Thermoplastic resin composition

By combining materials such as aromatic vinyl monomers, vinyl cyanide monomers, maleimide monomers, and polyvinyl alcohol in thermoplastic resins, a thermoplastic resin composition with excellent chemical resistance and sprayability is formed. , which solves the problems of cracking and peeling of diene grafted polymer thermoplastic resin molded products during painting, and improves their heat resistance and processability.

CN113490716BActive Publication Date: 2024-10-01LG CHEM LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202080016957.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-21
Filing Date
2020-09-07
Publication Date
2024-10-01
Estimated Expiration
2040-09-07

AI Technical Summary

Technical Problem

Thermoplastic resin molded articles made from diene-based graft polymers are prone to small cracks and paint peeling when solvent spray paint is used, resulting in surface defects.

Method used

Develop a thermoplastic resin composition comprising a first polymer graft-polymerized by an aromatic vinyl-based monomer and a vinyl cyanide-based monomer, a maleimide-based monomer, and a maleic acid-based monomer. Second polymer, and a third polymer of aromatic vinyl monomer and vinyl cyanide monomer, and adding an appropriate amount of polyvinyl alcohol to form a polymer with excellent chemical resistance, sprayability, tensile strength and processability composition.

Benefits of technology

Significantly reduces cracks and spray defects caused by solvents and improves the chemical resistance, sprayability, tensile strength and processability of thermoplastic resins for automotive interior and exterior materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003231146000000061
    Figure BDA0003231146000000061
  • Figure BDA0003231146000000071
    Figure BDA0003231146000000071
Patent Text Reader

Abstract

The present invention relates to a thermoplastic resin composition, comprising: 100 parts by weight of a base resin, wherein the base resin comprises a first polymer, a second polymer and a third polymer, wherein the first polymer is obtained by grafting an aromatic vinyl monomer and a vinyl cyanide monomer onto a diene rubber polymer, the second polymer comprises a maleimide monomer unit, a maleic acid monomer unit and an aromatic vinyl monomer unit, the third polymer comprises an aromatic vinyl monomer unit and a vinyl cyanide monomer unit; and 1 to 3 parts by weight of a fourth polymer, wherein the fourth polymer comprises polyvinyl alcohol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims priority to and the benefit of Korean Patent Application No. 10-2019-0130863, filed on October 21, 2019, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0004] The present invention relates to a thermoplastic resin composition, in particular to a thermoplastic resin composition containing an appropriate amount of polyvinyl alcohol. Background Art

[0005] Diene graft polymers are graft polymers obtained by polymerizing aromatic vinyl monomers and vinyl cyanide monomers onto diene rubber polymers. Compared with existing high-impact polystyrene, diene graft polymers have high impact resistance, chemical resistance, thermal stability, colorability, fatigue resistance, hardness, and processability. Due to these properties, thermoplastic resin molded products made of diene graft polymers are used as interior and exterior materials for automobiles, parts for office equipment and various electrical and electronic products, etc.

[0006] However, when thermoplastic resin molded articles made of diene-based graft polymers are painted and deposited using solvents, small cracks may occur, resulting in pinholes being formed on the surface, or paint peeling may occur.

[0007] Therefore, research has been conducted on developing a thermoplastic resin composition having excellent chemical resistance and sprayability while maintaining excellent physical properties of the diene-based graft polymer. Summary of the invention

[0008] Technical issues

[0009] An object of the present invention is to provide a thermoplastic resin composition having excellent chemical resistance, sprayability, tensile strength, heat resistance and processability.

[0010] Technical Solution

[0011] According to one aspect of the present invention, a thermoplastic resin composition is provided, comprising: 100 parts by weight of a base resin, wherein the base resin comprises: a first polymer obtained by grafting an aromatic vinyl monomer and a vinyl cyanide monomer onto a diene rubber polymer, a second polymer comprising a maleimide monomer unit, a maleic acid monomer unit and an aromatic vinyl monomer unit, and a third polymer comprising an aromatic vinyl monomer unit and a vinyl cyanide monomer unit; and 1 to 3 parts by weight of a fourth polymer comprising polyvinyl alcohol.

[0012] Beneficial Effects

[0013] The thermoplastic resin composition of the present invention has excellent chemical resistance, sprayability, tensile strength, heat resistance and processability. Therefore, when the thermoplastic resin composition is used as an interior and exterior material of an automobile, cracks caused by a solvent used for spray painting can be minimized, and spray defects caused by cracks can be minimized. DETAILED DESCRIPTION

[0014] Hereinafter, the present invention will be described in more detail to help understanding of the present invention.

[0015] The terms or words used in the specification and claims should not be construed as limited to common or dictionary contents, and should be construed as meanings and concepts consistent with the spirit of the present invention based on the principle that inventors can appropriately define the concepts of the terms in order to interpret their invention in the best manner.

[0016] In the present invention, the average particle size can be measured using a dynamic light scattering method, and specifically, can be measured using Nicomp 380 manufactured by Particle Sizing Systems. In the present invention, the average particle size may refer to the arithmetic average particle size in the particle size distribution measured by the dynamic light scattering method, that is, the intensity distribution average particle size.

[0017] In the present invention, the glass transition temperature may be measured by differential scanning calorimetry.

[0018] In the present invention, the diene rubber polymer may refer to a polymer prepared by crosslinking a diene monomer alone or a diene monomer and a comonomer copolymerizable therewith. The diene monomer may be one or more selected from 1,3-butadiene, isoprene, chloroprene and piperylene, wherein 1,3-butadiene is preferred. The comonomer may include aromatic vinyl monomers, vinyl cyanide monomers, olefin monomers, etc. The diene rubber polymer may include butadiene rubber polymer, butadiene-styrene rubber polymer, butadiene-acrylonitrile rubber polymer, etc. The diene rubber polymer is preferably a butadiene rubber polymer having excellent impact strength and excellent chemical resistance.

[0019] In the present invention, the aromatic vinyl monomer may be one or more selected from styrene, α-methylstyrene, α-ethylstyrene and p-methylstyrene, among which styrene is preferred.

[0020] In the present invention, the vinyl cyanide monomer may be one or more selected from acrylonitrile, methacrylonitrile, phenylacrylonitrile and α-chloroacrylonitrile, among which acrylonitrile is preferred.

[0021] In the present invention, the maleimide monomer may be one or more selected from maleimide, N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-isobutylmaleimide, N-tert-butylmaleimide, N-laurylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(4-chlorophenyl)maleimide, 2-methyl-N-phenylmaleimide, N-(4-bromophenyl)maleimide, N-(4-nitrophenyl)maleimide, N-(4-hydroxyphenyl)maleimide, N-(4-methoxyphenyl)maleimide, N-(4-carboxyphenyl)maleimide and N-benzylmaleimide, among which N-phenylmaleimide is preferred.

[0022] In the present invention, the maleic acid monomer may be one or more selected from maleic anhydride, maleic acid, maleic acid monoester and maleic acid diester, among which maleic anhydride is preferred.

[0023] 1. Thermoplastic resin composition

[0024] A thermoplastic resin composition according to one embodiment of the present invention comprises: 1) 100 parts by weight of a base resin, wherein the base resin comprises: a first polymer obtained by graft polymerization of an aromatic vinyl monomer and a vinyl cyanide monomer onto a diene rubber polymer, a second polymer comprising a maleimide monomer unit, a maleic acid monomer unit and an aromatic vinyl monomer unit, and a third polymer comprising an aromatic vinyl monomer unit and a vinyl cyanide monomer unit; and 1 to 3 parts by weight of a fourth polymer comprising polyvinyl alcohol.

[0025] The inventors of the present invention have found that the thermoplastic resin composition has improved impact resistance, heat resistance and processability through the synergistic effect of the first polymer and the second polymer, and when the thermoplastic resin composition contains an appropriate amount of the fourth polymer, its hardness, chemical resistance, sprayability and processability are improved, thereby completing the present invention.

[0026] Hereinafter, components of a thermoplastic resin composition according to one embodiment of the present invention will be described in detail.

[0027] 1) Base resin

[0028] The base resin may include: a first polymer obtained by grafting an aromatic vinyl monomer and a vinyl cyanide monomer onto a diene rubber polymer; a second polymer comprising a maleimide monomer unit, a maleic acid monomer unit and an aromatic vinyl monomer unit; and a third polymer comprising an aromatic vinyl monomer unit and a vinyl cyanide monomer unit.

[0029] The first polymer may impart excellent impact resistance, excellent heat resistance, and excellent processability to the thermoplastic resin composition through a synergistic effect with the second polymer.

[0030] The first polymer may be included in the thermoplastic resin composition in an amount of 15 to 35 parts by weight, preferably 20 to 40 parts by weight, relative to 100 parts by weight of the base resin. When the above range is met, excellent hardness, heat resistance, processability, impact resistance and tensile resistance may be imparted.

[0031] In the first polymer, the diene-based rubber polymer may have an average particle size in the range of 200 nm to 400 nm, preferably 250 nm to 300 nm, in order to achieve excellent impact resistance and surface gloss.

[0032] The first polymer may be a graft polymer obtained by graft-polymerizing styrene and acrylonitrile onto a butadiene rubber polymer.

[0033] The second polymer may be included in the thermoplastic resin composition in an amount of 5 to 25 parts by weight, preferably 10 to 20 parts by weight, relative to 100 parts by weight of the base resin. When the above range is met, the thermoplastic resin composition may be endowed with excellent heat resistance, processability and impact resistance.

[0034] The second polymer is a copolymer of a maleimide monomer, a maleic acid monomer and an aromatic vinyl monomer, and may be an N-phenylmaleimide / maleic anhydride / styrene polymer comprising an N-phenylmaleimide unit, a maleic anhydride unit and a styrene unit. Since the second polymer should be able to impart excellent heat resistance and processability to the thermoplastic resin composition, the glass transition temperature may be in the range of 180°C to 210°C, preferably 190°C to 200°C, and the melt flow index may be in the range of 1g / 10min to 5g / 10min, preferably 2g / 10min to 4g / 10min, under the conditions of 265°C and 10kg according to ASTM D1238.

[0035] The third polymer may be included in the thermoplastic resin composition in an amount of 50 to 70 parts by weight, preferably 55 to 65 parts by weight, relative to 100 parts by weight of the base resin. When the above range is met, the first polymer and the second polymer are included in the thermoplastic resin composition in appropriate amounts, thereby imparting excellent hardness, heat resistance and processability to the thermoplastic resin composition.

[0036] The third polymer is a copolymer of an aromatic vinyl-based monomer and a vinyl cyan-based monomer, and may be a styrene / acrylonitrile polymer including a styrene unit and an acrylonitrile unit.

[0037] 2) The fourth polymer

[0038] The fourth polymer includes polyvinyl alcohol. In addition to polyvinyl alcohol, the fourth polymer may include polyvinyl acetate that is not hydrolyzed when polyvinyl acetate is hydrolyzed to prepare polyvinyl alcohol.

[0039] Since the fourth polymer includes polyvinyl alcohol, the fourth polymer is water-soluble but may have the property of not being well dissolved in organic solvents mainly used for spray painting and deposition, so the fourth polymer can improve the heat resistance and sprayability of the thermoplastic resin composition.

[0040] The fourth polymer may be included in the thermoplastic resin composition in an amount of 1 to 3 parts by weight, preferably 1.5 to 2.5 parts by weight, relative to 100 parts by weight of the base resin. When the above range is met, the chemical resistance and sprayability of the thermoplastic resin composition can be significantly improved. On the other hand, when an amount less than the above range is included, the improvement effect of the chemical resistance and sprayability of the thermoplastic resin composition is not obvious. When an amount exceeding the above range is included, the chemical resistance and sprayability of the thermoplastic resin composition are improved, but its impact resistance, processability and heat resistance will be significantly deteriorated.

[0041] The weight average molecular weight of the fourth polymer may be 70,000 g / mol to 140,000 g / mol, preferably 85,000 g / mol to 124,000 g / mol. When the above range is satisfied, sprayability and chemical resistance may be significantly improved.

[0042] Hereinafter, the present invention will be described in detail with reference to the following embodiments so that those skilled in the art can easily implement the present invention. However, the present invention can be embodied in various forms and is not limited to the embodiments described herein.

[0043] Examples and Comparative Examples

[0044] The components used in the following examples and comparative examples are described below:

[0045] First polymer: DP270 manufactured by LC CHEM, LTD. (graft polymer obtained by graft-polymerizing styrene and acrylonitrile onto a butadiene rubber polymer (average particle diameter: 300 nm)).

[0046] Second polymer: MSNB (N-phenylmaleimide / maleic anhydride / styrene copolymer) manufactured by DENKA

[0047] Third polymer: 92HR (styrene / acrylonitrile copolymer) manufactured by LG CHEM, LTD.

[0048] Fourth copolymer: polyvinyl alcohol (manufacturer: Sigma Aldrich., product number: 363146, weight average molecular weight: 85,000 g / mol to 124,000 g / mol, hydrolysis: more than 99%)

[0049] The above components were mixed and stirred according to the contents shown in the following table to prepare a thermoplastic composition.

[0050] Experimental Example 1

[0051] The thermoplastic resin compositions of Examples and Comparative Examples were extruded to prepare pellets. The physical properties of the pellets were evaluated using the methods described below, and the results are shown in the following table.

[0052] ① Melt flow index (g / 10 min): measured according to ASTM D1238 under the conditions of 220°C and 10 kg.

[0053] Experimental Example 2

[0054] The thermoplastic resin compositions of Examples and Comparative Examples were extruded and injected to prepare test specimens. The physical properties of the test specimens were evaluated using the methods described below, and the results are shown in the following table.

[0055] ② Chemical resistance (seconds): A specimen measuring 200 mm x 12.7 mm x 3.2 mm was fixed on a bending fixture with a strain of 1.1%, and 1 cc of thinner was applied to the specimen, and then the time taken for cracks to appear in the specimen was measured. When no cracks appeared until 600 seconds after the thinner was applied, it was determined that the chemical resistance evaluation was passed. Those that passed the chemical resistance evaluation were described as >600.

[0056] ③ Sprayability: Degrease a sample of 10cm x 10cm with isopropyl alcohol, and then spray black paint on the sample. After 5 minutes from spraying the paint, spray clear paint and dry it in an oven at 85°C. Visually observe whether pinholes are generated and evaluate its sprayability.

[0057] A: Excellent, B: Average, C: Poor

[0058] ④Tensile strength (kgf / cm 2 ): Measured according to ASTM D638.

[0059] ⑤ Heat deformation temperature (°C): measured according to ASTM D648-7 under the conditions of 1 / 4 inch, 18.6 kgf and 120°C / hr.

[0060]

Table 1

[0061]

[0062]

[0063] Referring to the above table, it is confirmed that Examples 1 to 4 containing 1 to 3 parts by weight of polyvinyl alcohol have excellent chemical resistance, sprayability, tensile strength, and heat deformation temperature. It is also confirmed that the processability is also excellent because the melt flow index is at an appropriate level. In contrast, it is confirmed that the chemical resistance and sprayability of Comparative Example 1 not containing polyvinyl alcohol and Comparative Example 2 containing a small amount of polyvinyl alcohol are deteriorated. From these results, it can be predicted that when the molded articles manufactured by Comparative Examples 1 and 2 are used for spray painting, paint defects or peeling, etc. will occur.

[0064] It is confirmed that Comparative Example 3 containing an excess of polyvinyl alcohol exhibits excellent chemical resistance and sprayability, but the flow index, tensile strength and heat distortion temperature decrease. Based on these results, it can be predicted that the molded article produced by Comparative Example 3 will show deteriorated processability, hardness and heat resistance.

[0065] It was also confirmed that Comparative Example 5, which did not contain the second polymer, exhibited excellent chemical resistance, sprayability and tensile strength, but the melt flow index was too high and the heat deformation temperature was reduced. Based on these results, it can be predicted that the molded article produced by Comparative Example 5 would exhibit deteriorated processability and heat resistance.

Claims

1. A thermoplastic resin composition comprising: 100 parts by weight of a base resin, the base resin comprising 20 to 40 parts by weight of a first polymer, 5 to 25 parts by weight of a second polymer, and 50 to 70 parts by weight of a third polymer, wherein the first polymer is obtained by graft polymerization of an aromatic vinyl monomer and a vinyl cyanide monomer onto a diene rubber polymer, the second polymer comprises a maleimide monomer unit, a maleic acid monomer unit, and an aromatic vinyl monomer unit, and the third polymer comprises an aromatic vinyl monomer unit and a vinyl cyanide monomer unit; and 1.5 to 2.5 parts by weight of a fourth polymer, the fourth polymer being polyvinyl alcohol, in, The fourth polymer has a weight average molecular weight of 70,000 g / mol to 140,000 g / mol.

2. The thermoplastic resin composition according to claim 1, wherein The diene rubber polymer of the first polymer has an average particle size of 200 nm to 400 nm.

3. The thermoplastic resin composition according to claim 1, wherein The second polymer has a glass transition temperature of 180°C to 210°C.

4. The thermoplastic resin composition according to claim 1, wherein According to ASTM D1238, at 265° C. and 10 kg, the melt flow index of the second polymer is 1 g / 10 min to 5 g / 10 min.

Citation Information

Patent Citations

  • Bandwidth allocating apparatus and method for providing low-latency service in optical network

    KR1020190130863A

  • Maleimide type heat-resisting ABS alloy and preparation method thereof

    CN104945834A

  • Thermoplastic resin composition, method for producing same, and molded article of same

    CN107001760A

  • Flame retardant thermoplastic resin composition having excellent thermal stability, preparation method therefor, and molded product prepared therefrom

    CN107109024A

  • Thermoplastic resin composition and article produced therefrom

    CN107880426A