HEMT epitaxial wafer and preparation method thereof, HEMT
By optimizing the stacked structure and Mg doping in HEMT epitaxial wafers, the heat dissipation and dislocation defects caused by lattice mismatch were solved, thereby improving the performance and reliability of the devices.
Patent Information
- Application Number
- CN202411162491.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Existing HEMT devices face lattice mismatch issues during manufacturing, leading to difficulties in heat dissipation, reduced carrier mobility, and unstable device performance, especially when using silicon substrates, where dislocation defects are severe.
A HEMT epitaxial wafer structure is adopted, comprising a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer and a second AlInGaN layer stacked sequentially on a substrate. By controlling the composition and thickness of each layer and the growth conditions, lattice mismatch and dislocation propagation are optimized, and Mg doping is combined to reduce leakage current.
It improves the crystal quality and two-dimensional electron gas concentration of HEMT devices, reduces leakage current, enhances the breakdown voltage and reliability of devices, and strengthens thermal homogenization capabilities.
Smart Images

Figure CN118676200B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of field effect transistors, and in particular to a HEMT epitaxial wafer and a preparation method thereof, and a HEMT. Background Art
[0002] HEMT based on gallium nitride and related group III nitride materials (AlN, InN) is currently a hot topic in the research of compound semiconductor electronic devices. In particular, gallium nitride has advantages such as wide bandgap, high critical breakdown electric field, high electron saturation velocity, high thermal conductivity, and strong radiation resistance. Therefore, HEMT based on AlGaN / GaN heterojunction materials is currently the most widely used power device.
[0003] Gallium nitride-based high electron mobility transistors (HEMTs) face a challenge in the manufacturing process, which is the lack of a homogeneous epitaxial substrate that fully matches them. This results in them usually growing on substrates that do not match the gallium nitride lattice and thermal expansion coefficient, such as sapphire, silicon carbide or silicon. When using sapphire as a substrate, its low thermal conductivity makes it difficult for the heat generated by the device during operation to dissipate quickly, thereby inducing high-temperature lattice scattering, which reduces the mobility of carriers and thus affects the high-frequency response capability of the device. Although the thermal conductivity of silicon carbide substrates is high, their high cost limits their widespread application. In contrast, silicon substrates not only have higher thermal conductivity and lower cost, but the significant lattice and thermal expansion coefficient mismatch between silicon and gallium nitride will lead to a large number of dislocation defects, which will significantly reduce the quality of the epitaxial layer, thereby negatively affecting the overall performance of the HEMT device. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a HEMT epitaxial wafer and a preparation method thereof, which can reduce leakage current and improve device performance and reliability.
[0005] Another technical problem to be solved by the present invention is to provide a HEMT with small leakage current, strong device performance and high reliability.
[0006] In order to solve the above technical problems, the present invention provides a HEMT epitaxial wafer, comprising a substrate, a buffer layer, a channel layer, an insertion layer, a barrier layer and a cap layer sequentially stacked on the substrate; the buffer layer comprises a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer and a second AlInGaN layer sequentially stacked on the substrate;
[0007] The lattice constant of the first AlInGaN layer is greater than the lattice constant of the second AlInGaN layer.
[0008] As an improvement of the above technical solution, the proportion of In component in the first AlInGaN layer is 0.01-0.1, the proportion of Al component is 0.01-0.3, and the thickness is 10nm-100nm; and / or
[0009] The second AlInGaN layer has an In component ratio of 0.01-0.1, an Al component ratio of 0.1-0.5, and a thickness of 10nm-100nm.
[0010] As an improvement of the above technical solution, the B component ratio in the first BGaN layer is 0.1-0.5, and the thickness thereof is 10nm-50nm; and / or
[0011] The thickness of the BN layer is 30nm to 50nm; and / or
[0012] The B component ratio in the second BGaN layer is 0.1-0.3, and the thickness is 10nm-50nm.
[0013] As an improvement of the above technical solution, the first AlInGaN layer and the second AlInGaN layer are doped with Mg;
[0014] The Mg doping concentration in the first AlInGaN layer is 1×10 19 cm -3 ~5×10 19 cm -3 ;
[0015] The Mg doping concentration in the second AlInGaN layer is 1×10 18 cm -3 ~1×10 19 cm -3 .
[0016] As an improvement of the above technical solution, along the growth direction of the HEMT epitaxial wafer, the Al component in the first AlInGaN layer increases and the In component decreases; and / or
[0017] Along the growth direction of the HEMT epitaxial wafer, the Al component and the In component in the second AlInGaN layer both show a decreasing change.
[0018] As an improvement of the above technical solution, the proportion of B component in the first BGaN layer is greater than the proportion of B component in the second BGaN layer, so that the band gap width of the first BGaN layer is greater than the band gap width of the second BGaN layer.
[0019] Correspondingly, the present invention also discloses a method for preparing a HEMT epitaxial wafer, which is used to prepare the above-mentioned HEMT epitaxial wafer, and comprises:
[0020] Providing a substrate, and sequentially growing a buffer layer, a channel layer, an insertion layer, a barrier layer, and a cap layer on the substrate; the buffer layer comprises a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer, and a second AlInGaN layer sequentially stacked on the substrate;
[0021] The lattice constant of the first AlInGaN layer is greater than the lattice constant of the second AlInGaN layer.
[0022] As an improvement of the above technical solution, the growth temperature of the first AlInGaN layer is 900° C. to 1100° C., and the growth pressure is 50 torr to 500 torr; and / or
[0023] The growth temperature of the first BGaN layer is 1000° C. to 1200° C., and the growth pressure is 50 torr to 500 torr; and / or
[0024] The growth temperature of the BN layer is 1100° C. to 1300° C., and the growth pressure is 100 torr to 500 torr; and / or
[0025] The growth temperature of the second BGaN layer is 1000° C. to 1200° C., and the growth pressure is 50 torr to 500 torr; and / or
[0026] The growth temperature of the second AlInGaN layer is 900° C. to 1100° C., and the growth pressure is 50 torr to 500 torr.
[0027] As an improvement of the above technical solution, the first AlInGaN layer and the second AlInGaN layer are doped with Mg;
[0028] During the growth of the first AlInGaN layer and the second AlInGaN layer, the In source is introduced periodically.
[0029] Correspondingly, the present invention also discloses a HEMT, which includes the above-mentioned HEMT epitaxial wafer.
[0030] Beneficial effects:
[0031] 1. In the HEMT epitaxial wafer provided by the present invention, the buffer layer includes a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer and a second AlInGaN layer stacked on the substrate in sequence; wherein the first AlInGaN layer and the second AlInGaN layer function to reduce the lattice mismatch between the substrate and the channel layer, improve the crystal quality of the channel layer, and thus increase the concentration of the two-dimensional electron gas in the channel layer. The main functions of the first BGaN layer and the second BGaN layer are to block the transmission of dislocations and prevent leakage electrons from penetrating, reduce vertical leakage current, improve the withstand voltage performance of the HEMT, and improve its reliability. First, the overall densification of the BN layer is higher, which can significantly reduce the dislocation density; second, the bandgap width of the BN layer is as high as 6.9eV, which can significantly reduce the vertical leakage current, improve the voltage resistance of the HEMT, and improve its reliability; third, the BN layer has good thermal conductivity, which can make the heat generated during the growth and use of the HEMT uniform, reduce the thermal stress caused by uneven heat conduction, improve the overall growth quality of the HEMT epitaxial wafer, and improve the reliability of the device based on the HEMT epitaxial wafer. In summary, based on the above-mentioned buffer layer, the overall crystal quality of the epitaxial wafer can be greatly improved, the concentration of the two-dimensional electron gas can be increased, and at the same time, leakage can be reduced and device performance can be improved. In addition, the buffer layer of the present invention can reduce the generation of thermal stress and improve the reliability of the device.
[0032] 2. In the HEMT epitaxial wafer of the present invention, Mg doping is introduced into the first AlInGaN layer and the second AlInGaN layer, which can effectively deplete the leakage current and improve the device performance and reliability. At the same time, the introduction of In can increase the activation energy of Mg, reduce its doping concentration, and reduce its adverse effect on crystal quality. Further, in order to increase the activation energy of Mg, a preparation method of pulsed introduction of In source is adopted. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the structure of a HEMT epitaxial wafer in one embodiment of the present invention;
[0034] Figure 2 FIG. 4 is a flow chart of a method for preparing a HEMT epitaxial wafer in one embodiment of the present invention. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.
[0036] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0037] In the present invention, “preferred” is only used to describe an implementation method or example with better effects, and it should be understood that it does not constitute a limitation on the protection scope of the present invention.
[0038] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0039] In the present invention, reference to a numerical range includes both endpoints of the numerical range unless otherwise specified.
[0040] To solve the above problems, the present invention provides a gallium nitride-based high electron mobility transistor epitaxial wafer, such as Figure 1 As shown, it includes a substrate 1, a buffer layer 2, a channel layer 3, an insertion layer 4, a barrier layer 5 and a cap layer 6 stacked on the substrate 1 in sequence; the buffer layer 2 includes a first AlInGaN layer 21, a first BGaN layer 22, a BN layer 23, a second BGaN layer 24 and a second AlInGaN layer 25 stacked on the substrate 1 in sequence. Among them, the first AlInGaN layer 21 and the second AlInGaN layer 25 mainly function to reduce the lattice mismatch between the substrate 1 and the channel layer 3, improve the crystal quality of the channel layer 3, and thus increase the concentration of the two-dimensional electron gas in the channel layer 3. Further, in order to better improve the crystal quality of the channel layer 3, the lattice constant of the first AlInGaN layer 21 is controlled to be greater than the lattice constant of the second AlInGaN layer 25, so as to form a lattice constant gradient structure between the substrate 1 and the channel layer 3, and reduce the generation of dislocations. The main function of the first BGaN layer 22 and the second BGaN layer 24 is to block the transmission of dislocations. Specifically, since the B atoms are small, they can better fill the defects on the surface of the film, making the film denser, thereby reducing the transmission of dislocations. At the same time, the first BGaN layer 22 and the second BGaN layer 24 have a large band gap width, which can effectively prevent leakage electrons from penetrating, making the buffer layer as a whole close to an insulating state, greatly reducing vertical leakage current, improving the withstand voltage performance of the HEMT, and improving its reliability. In addition, the first BGaN layer 22 and the second BGaN layer 24 can also improve the overall flatness of the buffer layer 2, making the later channel layer 3 more flat, and improving the concentration and mobility of the two-dimensional electron gas. Among them, the BN layer 23 has a higher overall densification degree, which can greatly reduce the dislocation density; secondly, the band gap width of the BN layer 23 is as high as 6.9eV, which can greatly reduce the vertical leakage current; thirdly, the BN layer 23 has good thermal conductivity, which can make the heat generated during the growth and use of the HEMT uniform, reduce the thermal stress caused by uneven heat conduction, improve the overall growth quality of the HEMT epitaxial wafer, and improve the reliability of the device based on the HEMT epitaxial wafer. In summary, based on the above-mentioned buffer layer, the overall crystal quality of the epitaxial wafer can be greatly improved, the concentration of the two-dimensional electron gas can be increased, and the leakage can be reduced, and the device performance can be improved. In addition, the buffer layer of the present invention can reduce the generation of thermal stress and improve the reliability of the device.
[0041] Among them, the In component ratio in the first AlInGaN layer 21 is 0.01-0.15. If the In component ratio is low, the lattice constant of the layer is small, and it is difficult to effectively buffer the lattice mismatch; if the In component ratio is too large, the crystal quality of the layer is too poor, and it is also difficult to effectively buffer the lattice mismatch. Exemplarily, the In component ratio in the first AlInGaN layer 21 is 0.03, 0.05, 0.07, 0.09, 0.11 or 0.13, but not limited thereto. Preferably, it is 0.01-0.1.
[0042] The proportion of Al in the first AlInGaN layer 21 is 0.01-0.5. The Al atom has a small volume, which is beneficial to improving the crystal quality of the layer. For example, the proportion of Al is 0.05, 0.13, 0.24, 0.36, 0.42 or 0.48, but not limited thereto. Preferably, it is 0.01-0.3.
[0043] The thickness of the first AlInGaN layer 21 is 10 nm to 200 nm, exemplarily 20 nm, 40 nm, 80 nm, 120 nm, 150 nm or 170 nm, but not limited thereto, preferably 10 nm to 100 nm.
[0044] The proportion of In component in the second AlInGaN layer 25 is 0.01-0.15. If the proportion of In component is low, the lattice constant of the layer is small and it is difficult to buffer the lattice mismatch. If the proportion of In component is too large, the lattice mismatch with the subsequently grown channel layer 3 is large. Exemplarily, the proportion of In component in the second AlInGaN layer 25 is 0.03, 0.05, 0.07, 0.09, 0.11 or 0.13, but not limited thereto. Preferably, it is 0.01-0.1.
[0045] The proportion of Al component in the second AlInGaN layer 25 is 0.05-0.5, exemplarily 0.08, 0.13, 0.24, 0.36, 0.42 or 0.48, but not limited thereto, preferably 0.1-0.5.
[0046] The thickness of the second AlInGaN layer 25 is 10 nm to 200 nm, exemplarily 20 nm, 40 nm, 80 nm, 120 nm, 150 nm or 170 nm, but not limited thereto, preferably 10 nm to 100 nm.
[0047] It should be noted that in the present invention, the proportion of In component in the first AlInGaN layer 21 and the second AlInGaN layer 25 refers to the ratio of the number of In atoms in the layer to the total number of Al atoms, In atoms and Ga atoms, and the proportion of Al component refers to the ratio of the number of Al atoms in the layer to the total number of Al atoms, In atoms and Ga atoms.
[0048] Preferably, in some embodiments, the first AlInGaN layer 21 and the second AlInGaN layer 25 are doped with Mg, and the holes generated by Mg doping can further deplete the leakage current, thereby improving the performance and reliability of the device. It should be noted that in the conventional GaN-based HEMT epitaxial structure, undoped GaN is generally used as a buffer layer, but the undoped GaN layer is generally weakly N-type, and there are background electrons, which reduces the withstand voltage performance. One solution is to perform compensation doping, using Mg, Fe or C for P-type doping, but these impurities mostly exist in deep acceptor energy levels and are difficult to ionize, resulting in the need for a higher doping concentration, which reduces the crystal quality of the buffer layer itself. In the present invention, Mg is doped in the first AlInGaN layer 21 and the second AlInGaN layer 25. Since the introduction of In reduces the activation energy of Mg and optimizes its activation, a lower doping concentration can be used, thereby improving the overall crystal quality of the buffer layer 2. Specifically, the Mg doping concentration in the first AlInGaN layer 21 is 1×10 19 cm -3 ~5×10 19 cm -3 ; The Mg doping concentration in the second AlInGaN layer 25 is 1×10 18 cm -3 ~1×10 19 cm -3 .
[0049] Preferably, in some embodiments, along the growth direction of the HEMT epitaxial wafer, the Al component in the first AlInGaN layer 21 increases, the In component decreases, and the Al component and the In component in the second AlInGaN layer 25 both decrease. Based on the above control, the stress distribution can be optimized and the generation of dislocations can be further reduced.
[0050] The proportion of B component in the first BGaN layer 22 is 0.05-0.5. If the proportion of B component is too low, it is difficult to effectively twist and block dislocation extension. If the proportion of B component is too high, the lattice mismatch between the first AlInGaN layer 21 is large. Exemplarily, the proportion of B component in the first BGaN layer 22 is 0.08, 0.11, 0.18, 0.25, 0.33, 0.4 or 0.45, but not limited thereto. Preferably, it is 0.1-0.5.
[0051] The thickness of the first BGaN layer 22 is 10 nm to 100 nm, and is exemplarily 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 50 nm, 60 nm or 80 nm, but is not limited thereto, and is preferably 10 nm to 50 nm.
[0052] The proportion of B component in the second BGaN layer 24 is 0.05-0.4. If the proportion of B component is too low, it is difficult to effectively twist and block dislocation extension. If the proportion of B component is too high, the lattice mismatch between the second AlInGaN layer 25 is large. Exemplarily, the proportion of B component in the second BGaN layer 24 is 0.08, 0.13, 0.18, 0.24, 0.28, 0.33 or 0.37, but not limited thereto. Preferably, it is 0.1-0.3.
[0053] It should be noted that the proportion of the B component in the first BGaN layer 22 and the second BGaN layer 24 in the present invention refers to the ratio of the number of B atoms to the total number of B atoms and Ga atoms in the layer.
[0054] Preferably, in some embodiments, the proportion of B component in the first BGaN layer 22 is controlled to be greater than the proportion of B component in the second BGaN layer 24. Based on the control of the components, the band gap width of the first BGaN layer 22 can be made greater than the band gap width of the second BGaN layer 24, which can further reduce the leakage current.
[0055] The thickness of the BN layer 23 is 30 nm to 100 nm, exemplarily 35 nm, 40 nm, 50 nm, 60 nm, 70 nm or 80 nm, but not limited thereto, preferably 30 nm to 50 nm.
[0056] The substrate 1 is a Si substrate, a sapphire substrate or a GaN substrate, but is not limited thereto, and preferably a sapphire substrate.
[0057] The channel layer 3 is a non-doped GaN layer, and its thickness is 200nm-500nm.
[0058] The insertion layer 4 is an AlN layer, which can further improve the flatness of the interface and the concentration and mobility of the two-dimensional electron gas. Its thickness is 0.5nm~5nm.
[0059] The barrier layer 5 is an AlGaN layer, the Al component ratio thereof is 0.2-0.3, and the thickness is 20nm-35nm.
[0060] The cap layer 6 is a GaN cap layer, and its thickness is 2nm-6nm.
[0061] Accordingly, refer to Figure 2 The present invention also provides a method for preparing a HEMT epitaxial wafer, which is used to prepare the above-mentioned HEMT epitaxial wafer, and comprises the following steps:
[0062] S1: providing a substrate;
[0063] S2: sequentially growing a buffer layer, a channel layer, an insertion layer, a barrier layer and a cap layer on the substrate;
[0064] Specifically, in some implementations, step S2 includes:
[0065] S21: growing a buffer layer on the substrate;
[0066] Specifically, the buffer layer includes a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer and a second AlInGaN layer which are sequentially stacked on the substrate.
[0067] Specifically, in some embodiments, the buffer layer is grown by MOCVD, specifically, the growth temperature of the first AlInGaN layer is 900℃~1100℃, and the growth pressure is 50torr~500torr; the growth temperature of the first BGaN layer is 1000℃~1200℃, and the growth pressure is 50torr~500torr; the growth temperature of the BN layer is 1100℃~1300℃, and the growth pressure is 100torr~500torr; the growth temperature of the second BGaN layer is 1000℃~1200℃, and the growth pressure is 50torr~500torr; the growth temperature of the second AlInGaN layer is 900℃~1100℃, and the growth pressure is 50torr~500torr.
[0068] Preferably, in some embodiments, the In source is introduced periodically during the growth of the first AlInGaN layer and the second AlInGaN layer. More specifically, the In source is introduced for 5s to 10s, stopped for 3s to 5s, and then repeatedly introduced.
[0069] S22: growing a channel layer on the buffer layer;
[0070] Specifically, in some embodiments, a non-doped GaN layer is grown by MOCVD as a channel layer, and the growth temperature thereof is 1000° C. to 1200° C. and the growth pressure is 50 torr to 500 torr.
[0071] S23: growing an insertion layer on the channel layer;
[0072] Specifically, in some embodiments, an AlN layer is grown by MOCVD as an insertion layer at a growth temperature of 700° C. to 1100° C. and a growth pressure of 100 torr to 200 torr.
[0073] S24: growing a barrier layer on the insertion layer;
[0074] Specifically, in some embodiments, an AlGaN layer is grown by MOCVD as a barrier layer at a growth temperature of 800° C. to 1200° C. and a growth pressure of 100 torr to 200 torr.
[0075] S25: growing a cap layer on the barrier layer.
[0076] Specifically, in some embodiments, a GaN cap layer is grown by MOCVD as the cap layer, with a growth temperature of 700° C. to 1100° C. and a growth pressure of 100 torr to 200 torr.
[0077] Correspondingly, the present invention also provides a HEMT, which includes the above-mentioned HEMT epitaxial wafer.
[0078] The present invention is further described below with specific embodiments:
[0079] Example 1
[0080] This embodiment provides a HEMT epitaxial wafer, which includes a substrate (sapphire), a buffer layer, a channel layer, an insertion layer, a barrier layer and a cap layer stacked in sequence on the substrate.
[0081] Among them, the buffer layer includes a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer and a second AlInGaN layer stacked on the substrate in sequence; the In component ratio in the first AlInGaN layer is 0.05, the Al component ratio is 0.2, and its thickness is 80nm. The B component ratio in the first BGaN layer is 0.3, and its thickness is 50nm. The thickness of the BN layer is 30nm. The B component ratio in the second BGaN layer is 0.3, and its thickness is 50nm. The In component ratio in the second AlInGaN layer is 0.02, the Al component ratio is 0.3, and its thickness is 50nm.
[0082] The channel layer is a non-doped GaN layer with a thickness of 300 nm. The insertion layer is an AlN layer with a thickness of 2 nm. The barrier layer 5 is an AlGaN layer with an Al component ratio of 0.2 and a thickness of 25 nm. The cap layer is a GaN cap layer with a thickness of 4 nm.
[0083] In this embodiment, the HEMT epitaxial wafer is prepared by MOCVD, and the specific preparation method is as follows:
[0084] (1) Providing a substrate;
[0085] (2) growing a buffer layer on a sapphire substrate;
[0086] The growth temperature of the first AlInGaN layer is 950°C and the growth pressure is 200 torr. The growth temperature of the first BGaN layer is 1100°C and the growth pressure is 300 torr. The growth temperature of the BN layer is 1250°C and the growth pressure is 100 torr. The growth temperature of the second BGaN layer is 1100°C and the growth pressure is 300 torr. The growth temperature of the second AlInGaN layer is 1000°C and the growth pressure is 200 torr.
[0087] (3) growing a channel layer on the buffer layer;
[0088] Specifically, a non-doped GaN layer is grown on the buffer layer as a channel layer, and the growth temperature is 1050° C. and the growth pressure is 300 torr.
[0089] (4) growing an insertion layer on the channel layer;
[0090] Specifically, an AlN layer is grown on the channel layer as an insertion layer at a growth temperature of 1100° C. and a growth pressure of 100 torr.
[0091] (5) growing a barrier layer on the insertion layer;
[0092] Specifically, an AlGaN layer is grown on the insertion layer as a barrier layer at a growth temperature of 1120° C. and a growth pressure of 150 Torr.
[0093] (6) Growing a cap layer on the barrier layer.
[0094] Specifically, a GaN cap layer is grown on the barrier layer as a cap layer at a growth temperature of 1000° C. and a growth pressure of 150 torr.
[0095] Example 2
[0096] This embodiment provides a HEMT epitaxial wafer, which is different from the embodiment 1 in that:
[0097] The first AlInGaN layer and the second AlInGaN layer are doped with Mg; the Mg doping concentration in the first AlInGaN layer is 3×10 19 cm -3 ; The Mg doping concentration in the second AlInGaN layer is 8×10 18 cm -3 .
[0098] The rest are the same as in Example 1.
[0099] Example 3
[0100] This embodiment provides a HEMT epitaxial wafer, which differs from Embodiment 2 in that:
[0101] In the first AlInGaN layer, the In content decreases from 0.08 to 0.05, and the Al content increases from 0.2 to 0.3;
[0102] In the second AlInGaN layer, the In composition decreases from 0.02 to 0.01, and the Al composition decreases from 0.3 to 0.1.
[0103] The rest are the same as in Example 2.
[0104] Example 4
[0105] This embodiment provides a HEMT epitaxial wafer, which is different from the embodiment 3 in that:
[0106] The B component ratio in the first BGaN layer is 0.4, and the thickness is 40nm; the B component ratio in the second BGaN layer is 0.2, and the thickness is 45nm.
[0107] The rest is the same as Example 3.
[0108] Comparative Example 1
[0109] This comparative example provides a HEMT epitaxial wafer, which differs from Example 1 in that:
[0110] The first AlInGaN layer and the second AlInGaN layer are not included.
[0111] The rest are the same as in Example 1.
[0112] Comparative Example 2
[0113] This comparative example provides a HEMT epitaxial wafer, which differs from Example 1 in that:
[0114] The first BGaN layer and the second BGaN layer are not included.
[0115] The rest are the same as in Example 1.
[0116] Comparative Example 3
[0117] This comparative example provides a HEMT epitaxial wafer, which differs from Example 1 in that:
[0118] The BN layer is not included.
[0119] The rest are the same as in Example 1.
[0120] Comparative Example 4
[0121] This comparative example provides a HEMT epitaxial wafer, which differs from Example 1 in that:
[0122] The buffer layer is a C-doped GaN layer with a doping concentration of 1×10 20 cm-3 , with a thickness of 2μm. Its growth temperature is 1000℃ and the growth pressure is 200torr.
[0123] The rest are the same as in Example 1.
[0124] The HEMT epitaxial wafers obtained in Examples 1 to 4 and Comparative Examples 1 to 4 were made into HEMTs and tested. The specific results are as follows:
[0125]
[0126] By comparing the test data of Examples 1 to 4 and Comparative Examples 1 to 4, it can be seen that the HEMT epitaxial wafer provided by the present invention inserts a buffer layer of a specific structure between the substrate and the channel layer. Under the above specific structure, the present invention can reduce the leakage current and breakdown voltage of the device and improve the performance and reliability of the device.
[0127] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A HEMT epitaxial wafer, comprising a substrate, a buffer layer, a channel layer, an insertion layer, a barrier layer and a cap layer sequentially stacked on the substrate; It is characterized in that The buffer layer includes a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer and a second AlInGaN layer sequentially stacked on the substrate; The lattice constant of the first AlInGaN layer is greater than the lattice constant of the second AlInGaN layer; The proportion of B component in the first BGaN layer is greater than the proportion of B component in the second BGaN layer, so that the band gap width of the first BGaN layer is greater than the band gap width of the second BGaN layer.
2. The HEMT epitaxial wafer according to claim 1, It is characterized in that The first AlInGaN layer has an In component ratio of 0.01-0.1, an Al component ratio of 0.01-0.3, and a thickness of 10nm-100nm; and / or The second AlInGaN layer has an In component ratio of 0.01-0.1, an Al component ratio of 0.1-0.5, and a thickness of 10nm-100nm.
3. The HEMT epitaxial wafer according to claim 1, It is characterized in that The B component ratio in the first BGaN layer is 0.1-0.5, and the thickness thereof is 10nm-50nm; and / or The thickness of the BN layer is 30nm to 50nm; and / or The B component ratio in the second BGaN layer is 0.1-0.3, and the thickness thereof is 10nm-50nm.
4. The HEMT epitaxial wafer according to any one of claims 1 to 3, It is characterized in that The first AlInGaN layer and the second AlInGaN layer are doped with Mg; The Mg doping concentration in the first AlInGaN layer is 1×10 19 cm -3 ~5×10 19 cm -3 ; The Mg doping concentration in the second AlInGaN layer is 1×10 18 cm -3 ~1×10 19 cm -3 .
5. The HEMT epitaxial wafer according to any one of claims 1 to 3, It is characterized in that Along the growth direction of the HEMT epitaxial wafer, the Al component in the first AlInGaN layer increases and the In component decreases; and / or Along the growth direction of the HEMT epitaxial wafer, the Al component and the In component in the second AlInGaN layer both show a decreasing change.
6. A method for preparing a HEMT epitaxial wafer, for preparing the HEMT epitaxial wafer according to any one of claims 1 to 5, It is characterized in that include: Providing a substrate, and sequentially growing a buffer layer, a channel layer, an insertion layer, a barrier layer, and a cap layer on the substrate; the buffer layer comprises a first AlInGaN layer, a first BGaN layer, a BN layer, a second BGaN layer, and a second AlInGaN layer sequentially stacked on the substrate; The lattice constant of the first AlInGaN layer is greater than the lattice constant of the second AlInGaN layer.
7. The method for preparing a HEMT epitaxial wafer according to claim 6, It is characterized in that The growth temperature of the first AlInGaN layer is 900° C. to 1100° C., and the growth pressure is 50 torr to 500 torr; and / or The growth temperature of the first BGaN layer is 1000° C. to 1200° C., and the growth pressure is 50 torr to 500 torr; and / or The growth temperature of the BN layer is 1100° C. to 1300° C., and the growth pressure is 100 torr to 500 torr; and / or The growth temperature of the second BGaN layer is 1000° C. to 1200° C., and the growth pressure is 50 torr to 500 torr; and / or The growth temperature of the second AlInGaN layer is 900° C. to 1100° C., and the growth pressure is 50 torr to 500 torr.
8. The method for preparing a HEMT epitaxial wafer according to claim 6, It is characterized in that The first AlInGaN layer and the second AlInGaN layer are doped with Mg; During the growth of the first AlInGaN layer and the second AlInGaN layer, the In source is introduced periodically.
9. A HEMT, It is characterized in that Comprising the HEMT epitaxial wafer as described in any one of claims 1 to 5.