution method, and the film thickness of the cathode layer is 10nm to 500nm.
[0124] Step S302: forming an electron transport layer on the cathode layer.
[0125] In this embodiment, the electron transport layer is formed on the cathode layer by a solution method using a ZnO ethanol solution with a concentration of 20 mg / mL. The film thickness of the electron transport layer is 1 nm to 500 nm.
[0126] Step S303, forming a photoactive layer on the electron transport layer.
[0127] In this embodiment, the photoactive layer adopts an organic photoactive solution, wherein the organic photoactive solution is prepared by adding 10 mg PTB7-th and 15 mg PC71BM to 1 mL chlorobenzene / 1,8-diiodooctane (volume ratio of 97:3) solvent, and heating and stirring at 80°C for 12 hours. A photoactive layer is formed on the electron transport layer by a solution method, and the film thickness of the photoactive layer is 20 nm to 2000 nm.
[0128] Step S304, forming a hole transport layer on the photoactive layer.
[0129] In this embodiment, the hole transport layer is made of MoO3 and is formed on the photoactive layer by evaporation. The film thickness of the hole transport layer is 10 nm to 500 nm.
[0130] Step S305, forming an anode layer on the hole transport layer.
[0131] In this embodiment, the anode layer is made of Ag and is formed on the hole transport layer by evaporation. The thickness of the anode layer is 10 nm to 500 nm.
[0132] In this embodiment, the solution method includes but is not limited to spin coating, printing, scraping, dip pulling, immersion, spraying, roll coating, casting, slit coating, and strip coating; the evaporation method can be a chemical method or a physical coating method, wherein the chemical method includes but is not limited to one or more of chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition, and co-precipitation; the physical coating method includes but is not limited to one or more of thermal evaporation coating, electron beam evaporation coating, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition, and pulsed laser deposition.
[0133] The method for preparing a flexible solar cell device provided in an embodiment of the present application simplifies the device preparation process and has good production continuity by sequentially preparing a thermally conductive smoothing layer and a photovoltaic device combination layer on a paper-based substrate. At the same time, the thermally conductive smoothing layer is arranged between the paper-based substrate and the photovoltaic device combination layer, which can reduce the surface roughness of the paper-based substrate and improve the thermal conductivity, thereby improving the working performance and working stability of the flexible solar cell device.
[0134] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present invention are described in detail as follows:
[0135] Example 1
[0136] ⑴Cut the glossy paper into a square with a side length of 4 cm.
[0137] ⑵ Add 2g of commercial graphite fluoride powder to 500ml of hexafluoroisopropanol and perform ultrasonic treatment for at least 24h to exfoliate the graphite fluoride into layered graphite fluoride; and centrifuge the layered graphite fluoride suspension at a speed of 3000rpm for 10min to remove the unexfoliated graphite fluoride precipitate; maintain the ambient temperature above 60°C, perform ultrasonic treatment on the layered graphite fluoride suspension for at least 10min, and concentrate the layered graphite fluoride suspension to a concentration of 45mg / ml; take 20ml of the above-mentioned layered graphite fluoride suspension with a concentration of 45mg / ml, add 1g of PEF material, and perform ultrasonic treatment for at least 30min to complete the preparation of the thermally conductive smoothing layer solution, wherein the doping mass percentage of the fluorinated graphene in the thermally conductive smoothing layer solution is the mass of fluorinated graphene: the mass of PEF = 45mg / ml*20ml: 1000mg = 90wt%.
[0138] ⑶ A 1 mm thick thermally conductive smoothing layer solution was coated on the cut glossy paper, and then annealed on a hot plate at 50° C. for 3 h to prepare a thermally conductive smoothing layer. In this embodiment, the film thickness of the thermally conductive smoothing layer is 150 μm.
[0139] Example 2
[0140] The difference between Example 2 and Example 1 is that in step (2), the doping mass percentage of fluorinated graphene in the thermally conductive smoothing layer solution is 40wt%.
[0141] Example 3
[0142] The difference between Example 3 and Example 1 is that in step (2), the doping mass percentage of fluorinated graphene in the thermally conductive smoothing layer solution is 50wt%.
[0143] Example 4
[0144] The difference between Example 4 and Example 1 is that in step (2), the doping mass percentage of fluorinated graphene in the thermally conductive smoothing layer solution is 60wt%.
[0145] Example 5
[0146] The difference between Example 5 and Example 1 is that in step (2), the doping mass percentage of the fluorinated graphene in the thermally conductive smoothing layer solution is 70 wt %.
[0147] Example 6
[0148] The difference between Example 6 and Example 1 is that in step (2), the doping mass percentage of the fluorinated graphene in the thermally conductive smoothing layer solution is 80wt%.
[0149] Comparative Example 1
[0150] The difference between Comparative Example 1 and Example 1 is that after the glossy paper is cut in step (1), step (3) is directly performed to spin-coat the glossy paper with the PEF solution, followed by annealing on a hot plate at 50° C. for 3 h to prepare a thermally conductive smoothing layer.
[0151] Application Example 1
[0152] (4) Spin-coat a PEDOT:PSS (PH1000) solution on the thermally conductive smooth layer obtained in Example 1, and then dry at 100° C. for 30 min to prepare a cathode layer, wherein the cathode layer has a film thickness of 100 nm.
[0153] (5) Spin-coat a ZnO ethanol solution with a concentration of 20 mg / mL on the cathode layer, and then anneal on a hot plate at 170° C. for 10 min to prepare an electron transport layer, wherein the film thickness of the electron transport layer is 30 nm.
[0154] (6) Spin coating an organic photoactive solution on the electron transport layer, and then annealing on a hot plate at 110° C. for 10 min to prepare a photoactive layer, wherein the film thickness of the photoactive layer is 90 nm.
[0155] ⑺Place the glossy paper treated in step ⑹ in a vapor deposition chamber, reduce the air pressure of the vacuum system to less than 10-6mbar, and vapor-deposit MoO3 on the photoactive layer to prepare a hole transport layer, wherein the film thickness of the hole transport layer is 8nm.
[0156] ⑻Vapor-deposit Ag on the hole transport layer to prepare an anode layer, wherein the thickness of the anode layer is 100 nm, to form a flexible solar cell device.
[0157] Application Example 2
[0158] The difference between Application Example 2 and Application Example 1 is that the same steps are adopted to prepare the photovoltaic device assembly layer on the thermally conductive smooth layer obtained by Example 2 to form a flexible solar cell device.
[0159] Application Example 3
[0160] The difference between Application Example 3 and Application Example 1 is that the same steps are adopted to prepare the photovoltaic device assembly layer on the thermally conductive smooth layer obtained by Example 3 to form a flexible solar cell device.
[0161] Application Example 4
[0162] The difference between Application Example 4 and Application Example 1 is that the same steps are adopted to prepare the photovoltaic device combination layer on the thermally conductive smooth layer obtained by Example 4 to form a flexible solar cell device.
[0163] Application Example 5
[0164] The difference between Application Example 5 and Application Example 1 is that the same steps are adopted to prepare the photovoltaic device assembly layer on the thermally conductive smooth layer obtained by Example 5 to form a flexible solar cell device.
[0165] Application Example 6
[0166] The difference between Application Example 6 and Application Example 1 is that the same steps are adopted to prepare the photovoltaic device combination layer on the thermally conductive smooth layer obtained by Example 6 to form a flexible solar cell device.
[0167] Control group 1
[0168] The difference between the control group 1 and the application example 1 is that the same steps are adopted to prepare the photovoltaic device combination layer on the thermally conductive smooth layer obtained by the comparative example 1 to form a flexible solar cell device.
[0169] Test result analysis:
[0170] The performance test of the flexible solar cell device obtained by the preparation method of the corresponding use cases 1 to 6 and the control group 1 was carried out. The device was irradiated with an irradiance of 1 sun, and the thermal conductivity of the flexible solar cell device was tested by the Flex TPS transient plane heat source mode in the Trident thermal conductivity meter. The volume resistivity of the polymer substrate formed by the paper-based substrate and the thermally conductive smooth layer of the flexible solar cell device was tested by the ZC-90G insulation resistance tester at room temperature (25°C). The test results are shown in Table 1 below:
[0171] Table 1
[0172]
[0173] It can be seen from Table 1 above that as the doping mass percentage of fluorinated graphene increases, the thermal conductivity increases and a certain volume resistivity is maintained, indicating that the thermal conductivity of the polymer substrate formed by the combination of the paper-based substrate and the thermally conductive smoothing layer increases and has certain insulation properties; relative to Comparative Example 1, the thermal conductivity of the thermally conductive smoothing layer solution doped with fluorinated graphene is higher, so in this embodiment, doping with fluorinated graphene can enable the thermally conductive smoothing layer to have good thermal conductivity, wherein the thermal conductivity of the thermally conductive smoothing layer solution used in Example 1 with a doping mass percentage of fluorinated graphene of 90wt% is significantly higher than that of other embodiments. In addition, since the paper-based substrate itself has a relatively high volume resistivity (i.e., 1.3×1013Ω·m when undoped), when the thermally conductive smoothing layer is disposed on the paper-based substrate, the volume resistivity of the polymer substrate will gradually approach the volume resistivity of the thermally conductive smoothing layer containing the doped material. Therefore, since the volume resistivity of the thermally conductive smoothing layer solution with a fluorinated graphene doping mass percentage of 90wt% in this embodiment 1 is 0.7×1013Ω·m, the polymer substrate can maintain a certain volume resistivity, that is, it has a certain insulation performance.
[0174] In summary, the thermally conductive smoothing layer of the embodiment of the present application adopts a thermally conductive smoothing solution with a doping weight percentage of 90wt% of fluorinated graphene, which can provide good thermal conductivity and insulation performance, can quickly dissipate heat for flexible solar cell devices, and protect the combined layer of optoelectronic devices, and reduce the surface roughness of the paper-based substrate to avoid the occurrence of short circuits between the anode layer and the cathode layer. In addition, the doping material of the thermally conductive smoothing layer is further tested, and the thermal conductivity and resistivity of the thermally conductive smoothing films of different doping materials are compared when the doping weight percentage is 90wt%. The device is irradiated with an irradiance of 1sun, and the thermal conductivity of the flexible solar cell device is tested by the Flex TPS transient plane heat source mode in the Trident thermal conductivity meter, and the volume resistivity of the polymer substrate formed by the paper-based substrate and the thermally conductive smoothing layer of the flexible solar cell device is tested at room temperature (25°C) by the ZC-90G insulation resistance tester. The test results are shown in Table 2 below:
[0175] Table 2
[0176]
[0177] It can be seen from Tables 1 and 2 above that although the thermal conductivity of the thermally conductive smoothing layer using fluorinated graphene as the doping material is low, its resistivity is much higher than that of the other two doping materials. Since the volume resistivity of the thermally conductive smoothing film doped with reduced graphene oxide and the thermally conductive smoothing film doped with graphite is much lower than that of the paper-based substrate, if reduced graphene oxide (RGO) or graphite (graphite) is used as the doping material of the thermally conductive smoothing film, the polymer substrate will lose its insulating properties. Therefore, the thermally conductive smoothing layer using fluorinated graphene as the doping material in the embodiment of the present application can have both good thermal conductivity and insulating properties, which can not only quickly dissipate heat for the flexible solar cell device, but also protect the photovoltaic device combination layer to avoid short circuits between the anode layer and the cathode layer.
[0178] The flexibility test of the solar flexible cell obtained in the above-mentioned Example 1 was further performed. The solar flexible cell described in Example 1 was bent using a bending platform (the curvature radius of each bend was 5 mm), wherein the solar flexible cell that was not bent was used as Example 1, the solar flexible cell that was bent 200 times was used as Comparative Example 2, and the solar flexible cell that was bent 500 times was used as Comparative Example 3. The flexibility test of the solar flexible cells of Example 1, Comparative Example 2, and Comparative Example 3 was performed, and the device was irradiated with an irradiance of 1 sun (one sun illumination intensity). The photoelectric conversion efficiency (PCE) of the flexible solar cell device was tested by an IV test system, and the test results are shown in the following table:
[0179] Table 3
[0180] Bending times PCE(%) 0 9.3 200 9.1 500 9.1
[0181] It can be seen from Table 3 above that the photoelectric conversion efficiency of the flexible solar device based on the biodegradable material doped with fluorinated graphene as the thermal conductive smoothing layer did not show a significant decrease after multiple bending. Compared with the unbent flexible solar device, the performance of the flexible solar cell after multiple bending treatments was stable. Therefore, the flexible solar cell using fluorinated graphene as the thermal conductive smoothing layer of the doping material in the embodiment of the present application has excellent flexibility and stable performance.
[0182] Obviously, the embodiments described above are only some embodiments of the present application, rather than all embodiments. The preferred embodiments of the present application are given in the accompanying drawings, but they do not limit the patent scope of the present application. The present application can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive. Although the present application is described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific implementation methods, or to perform equivalent replacement of some of the technical features therein. Any equivalent structure made using the contents of the specification and drawings of this application, directly or indirectly used in other related technical fields, is similarly within the scope of patent protection of this application.
Claims
1. A flexible substrate, characterized in that: include: Paper-based substrate; A thermally conductive smoothing layer is disposed on the paper-based substrate, wherein the thermally conductive smoothing layer comprises a biodegradable material doped with fluorinated graphene.
2. The flexible substrate according to claim 1, characterized in that The fluorination degree of the fluorinated graphene is C / F=1.
3. The flexible substrate according to claim 1, characterized in that: The mass percentage of the fluorinated graphene doping is 40wt% to 90wt%.
4. The flexible substrate according to claim 1, characterized in that: The biodegradable materials include furan dicarboxylic acid-based polyesters and polyhydroxy fatty acids (PHA); Optionally, the furan dicarboxylic acid-based polyester includes polyethylene furandicarboxylate (PEF), p-xylene dimer (PCF), and high-toughness furan copolyester (PECF); Optionally, the polyhydroxyalkanoic acid includes polylactic acid (PLA), polyglycolic acid (PGA), polyhydroxyhexanoate (PHHx), polyhydroxyvalerate (PHV), polyhydroxyoctanoate (PHO), and polybutylene glycol succinate (PBS).
5. The flexible substrate according to claim 1, characterized in that: The paper-based substrate is selected from at least one of stone paper, printing paper, filter paper, coated paper, sulfuric acid paper, photographic paper, copy paper, glossy paper, art adhesive paper, and graphite paper.
6. A method for preparing a flexible substrate, characterized in that: The following steps are involved: providing a paper-based substrate; placing a thermally conductive smoothing layer solution on the paper-based substrate to form a thermally conductive smoothing layer; Wherein, the thermally conductive smoothing layer solution comprises a biodegradable material doped with fluorinated graphene.
7. The method for preparing a flexible substrate according to claim 6, characterized in that: The thermally conductive smoothing layer solution is prepared by the following steps: Adding graphite fluoride to a hexafluoroisopropanol solution to form a mixed solution and subjecting it to ultrasonic treatment, and then subjecting it to centrifugal treatment, removing the precipitate, and obtaining a thermal conductor, wherein the degree of fluorination of the thermal conductor is C / F=1; Adding biodegradable materials to the thermal conductor to form a mixed solution, and performing ultrasonic treatment to form a thermally conductive smooth layer solution, wherein the mass percentage of the thermal conductor doped is 40wt% to 90wt%; Wherein, the biodegradable material includes furan dicarboxylic acid-based polyester and polyhydroxy fatty acid (PHA); Optionally, the furan dicarboxylic acid-based polyester includes polyethylene furandicarboxylate (PEF), p-xylene dimer (PCF), and high-toughness furan copolyester (PECF); Optionally, the polyhydroxyalkanoic acid includes polylactic acid (PLA), polyglycolic acid (PGA), polyhydroxyhexanoate (PHHx), polyhydroxyvalerate (PHV), polyhydroxyoctanoate (PHO), and polybutylene glycol succinate (PBS).
8. The method for preparing a flexible substrate according to claim 7, characterized in that: Before adding the biodegradable material into the thermal conductive agent to form a mixed solution, the following steps are also included: The thermal conductor is concentrated, and then the biodegradable material is added to the concentrated thermal conductor to form a mixed solution.
9. A flexible solar cell device, characterized in that: include: A flexible substrate, wherein the flexible substrate is the flexible substrate according to any one of claims 1 to 5, or is prepared by the method for preparing a flexible substrate according to any one of claims 6 to 8; The optoelectronic device assembly layer is arranged on the thermally conductive smooth layer of the flexible substrate.
10. The flexible solar cell device according to claim 9, wherein the photovoltaic device assembly layer comprises: An anode layer and a cathode layer are arranged opposite to each other; a photoactive layer disposed between the anode layer and the cathode layer; An electron transport layer, disposed between the photoactive layer and the cathode layer; A hole transport layer, which is disposed between the photoactive layer and the anode layer; And / or, the material of the anode layer and the cathode layer is selected from at least one of a metal material, a carbon material and a metal oxide, wherein the metal material is selected from at least one of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material is selected from at least one of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes a doped or undoped metal oxide, including at least one of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, and the composite electrode includes at least one of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2; And / or, the material of the electron transport layer is selected from oxides, fullerenes and their derivatives, graphene and its derivatives, low work function metals, polyfluorene derivatives such as, conjugated polyelectrolytes, NDI derivatives, perylene diimide (PDI) derivatives, naphthalene diimide-like molecules NDIO, star-shaped conjugated small molecule electrolyte interface materials TzPyBr, black scale (BP), Mxenes, metal oxides, doped metal oxides, II-VI semiconductor materials, III-V semiconductor materials and I-III-VI semiconductor materials, the low work function metal is selected from at least one of Ca and Ba; the polyfluorene derivative is selected from at least one of PFN and PFNBr; the NDI derivative is selected from PDNI-F3 N, PDNI-F3N-Br; the metal oxide is selected from at least one of ZnO, TiO2, SnO2; the perylene diimide (PDI) derivative is selected from at least one of PDIN, PDINO, PDINN; the metal oxide in the doped metal oxide is selected from at least one of ZnO, TiO2, SnO2, the doping element is selected from at least one of Al, Mg, Li, In, Ga, the II-VI semiconductor material is selected from at least one of ZnS, ZnSe, CdS; the III-V semiconductor material is selected from at least one of InP and GaP; the I-III-VI semiconductor material is selected from at least one of CuInS and CuGaS; And / or, the material of the photoactive layer is selected from at least one of an organic photovoltaic material, a perovskite photovoltaic material or a dye-sensitized photovoltaic material; And / or, the material of the hole transport layer is selected from Spiro-OMeTAD, PEDOT:PSS, PTAA, P3HT, CuSCN, molybdenum oxide, graphene oxide (GO), CuI, 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-bis(3 -methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), polyaniline, polypyrrole , poly(p-phenylene vinylene), poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] and poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, poly(N-vinylcarbazole) and its Derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine, spiro NPB, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO.