Silicon nitride and its preparation method and application
By optimizing the sintering temperature rise curve and gas flow during the preparation process of silicon nitride powder, the hydrogen safety problem and uneven crystal growth problems are solved, and the preparation of silicon nitride powder with high density and high α-Si3N4 content is achieved.
Patent Information
- Application Number
- CN202411233279.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-04
AI Technical Summary
There are safety problems with the use of hydrogen in the existing preparation methods of silicon nitride powder, and step-up temperatures cause silicon nitride crystals to grow too early or too fast, forming short needle-like crystals, affecting product performance.
Under hydrogen-free conditions, by optimizing the heating curve of the second stage of sintering process, adjusting the flow rate of nitrogen and argon in different temperature segments, controlling the nucleation and growth rate of silicon nitride, avoiding local overheating, and promoting complete nitriding of silicon powder. Increase the content of α-Si3N4.
A crystal size with a small particle size and uniform particle size is obtained, the density of silicon nitride products is increased, the generation of needle-shaped silicon nitride (β phase) is inhibited, and the content of α-Si3N4 and the process nitriding rate are improved.
Smart Images

Figure CN118724597B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of ceramic materials, and in particular to silicon nitride and a preparation method and application thereof. Background Art
[0002] Silicon nitride (Si3N4) ceramics not only have high melting point, high hardness, and wear resistance, but also high bending strength and good thermal conductivity. They have been widely used in key areas such as national defense, military industry, and electronics. The key to preparing silicon nitride ceramics with excellent performance is to use silicon nitride powder with high purity, small particle size, and high α-phase content.
[0003] Common methods for preparing silicon nitride powder include direct nitridation of silicon powder, liquid phase method, and self-propagating combustion method. Among them, direct nitridation of silicon powder is considered to be a cheap and simple method for industrial production of silicon nitride powder. At present, mainstream manufacturers at home and abroad usually add hydrogen as a reducing gas to the silicon powder nitridation process to participate in the reaction, help control the reaction temperature and reaction rate, and accelerate the nitridation reaction, thereby increasing the α-phase content in the nitridation product. However, hydrogen has a series of safety issues in industrial production, including but not limited to hydrogen leakage and diffusion, hydrogen explosion, hydrogen control system reliability, pipeline design and installation, etc., which greatly increase the resistance to factory safety production. Therefore, the development of a hydrogen-free nitridation process for silicon powder is crucial for the safe production of high-α-phase silicon nitride.
[0004] The related prior art discloses a method for preparing silicon nitride by hydrogen-free nitridation of silicon powder. The nitridation process of the method is to slowly increase the temperature under the condition of continuously introducing nitrogen to 0.5 bar-1.0 bar, wherein the first heating stage is to increase the temperature to 1180°C-1220°C at 1°C / min-3°C / min and keep it warm for 20h-30h; the second heating stage is to increase the temperature to 1260°C-1300°C at 0.5°C / min-1°C / min and keep it warm for 20h-30h; the third heating stage is to increase the temperature to 1340°C-1380°C at 0.5°C / min-1°C / min and keep it warm for 5h-8h. The above method adopts step-by-step heating, which makes the temperature change faster, which not only causes the silicon nitride crystals in some areas of the furnace to grow prematurely or too fast, thereby forming short needle-shaped crystals (β-silicon nitride), but also causes incomplete nitridation of silicon powder, which ultimately affects the performance of silicon nitride products. Summary of the invention
[0005] The present application provides a method for preparing silicon nitride, which aims to solve at least one of the above problems to a certain extent.
[0006] In a first aspect, the present application provides a method for preparing silicon nitride, comprising the following steps:
[0007] S1. Preparation of silicon block blank
[0008] The silicon powder is mixed with a diluent and a binder and then pressed into a shape to obtain a silicon block blank;
[0009] S2. Preparation of silicon nitride blocks
[0010] The silicon block blank prepared by S1 is placed in a vacuum environment for a first-stage sintering, and then nitrogen and argon are introduced under a slightly positive pressure condition for a second-stage sintering to obtain a silicon nitride block;
[0011] The following process is used in the second stage sintering process:
[0012] S21, introducing nitrogen and argon from 600°C-650°C, with a flow ratio of nitrogen to argon being 5-15:1, and raising the temperature to 900°C-1000°C at a rate of 60°C / h-65°C / h;
[0013] S22, raising the temperature from 900°C-1000°C to 1180°C-1200°C at a rate of 8°C / h-10°C / h, during which the flow ratio of nitrogen to argon is maintained at 5-15:1;
[0014] S23, raising the temperature from 1180°C-1200°C to 1250°C-1290°C at a rate of 2°C / h-2.5°C / h, during which the flow rate of argon gas is increased so that the flow ratio of nitrogen to argon gas is 3-7:1;
[0015] S24, raising the temperature from 1250°C-1290°C to 1320°C-1350°C at a rate of 2.5°C / h-3°C / h, during which the flow rate of argon is reduced so that the flow ratio of nitrogen to argon is 5-15:1;
[0016] S25, raising the temperature from 1320°C-1350°C to 1380°C at a rate of 3°C / h-4°C / h, during which the flow rate of argon is reduced so that the flow ratio of nitrogen to argon is 13-30:1;
[0017] S26, keeping the temperature at 1380°C for 10-12 hours, during which time nitrogen is continuously introduced but argon is stopped;
[0018] The flow rate of nitrogen in S21~S26 is 8L / min-12L / min.
[0019] In an optional embodiment, the flow rate of argon gas in S21 is 0.8 L / min-1.2 L / min.
[0020] In an optional embodiment, the flow rate of argon in S22 is 0.8 L / min-1.2 L / min.
[0021] In an optional embodiment, the flow rate of argon gas in S23 is 1.8 L / min-2.2 L / min.
[0022] In an optional embodiment, the flow rate of argon gas in S24 is 0.8 L / min-1.2 L / min.
[0023] In an optional embodiment, the flow rate of argon gas in S25 is 0.4 L / min-0.6 L / min.
[0024] In an optional embodiment, at least one step of S21 to S26 also includes at least one emptying process, and the relative pressure of the system is 20kPa±5kPa at the end of each emptying, and the relative pressure of the system before and after emptying is maintained at 80kPa±5kPa.
[0025] In an optional embodiment, at least one of steps S24 to S26 further comprises introducing an auxiliary gas, wherein the auxiliary gas comprises helium and / or neon, and the flow rate of the auxiliary gas is 0.4 L / min-0.6 L / min.
[0026] In an optional embodiment, during the first sintering process, the vacuum is evacuated to below 50 Pa, the temperature is raised from room temperature to 600°C-650°C at a rate of 40°C / h-50°C / h, and the vacuum is stopped after maintaining the temperature for 3h-5h.
[0027] In an optional embodiment, in S1, the mixed powder of silicon powder, diluent and binder is first spheroidized to obtain silicon particles, and then the silicon particles are pressed into shape to obtain a silicon block blank.
[0028] In an optional embodiment, the particle size D50 of the silicon particles is 400 μm-800 μm.
[0029] In an optional embodiment, the silicon block blank has a plurality of through holes for gas circulation, and the diameter of the through holes is 6 mm-12 mm.
[0030] In an optional embodiment, the silicon powder is first mixed with the diluent to form an intermediate, and then the intermediate is mixed with the binder to form the mixed powder.
[0031] In an optional embodiment, the mass ratio of the silicon powder to the diluent is 85-95:5-15.
[0032] In an optional embodiment, the particle size D50 of the silicon powder is 3 μm-8 μm, wherein the metal content is less than 0.07%, and the carbon content is less than 0.05%.
[0033] In an optional embodiment, the diluent is silicon nitride, wherein the α-phase content is ≥ 90%.
[0034] In an optional embodiment, the binder is PVB and PEG in a mass ratio of 1:1.
[0035] In an optional embodiment, the mass ratio of the binder to the intermediate is 5-10:95-90.
[0036] In an optional embodiment, the compression molding includes using a pressure of 0.1 MPa-0.5 MPa and maintaining the pressure for 10s-30s.
[0037] In an optional embodiment, the preparation method further comprises S3 preparing silicon nitride powder, crushing the silicon nitride blocks prepared in S2 into silicon nitride powder with a particle size D50≤0.6 μm by dry crushing and closed refining process.
[0038] In a second aspect, the present application provides a silicon nitride powder, which is prepared using the silicon nitride preparation method described in the first aspect of the present application.
[0039] In an optional embodiment, in the silicon nitride powder, the α-Si3N4 content is above 94%, the oxygen content does not exceed 0.6%, the carbon content does not exceed 0.1%, and the free silicon content does not exceed 0.05%.
[0040] In a third aspect, the present application also provides the use of the silicon nitride powder described in the second aspect of the present application in the preparation of ceramic products.
[0041] The technical solution of this application has the following advantages:
[0042] The preparation method of silicon nitride provided in the present application optimizes the heating curve of the second sintering process and adjusts the flow rates of nitrogen and argon in different temperature sections under hydrogen-free conditions. On the one hand, it can better control the nucleation and growth rates of silicon nitride, thereby obtaining a smaller and uniform crystal size, showing good fragility and a narrower particle size distribution during the crushing process, which is beneficial to improving the density of the silicon nitride product; on the other hand, it can also avoid local overheating, which leads to the appearance of liquid phase, inhibits the formation of needle-shaped silicon nitride (β phase), and thus increases the content of α-Si3N4; thirdly, in the hydrogen-free silicon powder nitriding process, the use of a slowly heating nitriding system compared to a step-heating nitriding system can form a silicon nitride film on the surface of the silicon powder and then gradually carry out a nitriding reaction into the silicon powder, thereby promoting the complete nitridation of the silicon powder as much as possible, thereby improving the process nitriding rate.
[0043] Additional aspects and advantages of the embodiments of the present application will be described and shown in part in the subsequent description, or explained through the implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0045] Figure 1 This is the XRD diagram of the silicon nitride powder prepared in Example 1 of the present application.
[0046] Figure 2 This is the XRD diagram of the silicon nitride powder prepared in Example 2 of the present application.
[0047] Figure 3 This is the XRD diagram of the silicon nitride powder prepared in Example 3 of the present application.
[0048] Figure 4 This is the XRD diagram of the silicon nitride powder prepared in Example 4 of the present application.
[0049] Figure 5 This is the XRD diagram of the silicon nitride powder prepared in Example 5 of the present application.
[0050] Figure 6 This is the XRD diagram of the silicon nitride powder prepared in Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0051] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the description and claims of this application and any variations thereof are intended to cover non-exclusive inclusions.
[0053] In the description of the embodiments of the present application, “plurality” means more than two, unless otherwise clearly and specifically defined.
[0054] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0055] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0056] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0057] The actual reaction process of preparing silicon nitride powder by silicon powder nitridation is very complicated. On the one hand, the theoretical temperature of silicon powder nitridation to generate silicon nitride powder is very close to the melting point of silicon. On the other hand, the silicon powder nitridation reaction is a strong exothermic reaction. It is easy to cause local overheating to cause silicon powder melting, silicon overflow and liquid phase. The liquid phase will fill the gaps between the silicon powders and block the diffusion of nitrogen, affecting the smooth progress of the nitridation reaction. Therefore, in the process of preparing silicon nitride powder by silicon powder nitridation, hydrogen is often used to eliminate the factors that hinder nitridation of the silicon powder oxide layer and reduce the temperature of the initial reaction, but the use of hydrogen will bring a series of safety problems. The related prior art proposes a method for preparing silicon nitride by hydrogen-free nitridation of silicon powder, which adopts a temperature control process of three-stage slow heating and two-stage slow cooling, but the results show that this method will not only cause silicon nitride crystals in certain areas of the furnace to grow prematurely or too quickly, thereby forming short needle-shaped crystals (β-silicon nitride), but also cause incomplete nitridation of silicon powder, ultimately affecting the performance of silicon nitride products.
[0058] In order to solve the problems existing in the above-mentioned related art, according to the first aspect of the present application, a method for preparing silicon nitride is provided, comprising the following steps:
[0059] S1. Preparation of silicon block blank
[0060] The silicon powder is mixed with a diluent and a binder and then pressed into a shape to obtain a silicon block blank;
[0061] S2. Preparation of silicon nitride blocks
[0062] The silicon block blank prepared by S1 is placed in a vacuum environment for a first-stage sintering, and then nitrogen and argon are introduced under a slightly positive pressure condition for a second-stage sintering to obtain a silicon nitride block;
[0063] The following process is used in the second stage sintering process:
[0064] S21, introducing nitrogen and argon from 600°C-650°C, with a flow ratio of nitrogen to argon being 5-15:1, and raising the temperature to 900°C-1000°C at a rate of 60°C / h-65°C / h;
[0065] As an example, the S21 starting temperature may be, for example, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, etc., or within the range formed by any two of the above values, the flow ratio of nitrogen to argon may be 5:1, 7:1, 9:1, 11:1, 13:1, 15:1, etc., or within the range formed by any two of the above values, the heating rate may be, for example, 60°C / h, 61°C / h, 62°C / h, 63°C / h, 64°C / h, 65°C / h, etc., or within the range formed by any two of the above values, the S21 endpoint temperature may be 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, etc., or within the range formed by any two of the above values;
[0066] S22, raising the temperature from 900°C-1000°C to 1180°C-1200°C at a rate of 8°C / h-10°C / h, during which the flow ratio of nitrogen to argon is maintained at 5-15:1;
[0067] As an example, the S22 starting temperature may be, for example, 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, etc., or within the range formed by any two of the above values, the flow ratio of nitrogen to argon may be 5:1, 7:1, 9:1, 11:1, 13:1, 15:1, etc., or within the range formed by any two of the above values, the heating rate may be, for example, 8°C / h, 8.5°C / h, 9°C / h, 9.5°C / h, 10°C / h, etc., or within the range formed by any two of the above values, the S22 endpoint temperature may be 1180°C, 1185°C, 1190°C, 1195°C, 1200°C, etc., or within the range formed by any two of the above values;
[0068] S23, raising the temperature from 1180°C-1200°C to 1250°C-1290°C at a rate of 2°C / h-2.5°C / h, during which the flow rate of argon gas is increased so that the flow ratio of nitrogen to argon gas is 3-7:1;
[0069] As an example, the starting temperature of S23 may be, for example, 1180°C, 1185°C, 1190°C, 1195°C, 1200°C, etc., or within the range formed by any two of the above values, the flow ratio of nitrogen to argon may be 3:1, 4:1, 5:1, 6:1, 7:1, etc., or within the range formed by any two of the above values, the heating rate may be, for example, 2°C / h, 2.1°C / h, 2.2°C / h, 2.3°C / h, 2.4°C / h, 2.5°C / h, etc., or within the range formed by any two of the above values, and the end temperature of S23 may be 1250°C, 1260°C, 1270°C, 1280°C, 1290°C, etc., or within the range formed by any two of the above values;
[0070] S24, raising the temperature from 1250°C-1290°C to 1320°C-1350°C at a rate of 2.5°C / h-3°C / h, during which the flow rate of argon is reduced so that the flow ratio of nitrogen to argon is 5-15:1;
[0071] As an example, the starting temperature of S24 may be, for example, 1250°C, 1260°C, 1270°C, 1280°C, 1290°C, etc., or within the range formed by any two of the above values, the flow ratio of nitrogen to argon may be 5:1, 7:1, 9:1, 11:1, 13:1, 15:1, etc., or within the range formed by any two of the above values, the heating rate may be, for example, 2.5°C / h, 2.6°C / h, 2.7°C / h, 2.8°C / h, 2.9°C / h, 3°C / h, etc., or within the range formed by any two of the above values, and the end temperature of S24 may be 1320°C, 1330°C, 1340°C, 1350°C, etc., or within the range formed by any two of the above values;
[0072] S25, raising the temperature from 1320°C-1350°C to 1380°C at a rate of 3°C / h-4°C / h, during which the flow rate of argon is reduced so that the flow ratio of nitrogen to argon is 13-30:1;
[0073] As an example, the starting temperature of S25 may be, for example, 1320°C, 1330°C, 1340°C, 1350°C, etc., or within the range formed by any two of the above values. The flow ratio of nitrogen to argon may be 13:1, 15:1, 17:1, 19:1, 21:1, 23:1, 25:1, 27:1, 30:1, etc., or within the range formed by any two of the above values. The heating rate may be, for example, 3°C / h, 3.2°C / h, 3.4°C / h, 3.6°C / h, 3.8°C / h, 4°C / h, etc., or within the range formed by any two of the above values.
[0074] S26, keeping the temperature at 1380°C for 10-12 hours, during which time nitrogen is continuously introduced but argon is stopped;
[0075] The flow rate of nitrogen in S21~S26 is 8L / min-12L / min;
[0076] As an example, the insulation time of S26 can be 10h, 10.5h, 11h, 11.5h, 12h, etc. or within the range of any two of the above values. In S21~S26, the nitrogen flow rate can be, for example, 8L / min, 9L / min, 10L / min, 11L / min, 12L / min, etc. or within the range of any two of the above values.
[0077] Research has shown that the nitridation reaction of silicon powder can be roughly divided into three stages: in the first stage, nitrogen molecules are adsorbed on the silicon surface and react with surface silicon atoms to form a silicon nitride film; in the second stage, the silicon nitride film has a certain thickness, which will isolate the nitrogen and silicon participating in the reaction. At this time, silicon and nitrogen must diffuse to the Si / Si3N4 interface driven by chemical potential difference to react, which involves two processes in this stage, one is diffusion and the other is reaction. Therefore, the growth factor of the silicon nitride film is jointly determined by the above two processes; in the third stage, after a thick and dense silicon nitride film is formed on the silicon surface, it is difficult for nitrogen atoms to diffuse through the silicon nitride film to reach the Si / Si3N4 interface and then react. At this time, the growth factor of the silicon nitride film is mainly determined by the diffusion of atoms. Based on this, the present application subdivides and optimizes the second stage sintering process into six temperature stages: S21 is to heat up to the reaction temperature at a faster rate after the completion of the first stage sintering; S22 is to slowly heat up to allow the silicon powder nitriding reaction to proceed initially, and use the residual carbon produced by the first stage sintering to remove the oxide layer on the surface of the silicon powder; S23 is to eliminate the oxide layer on the surface of the silicon powder, and the nitriding reaction is more intense, so it is necessary to increase the content of the diluent gas (argon) and reduce the heating rate, thereby slowing down the reaction rate and avoiding silicon overflow. In addition, the slow heating in the low temperature stage is more conducive to the formation of the α phase, and the α-Si3N4 formed at this time can also act as a diluent; Since the α-Si3N4 formed in the early stage can reduce the heat accumulation phenomenon, the heating rate can be slightly increased and the dilution gas content can be reduced in step S24 to promote the spread of the nitridation reaction inside the silicon block body, so that more silicon powder can generate α-Si3N4; further, in S25, the heating rate is gradually increased, and the dilution gas content is reduced at the same time to accelerate the diffusion of nitrogen atoms through the silicon nitride film to reach the Si / Si3N4 interface for further reaction, thereby promoting complete nitridation of silicon powder and reducing the free silicon content; then S26 removes the argon gas and keeps the temperature at 1380°C for a period of time to ensure that the silicon powder is completely nitrided and improve the uniformity of the silicon powder nitridation throughout the furnace. In summary, by optimizing the second stage sintering process, the temperature / temperature field, gas flow rate and pressure are precisely controlled at different nitriding stages. On the one hand, silicon overflow can be avoided, ensuring that the silicon block can be fully nitrided, achieving uniform temperature inside the silicon block, and ensuring batch stability of the silicon nitride block; on the other hand, it can also avoid the transformation of α-silicon nitride to β-silicon nitride, thereby controlling the α phase content of the silicon nitride powder to more than 94%, the oxygen content not exceeding 0.6%, the carbon content not exceeding 0.1%, and the free silicon content not exceeding 0.05%. At the same time, by controlling the nitrogen flow rate between 8L / min-12L / min, sufficient nitrogen raw materials can be provided for the nitridation reaction of silicon powder. This application study found that if the nitrogen flow rate is too large, the nitridation reaction rate of silicon powder will be too fast, causing silicon overflow. On the contrary, if the nitrogen flow rate is too small, the nitridation reaction rate of silicon powder will be too slow, extending the nitridation time, and the small nitrogen flow rate may cause the silicon powder to be unable to be completely nitrided.
[0078] Therefore, the preparation method of silicon nitride provided in the present application, by optimizing the heating curve of the second sintering process and adjusting the flow rates of nitrogen and argon in different temperature sections under hydrogen-free conditions, can better control the nucleation and growth rates of silicon nitride on the one hand, thereby obtaining a smaller and uniform crystal size, which exhibits good fragility and a narrower particle size distribution in the subsequent crushing process, and is beneficial to improving the density of the silicon nitride product; on the other hand, it can also avoid local overheating, which leads to the appearance of liquid phase, inhibits the formation of needle-shaped silicon nitride (β phase), and thus increases the content of α-Si3N4; thirdly, in the hydrogen-free silicon powder nitriding process, the use of a slow heating nitriding system compared to a step-heating nitriding system can form a silicon nitride film on the surface of the silicon powder and then gradually carry out a nitriding reaction into the silicon powder, thereby promoting the complete nitridation of the silicon powder as much as possible, thereby improving the process nitriding rate.
[0079] From the analysis of the kinetic theory mechanism, the nitridation of silicon powder is in the interface chemical control stage when the temperature rises to 100℃-1100℃. Therefore, the present application controls the nitrogen flow rate unchanged after 1100℃ and adjusts the dilution gas (argon) flow rate to better control the reaction rate. When the dilution gas flow rate is too much, the raw silicon powder reacts incompletely, the product agglomerates seriously, and the powder particle size range becomes wider; when the dilution gas flow rate is too little, the nitridation reaction is accelerated, the α phase in the product begins to transform into the β phase, and the β-silicon nitride is rod-shaped, which increases the powder particle size and the β phase, which is not conducive to the sintering and densification of ceramic products in the later stage. In some embodiments, the flow rate of argon gas in S21 is 0.8L / min-1.2L / min. As an example, the flow rate of nitrogen gas in S21 can be, for example, 0.8L / min, 0.9L / min, 1.0L / min, 1.1L / min, 1.2L / min, etc., or within the range formed by any two of the above values; in some embodiments, the flow rate of argon gas in S22 is 0.8L / min-1.2L / min. As an example, the flow rate of nitrogen gas in S22 can be, for example, 0.8L / min, 0.9L / min, 1.0L / min, 1.1L / min, 1.2L / min, etc., or within the range formed by any two of the above values; in some embodiments, the flow rate of argon gas in S23 is 1.8L / min-2.2L / min. As an example, the flow rate of nitrogen gas in S23 can be, for example, 1.8L / min, 1.9 L / min, 2.0 L / min, 2.1 L / min, 2.2 L / min, etc., or within the range formed by any two of the above values; in some embodiments, the flow rate of argon in S24 is 0.8 L / min-1.2 L / min. As an example, the flow rate of nitrogen in S24 can be, for example, 0.8 L / min, 0.9 L / min, 1.0 L / min, 1.1 L / min, 1.2 L / min, etc., or within the range formed by any two of the above values; in some embodiments, the flow rate of argon in S25 is 0.4 L / min-0.6 L / min. As an example, the flow rate of nitrogen in S25 can be, for example, 0.4 L / min, 0.45 L / min, 0.5 L / min, 0.55 L / min, 0.6 L / min, etc., or within the range formed by any two of the above values.
[0080] In an optional embodiment, at least one step of S21 to S26 also includes at least one emptying treatment, and the relative pressure of the system at the end of each emptying is 20kPa±5kPa. On the one hand, the gas in the nitriding furnace can be in a flowing state, thereby promoting the uniformity of the gas in the furnace and ensuring complete nitridation of the silicon powder; on the other hand, some by-products or impurity gases may be produced during the reaction, and the purity of the product can be improved by emptying treatment; thirdly, since the nitridation reaction of silicon powder is an exothermic reaction, the exhausted gas can take away part of the heat produced by the reaction to avoid silicon overflow; as an example, the relative pressure of the system after each emptying can be 15kPa, 17kPa, 20kPa, 23kPa, 25kPa, etc., or within the range formed by any two of the above values. The relative pressure of the system before and after emptying is maintained at 80kPa±5kPa, which is to assist nitrogen to directly contact silicon particles through the reaction products, and this pressure value has low requirements for nitriding equipment (low-pressure container) and a high safety factor; as an example, the system pressure before and after emptying can be 75kPa, 77kPa, 80kPa, 83kPa, 85kPa, etc. or within the range of any two of the above values. It can be understood that in S21~S26, the number of emptying times needs to be reasonably determined according to the speed of the silicon powder nitriding reaction. In some embodiments, S21~S26 need to be emptied once first, and can also be 2 times, 5 times, 6 times, 8 times, 10 times, etc. or within the range of any two of the above values. In the actual nitriding process, it needs to be dynamically adjusted according to the reaction rate.
[0081] The present application has found that after a thick and dense silicon nitride film has been formed on the silicon surface in the second half of the nitridation reaction, it is difficult for nitrogen atoms to diffuse through the silicon nitride film to reach the interface. Therefore, the present application introduces an auxiliary gas in at least one of steps S24 to S26. The auxiliary gas includes helium and / or neon. Since helium and neon have small atomic radii, they have high diffusion mobility and high permeability. During the silicon powder nitridation reaction, helium and / or neon can penetrate into the silicon nitride film and silicon powder, assisting nitrogen atoms to pass through the surface silicon nitride film to reach the Si / Si3N4 interface. On the one hand, it can promote the continuous progress of the nitridation reaction, ensure complete nitridation of silicon powder, improve the overall uniformity of silicon nitride powder, and improve the process nitridation rate. On the other hand, it can also increase the α phase content in the silicon nitride product. In some embodiments, the flow rate of the auxiliary gas is 0.4L / min-0.6L / min. As an example, the flow rate of the auxiliary gas can be 0.4L / min, 0.45L / min, 0.5L / min, 0.55L / min, 0.6L / min, etc. or within the range of any two of the above values.
[0082] It is understandable to those skilled in the art that when silicon powder is used as a raw material to react with nitrogen, since the particle size of silicon powder is very small, it is easy to be carried away by the airflow, which will have many adverse effects on product collection, tail gas purification, etc. Therefore, the relevant prior art first presses the silicon powder into a silicon block and then nitrides it. However, considering that directly pressing the silicon powder will make the density of the silicon block too large, it is not conducive to the nitrogen to enter the interior of the silicon block during nitridation. Therefore, the present application proposes to first spheroidize the silicon powder to obtain silicon particles, and then press the silicon particles into shape, so as to increase the porosity between the particles inside the silicon block, increase the nitrogen channel, and avoid being pressed too densely, so that the temperature is not easy to diffuse, resulting in temperature accumulation between the particles during the nitridation process. The phenomenon of silicon overflow occurs. In some embodiments, the particle size D50 of the silicon particles is 400μm-800μm. As an example, the particle size D50 of the silicon particles can be, for example, 400μm, 500μm, 600μm, 700μm, 800μm, etc. or within the range of any two of the above values.
[0083] In order to further increase the nitrogen channels in the silicon block and avoid heat accumulation, in some embodiments, the silicon block blank also has a plurality of through holes for gas circulation, and the diameter of the through holes is 6mm-12mm. It can be understood by those skilled in the art that the center of the mold used for pressing and molding in S1 is provided with N (N≥4) protrusions, for example, 8 cylinders, arranged in a circle, and correspondingly, the silicon block blank pressed by the mold has N through holes inside; in some embodiments, the volume of the mold is, for example, 190-210mm*90-110mm*40-60mm.
[0084] The powder blank making process of the present application utilizes the low-temperature plasticity of the binder to press the silicon powder into shape in a mold without the need for powder loading in a sagger and manual pressing, which greatly reduces the cost of manual furnace loading and improves the level of automated production of the production line. The hole design of the mold makes the temperature inside each blank uniform, promotes the flow of gas inside the blank, and increases the batch stability of silicon nitride in each furnace.
[0085] It is understood by those skilled in the art that adding a diluent to silicon powder can not only absorb most of the heat generated by the silicon-nitrogen reaction, hinder the formation of the liquid phase in the nitridation process, and avoid the occurrence of silicon overflow, but also make it easier to obtain growth nuclei in the early stage of the reaction, thereby promoting a faster nitridation rate. At the same time, in order to facilitate the compression molding of silicon powder, it is usually necessary to add an appropriate amount of binder, and the activated carbon formed by the binder at high temperature can also react with the oxide layer on the surface of the silicon powder to reduce the oxygen content of silicon nitride, so that the prepared silicon nitride product has a higher nitridation rate and α-phase content, and the oxygen content is relatively low. In some embodiments, in order to fully mix the silicon powder and the diluent, the silicon powder and the diluent can be mixed to form an intermediate, and then the intermediate can be mixed with the binder to form a mixed powder.
[0086] In an optional embodiment, the particle size D50 of the silicon powder is 3 μm-8 μm, wherein the metal content is less than 0.07%, and the carbon content is less than 0.05%. As an example, the particle size D50 of the silicon powder can be 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, etc., or within a range formed by any two of the above values.
[0087] In an optional embodiment, the mass ratio of the silicon powder to the diluent is 85-95:5-15. As an example, the mass ratio of silicon powder to the diluent can be 85:15, 82:18, 90:10, 93:7, 95:5, etc., or within the range of any two of the above values.
[0088] In an optional embodiment, the diluent is silicon nitride, wherein the α-phase content is ≥ 90%.
[0089] In an optional embodiment, the mass ratio of the binder to the intermediate is 5-10:95-90. As an example, the mass ratio of the binder to the intermediate can be 5:95, 6:94, 7:93, 8:92, 9:91, 10:90, etc. or within the range of any two of the above values.
[0090] In an optional embodiment, the binder is PVB and PEG in a mass ratio of 1:1. By adding PVB and PEG in equal mass, the silicon powder can be pressed and formed in the mold, which greatly reduces the cost of manual furnace loading and can also make the granulated powder have better sphericity and surface smoothness.
[0091] In an optional embodiment, the compression molding includes using a pressure of 0.1 MPa-0.5 MPa and maintaining the pressure for 10s-30s.
[0092] The silicon block blank prepared by S1 is placed in a vacuum environment for the first stage of sintering. The first stage of sintering can volatilize the organic binder in the silicon block blank by vacuum degreasing, further increasing the gas flowability in the silicon block, avoiding temperature accumulation inside the particles, and fully nitriding the silicon powder, thereby increasing the α-phase content of the silicon nitride powder. In an optional embodiment, during the first stage of sintering, the vacuum is evacuated to below 50Pa, the temperature is raised from room temperature to 600℃-650℃ at a rate of 40℃ / h-50℃ / h, and the vacuum is stopped after keeping the temperature for 3h-5h. As an example, the heating rate in the first sintering process can be 40℃ / h, 42℃ / h, 44℃ / h, 46℃ / h, 48℃ / h, 50℃ / h, etc., or within the range formed by any two of the above values; the sintering temperature can be 600℃, 610℃, 620℃, 630℃, 640℃, 650℃, etc., or within the range formed by any two of the above values; the holding time can be 3h, 3.5h, 4h, 4.5h, 5h, etc., or within the range formed by any two of the above values.
[0093] In an optional embodiment, the preparation method further includes S3 preparing silicon nitride powder, and using a dry crushing and closed refining process to crush the silicon nitride blocks obtained in S2 into silicon nitride powder with a particle size D50≤0.6μm. Compared with the traditional wet crushing and refining process, the dry crushing and closed refining process not only has the advantages of short process flow, low manufacturing cost, and high production safety, but also can regulate the oxygen content in the silicon nitride powder to meet the needs of high-end silicon nitride products. In some embodiments, the dry crushing and closed refining process includes using equipment such as a double-roll mill, a vibration mill, and an air flow mill (without adding alcohol) to crush and refine the silicon nitride blocks.
[0094] In a second aspect, the present application provides a silicon nitride powder, which is prepared using the silicon nitride preparation method described in the first aspect of the present application.
[0095] In an optional embodiment, in the silicon nitride powder, the α-Si3N4 content is above 94%, the oxygen content does not exceed 0.6%, the carbon content does not exceed 0.1%, and the free silicon content does not exceed 0.05%.
[0096] In a third aspect, the present application also provides the use of the silicon nitride powder described in the second aspect of the present application in the preparation of ceramic products.
[0097] The present application is further described in detail below in conjunction with specific examples, which should not be construed as limiting the scope of protection claimed in the present application. In all examples and comparative examples of the present application, the unit % represents the mass percentage content.
[0098] Example 1
[0099] The method for preparing silicon nitride powder provided in this embodiment comprises the following steps:
[0100] S1. Preparation of silicon block
[0101] S11, firstly, silicon powder and diluent are mixed uniformly at a mass ratio of 86:14 to obtain an intermediate, and then the intermediate and binder are mixed at a mass ratio of 92:8 to form a mixed powder; wherein,
[0102] The particle size D50 of silicon powder is about 4μm, the metal content is less than 0.07%, and the carbon content is less than 0.05%; the diluent is silicon nitride powder, in which the α phase content is ≥90%; the binder is PVB and PEG with a mass ratio of 1:1;
[0103] S12, spheroidizing the mixed powder obtained in S11 to obtain silicon particles with a particle size D50 of about 500 μm;
[0104] S13, placing the silicon particles obtained in S12 in a mold (volume 200 mm*100 mm*50 mm, with 8 cylinders arranged at the center), pressing and molding with a pressure of 0.4 MPa and maintaining the pressure for 15 seconds to obtain a silicon block green body;
[0105] S2. Preparation of silicon nitride blocks
[0106] The silicon block blanks prepared by S13 were placed on a graphite base plate, with 9 silicon blocks in length, 6 silicon blocks in width, and 8 silicon blocks in height. The first stage of sintering and debinding was carried out under the condition of vacuuming to below 50Pa, with the starting temperature being room temperature, the heating rate being 46℃ / h, heating to 610℃, and stopping vacuuming after keeping at 610℃ for 3h.
[0107] The material after the first stage of sintering is subjected to the second stage of sintering nitriding, specifically:
[0108] S21, heating from 610°C to 950°C, heating rate 65°C / h, introducing nitrogen and argon at 610°C, nitrogen flow rate 10L / min, argon flow rate 1L / min; evacuating twice, evacuating to a pressure of 20±5kPa, and maintaining the pressure at 80±5kPa before and after evacuation;
[0109] S22, heating from 950°C to 1200°C, heating rate 10°C / h; nitrogen flow rate 10L / min, argon flow rate 1L / min; evacuation 5 times, evacuation to pressure 20±5kPa, pressure maintained at 80±5kPa before and after evacuation; this step slowly heats up, silicon powder nitridation is preliminarily carried out and residual carbon is used to remove the oxide layer on the surface of silicon powder;
[0110] S23, heating from 1200°C to 1270°C, heating rate 2.4°C / h, nitrogen flow rate 10L / min, argon flow rate 2L / min; evacuating 8 times, evacuating to a pressure of 20±5kPa, and maintaining the pressure at 80±5kPa before and after evacuation; the nitridation reaction in this step is more intense, and it is necessary to increase the dilution gas content and reduce the heating rate to reduce the reaction rate and avoid silicon overflow;
[0111] S24, heating from 1270°C to 1330°C, heating rate 2.9°C / h, nitrogen flow rate 10L / min, argon flow rate 1.0L / min, and helium flow rate 0.5L / min; evacuate 6 times, evacuate to a pressure of 20±5kPa, and keep the insulation pressure at 80±5kPa; since the silicon nitride powder formed in the early stage can be used as a diluent to reduce heat accumulation, this step can slightly increase the heating rate, reduce the dilution gas content, and introduce helium at the same time to assist nitrogen atoms to pass through the surface silicon nitride film into the Si / Si3N4 interface for reaction, thereby promoting the nitridation reaction;
[0112] S25, heating from 1330°C to 1380°C, heating rate 3.9°C / h, nitrogen flow rate 10L / min, argon flow rate 0.5L / min, helium flow rate 0.5L / min; evacuate 5 times, evacuate to pressure 20±5kPa, keep insulation pressure at 80±5kPa; this step gradually increases heating rate, reduces dilution gas, accelerates nitrogen atoms diffusion through silicon nitride film to reach Si / Si3N4 interface and then reacts, promotes complete nitridation of silicon powder, and improves uniformity of silicon powder nitridation throughout the furnace;
[0113] S26, keep warm at 1380℃ for 10h, with a nitrogen flow rate of 10L / min and a helium flow rate of 0.5L / min; evacuate twice to a pressure of 20±5kPa, and keep the insulation pressure at 80±5kPa; stop sintering and cool naturally to room temperature; this step removes the diluent gas, and keeping warm at 1380℃ for 10h can promote complete nitridation of silicon powder;
[0114] S3. Preparation of silicon nitride powder
[0115] The reaction product of S26 was taken out and finally obtained high-purity ultrafine silicon nitride powder with a median particle size of ≤0.55μm through a dry crushing and closed refinement process. Its XRD spectrum is shown in Figure 1 .
[0116] Example 2
[0117] The method for preparing silicon nitride powder provided in this embodiment comprises the following steps:
[0118] S1. Preparation of silicon block
[0119] S11, firstly, silicon powder and diluent are mixed uniformly at a mass ratio of 90:10 to obtain an intermediate, and then the intermediate and binder are mixed at a mass ratio of 95:5 to form a mixed powder; wherein,
[0120] The particle size D50 of silicon powder is about 6μm, the metal content is less than 0.07%, and the carbon content is less than 0.05%; the diluent is silicon nitride powder, in which the α phase content is ≥90%; the binder is PVB and PEG with a mass ratio of 1:1;
[0121] S12, spheroidizing the mixed powder obtained in S11 to obtain silicon particles with a particle size D50 of about 400 μm;
[0122] S13, placing the silicon particles obtained in S12 in a mold (volume is 200 mm*100 mm*50 mm, and 8 cylinders are arranged at the center thereof), pressing and molding with a pressure of 0.3 MPa and maintaining the pressure for 20 seconds to obtain a silicon block green body;
[0123] S2. Preparation of silicon nitride blocks
[0124] S21, placing the silicon block blanks obtained in S13 on a graphite base plate, with 9 silicon blocks in length, 6 silicon blocks in width, and 8 silicon blocks in height; performing the first stage of sintering and debinding under the condition of evacuating to below 50Pa, with the starting temperature being room temperature, the heating rate being 44°C / h, heating to 650°C, and stopping evacuating after keeping at 650°C for 3h;
[0125] The material after the first stage sintering is subjected to the second stage sintering nitriding, specifically:
[0126] S21, heating from 650°C to 980°C, heating rate 63°C / h, introducing nitrogen and argon at 650°C, nitrogen flow rate 8L / min, argon flow rate 1.2L / min; evacuating twice, evacuating to a pressure of 20±5kPa, and maintaining the pressure at 80±5kPa before and after evacuation;
[0127] S22, heating from 980°C to 1190°C, heating rate 9°C / h; nitrogen flow rate 8L / min, argon flow rate 1.2L / min; evacuation 5 times, evacuation to pressure 20±5kPa, pressure maintained at 80±5kPa before and after evacuation; this step slowly heats up, silicon powder nitridation is preliminarily carried out and residual carbon is used to remove the oxide layer on the surface of silicon powder;
[0128] S23, heating from 1190°C to 1280°C, heating rate 2.2°C / h, nitrogen flow rate 8L / min, argon flow rate 2.2L / min; evacuating 8 times, evacuating to a pressure of 20±5kPa, and maintaining the pressure at 80±5kPa before and after evacuation; the nitridation reaction in this step is more intense, and it is necessary to increase the dilution gas content and reduce the heating rate to reduce the reaction rate and avoid silicon overflow;
[0129] S24, heating from 1280°C to 1340°C, heating rate 2.7°C / h, nitrogen flow rate 10L / min, argon flow rate 1.2L / min, and helium flow rate 0.6L / min; evacuate 6 times, evacuate to a pressure of 20±5kPa, and keep the insulation pressure at 80±5kPa; since the silicon nitride powder formed in the early stage can be used as a diluent to reduce heat accumulation, the heating rate can be slightly increased in this step, the dilution gas content can be reduced, and helium can be introduced at the same time to assist nitrogen atoms to pass through the surface silicon nitride film and enter the Si / Si3N4 interface for reaction, thereby promoting the nitridation reaction;
[0130] S25, heating from 1340°C to 1380°C, heating rate 3.6°C / h, nitrogen flow rate 8L / min, argon flow rate 0.6L / min, helium flow rate 0.6L / min; evacuate 5 times, evacuate to pressure 20±5kPa, keep insulation pressure at 80±5kPa; this step gradually increases heating rate, reduces dilution gas, accelerates nitrogen atoms diffusion through silicon nitride film to reach Si / Si3N4 interface and then reacts, promotes complete nitridation of silicon powder, and improves uniformity of silicon powder nitridation throughout the furnace;
[0131] S26, keep warm at 1380℃ for 11h, with a nitrogen flow rate of 8L / min and a helium flow rate of 0.6L / min; evacuate twice to a pressure of 20±5kPa, and keep the insulation pressure at 80±5kPa; stop sintering and cool naturally to room temperature; this step removes the diluent gas, and keeping warm at 1380℃ for 11h can promote complete nitridation of silicon powder;
[0132] S3. Preparation of silicon nitride powder
[0133] The reaction product of S26 was taken out and finally obtained high-purity ultrafine silicon nitride powder with a median particle size of ≤0.6μm through a dry crushing and closed refinement process. Its XRD spectrum is shown in Figure 2 .
[0134] Example 3
[0135] The method for preparing silicon nitride powder provided in this embodiment comprises the following steps:
[0136] S1. Preparation of silicon block
[0137] S11, firstly, silicon powder and diluent are mixed uniformly at a mass ratio of 95:5 to obtain an intermediate, and then the intermediate and binder are mixed at a mass ratio of 90:10 to form a mixed powder; wherein,
[0138] The particle size D50 of silicon powder is about 8μm, the metal content is less than 0.07%, and the carbon content is less than 0.05%; the diluent is silicon nitride powder, in which the α phase content is ≥90%; the binder is PVB and PEG with a mass ratio of 1:1;
[0139] S12, spheroidizing the mixed powder obtained in S11 to obtain silicon particles with a particle size D50 of about 800 μm;
[0140] S13, placing the silicon particles obtained in S12 in a mold (volume 200 mm*100 mm*50 mm, with 8 cylinders arranged at the center), pressing and molding with a pressure of 0.2 MPa and maintaining the pressure for 15 seconds to obtain a silicon block green body;
[0141] S2. Preparation of silicon nitride blocks
[0142] S21, placing the silicon block blanks obtained in S13 on a graphite base plate, with 9 silicon blocks in length, 6 silicon blocks in width, and 8 silicon blocks in height; performing the first stage of sintering and degreasing under the condition of vacuuming to below 50Pa, with the starting temperature being room temperature, the heating rate being 42°C / h, heating to 650°C, and stopping vacuuming after keeping the temperature at 650°C for 3h;
[0143] The material after the first stage sintering is subjected to the second stage sintering nitriding, specifically:
[0144] S21, heating from 650°C to 1000°C, heating rate 61°C / h, introducing nitrogen and argon at 650°C, nitrogen flow rate 12L / min, argon flow rate 0.8L / min; evacuating twice, evacuating to a pressure of 20±5kPa, and maintaining the pressure at 80±5kPa before and after evacuation;
[0145] S22, heating from 1000°C to 1180°C, heating rate 8°C / h; nitrogen flow rate 12L / min, argon flow rate 1.2L / min; evacuation 5 times, evacuation to pressure 20±5kPa, pressure maintained at 80±5kPa before and after evacuation; this step slowly heats up, silicon powder nitridation is preliminarily carried out and residual carbon is used to remove the oxide layer on the surface of silicon powder;
[0146] S23, heating from 1180°C to 1290°C, heating rate 2°C / h, nitrogen flow rate 12L / min, argon flow rate 1.8L / min; evacuating 8 times, evacuating to a pressure of 20±5kPa, and maintaining the pressure at 80±5kPa before and after evacuation; the nitridation reaction in this step is more intense, and it is necessary to increase the dilution gas content and reduce the heating rate to reduce the reaction rate and avoid silicon overflow;
[0147] S24, heating from 1290°C to 1350°C, heating rate 2.5°C / h, nitrogen flow rate 12L / min, argon flow rate 0.8L / min, and helium flow rate 0.4L / min; evacuate 6 times, evacuate to a pressure of 20±5kPa, and keep the insulation pressure at 80±5kPa; since the silicon nitride powder formed in the early stage can be used as a diluent to reduce heat accumulation, the heating rate can be slightly increased in this step, the dilution gas content can be reduced, and helium can be introduced at the same time to assist nitrogen atoms to pass through the surface silicon nitride film and enter the Si / Si3N4 interface for reaction, thereby promoting the nitridation reaction;
[0148] S25, heating from 1350°C to 1380°C, heating rate 3.1°C / h, nitrogen flow rate 12L / min, argon flow rate 0.4L / min, helium flow rate 0.4L / min; evacuate 5 times, evacuate to pressure 20±5kPa, keep insulation pressure at 80±5kPa; this step gradually increases heating rate, reduces dilution gas, accelerates nitrogen atoms diffusion through silicon nitride film to reach Si / Si3N4 interface and then reacts, promotes complete nitridation of silicon powder, and improves uniformity of silicon powder nitridation throughout the furnace;
[0149] S26, keep warm at 1380℃ for 12h, with a nitrogen flow rate of 12L / min and a helium flow rate of 0.4L / min; evacuate twice to a pressure of 20±5kPa, and keep the insulation pressure at 80±5kPa; stop sintering and cool naturally to room temperature; this step removes the diluent gas, and keeping warm at 1380℃ for 12h can promote complete nitridation of silicon powder;
[0150] S3. Preparation of silicon nitride powder
[0151] The reaction product of S26 was taken out and finally obtained high-purity ultrafine silicon nitride powder with a median particle size of ≤0.6μm through a dry crushing and closed refinement process. Its XRD spectrum is shown in Figure 3 .
[0152] Example 4
[0153] It is basically the same as Example 1, except that neon gas is used instead of helium gas in S24-S26.
[0154] Finally, high-purity ultrafine silicon nitride powder with a median particle size of ≤0.6μm was obtained, and its XRD spectrum is shown in Figure 4 .
[0155] Example 5
[0156] It is basically the same as Example 1, except that helium is not introduced.
[0157] Finally, high-purity ultrafine silicon nitride powder with a median particle size of ≤0.6μm was obtained, and its XRD spectrum is shown in Figure 5 .
[0158] Comparative Example 1
[0159] It is basically the same as Example 5, except that the second stage sintering nitriding is specifically as follows:
[0160] From 610℃ to 950℃, the heating rate is 50℃ / h. At 950℃, nitrogen and argon are introduced. The nitrogen flow rate is 9.2L / min and the argon flow rate is 1.72L / min. From 950℃ to 1200℃, the heating rate is 26℃ / h. Keep at 1200℃ for 55h. The nitrogen flow rate is 19.0L / min and the argon flow rate is 3.5L / min. Evacuate 6 times and the evacuation pressure is The temperature was kept at 1270℃ for 24h, with a nitrogen flow rate of 19.0L / min and an argon flow rate of 3.5L / min. The vacuum was evacuated 4 times to a pressure of 30kPa, and the insulation pressure was kept at 50±2kPa. The temperature was raised from 1200℃ to 1270℃ at a heating rate of 18℃ / h, with a nitrogen flow rate of 9.2L / min and an argon flow rate of 1.72L / min. The vacuum was kept at 1270℃ for 24h, with a nitrogen flow rate of 19.0L / min and an argon flow rate of 3.5L / min. The vacuum was evacuated 4 times to a pressure of 30kPa, and the insulation pressure was kept at Maintain 50±2kPa; increase from 1270℃ to 1330℃, the heating rate is 16℃ / h, the nitrogen flow rate is 9.2L / min, and the argon flow rate is 1.72L / min; keep at 1330℃ for 23h, the nitrogen flow rate is 19.0L / min, the argon flow rate is 3.5L / min, evacuate 4 times, evacuate to the pressure below 30kPa, and the insulation pressure is 50±2kPa; increase from 1330℃ to 1380℃, the heating rate is 16℃ / h, the nitrogen flow rate is 9.2L / min, and the argon flow rate is 1.72L / min; keep at 1380℃ for 10 hours, the nitrogen flow rate is 19.0L / min, the argon flow rate is 3.5L / min, evacuate 3 times, the evacuation pressure is below 30kPa, and the insulation pressure is 50±2kPa; stop sintering and return to room temperature for 11 hours.
[0161] Finally, ultrafine silicon nitride powder with a median particle size of ≤0.6μm was obtained, and its XRD spectrum is shown in Figure 6 .
[0162] Test Case
[0163] Silicon nitride powder was sampled and measured at seven locations in the whole furnace of Examples 1-5 and Comparative Example 1, and the results are shown in Tables 1-6.
[0164] Table 1 Quality of silicon nitride powder in Example 1
[0165]
[0166] Table 2 Quality of silicon nitride powder in Example 2
[0167]
[0168] Table 3 Quality of silicon nitride powder in Example 3
[0169]
[0170] Table 4 Quality of silicon nitride powder in Example 4
[0171]
[0172] Table 5 Quality of silicon nitride powder in Example 5
[0173]
[0174] Table 6 Quality of silicon nitride powder in Comparative Example 1
[0175]
[0176] It can be seen from Tables 1 to 6 that the α-phase content in the silicon nitride powders prepared in Examples 1 to 3 is all greater than 94wt%, the free silicon content is ≤0.05wt%, and the test data at different sampling positions are less discrete, which indicates that the silicon powder nitriding process of the present invention, which adopts slow heating and reasonably controls the ratio of nitrogen and argon gases during the heating process, and introduces helium in the second half of the nitriding reaction, has the advantages of high silicon powder nitriding rate, high α-phase content and good batch stability, thereby making the silicon nitride powder prepared by the present invention have good sintering activity.
[0177] Compared with Example 1, Example 4 uses neon, so that the free silicon content of Example 4 is higher than that of Example 1, indicating that helium is better than neon in promoting the diffusion of nitrogen atoms through the silicon nitride film to reach the Si / Si3N4 interface. This is because the atomic radius of helium is smaller than that of neon, and it is easier to penetrate into the silicon nitride film and silicon powder, thereby assisting nitrogen atoms to pass through the surface silicon nitride film to reach the Si / Si3N4 interface for nitridation reaction, thereby improving the process nitridation rate. Compared with Example 1, Example 5 does not use helium in the second half of the nitridation reaction, and the α-phase content in the silicon nitride powder prepared thereby is slightly lower than that in Example 1, and the free silicon content is slightly higher than that in Example 1, which indicates that the addition of helium during the nitridation reaction is conducive to the reaction of nitrogen with the internal silicon powder through the reaction product, thereby improving the silicon powder conversion rate and the α-phase content in silicon nitride.
[0178] Compared with Example 5, Comparative Example 1 adopts step-by-step heating, and the α-phase content in the prepared silicon nitride powder is less than 94wt%, the free silicon content is greater than 0.15wt%, and the data dispersion tested at different sampling positions is relatively high, indicating that this process is inferior to the silicon powder nitriding process of the present invention.
[0179] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A method for preparing silicon nitride, characterized in that: The steps include: S1. Preparation of silicon block blank The silicon powder is mixed with a diluent and a binder and then pressed into a shape to obtain a silicon block blank; In S1, a mixed powder of silicon powder, a diluent and a binder is first spheroidized to obtain silicon particles, and then the silicon particles are pressed into shape to obtain a silicon block blank; the particle size D50 of the silicon particles is 400 μm-800 μm, and the silicon block blank has a plurality of through holes for gas flow, and the diameter of the through holes is 6 mm-12 mm; wherein, The silicon powder is first mixed with the diluent to form an intermediate, and then the intermediate is mixed with the binder to form the mixed powder; the mass ratio of the silicon powder to the diluent is 85-95:5-15; the particle size D50 of the silicon powder is 3μm-8μm, wherein the metal content is less than 0.07%, and the carbon content is less than 0.05%; the diluent is silicon nitride, wherein the α phase content is ≥90%; the binder is PVB and PEG with a mass ratio of 1:1; the mass ratio of the binder to the intermediate is 5-10:95-90; S2. Preparation of silicon nitride blocks The silicon block blank prepared by S1 is placed in a vacuum environment for a first-stage sintering, and then nitrogen and argon are introduced under a slightly positive pressure condition for a second-stage sintering to obtain a silicon nitride block; The following process is used in the second stage sintering process: S21, introducing nitrogen and argon from 600°C-650°C, with a flow ratio of nitrogen to argon being 5-15:1, and raising the temperature to 900°C-1000°C at a rate of 60°C / h-65°C / h; S22, raising the temperature from 900°C-1000°C to 1180°C-1200°C at a rate of 8°C / h-10°C / h, during which the flow ratio of nitrogen to argon is maintained at 5-15:1; S23, raising the temperature from 1180°C-1200°C to 1250°C-1290°C at a rate of 2°C / h-2.5°C / h, during which the flow rate of argon gas is increased so that the flow ratio of nitrogen to argon gas is 3-7:1; S24, raising the temperature from 1250°C-1290°C to 1320°C-1350°C at a rate of 2.5°C / h-3°C / h, during which the flow rate of argon is reduced so that the flow ratio of nitrogen to argon is 5-15:1; S25, raising the temperature from 1320°C-1350°C to 1380°C at a rate of 3°C / h-4°C / h, during which the flow rate of argon is reduced so that the flow ratio of nitrogen to argon is 13-30:1; S26, keeping the temperature at 1380°C for 10-12 hours, during which time nitrogen is continuously introduced but argon is stopped; The flow rate of nitrogen in S21~S26 is 8L / min-12L / min; S3. Preparation of silicon nitride powder The silicon nitride blocks obtained from S2 are crushed into silicon nitride powder with a particle size D50≤0.6μm by dry crushing and closed refining process; in the silicon nitride powder, the α-Si3N4 content is above 94%, the oxygen content does not exceed 0.6%, the carbon content does not exceed 0.1%, and the free silicon content does not exceed 0.05%.
2. The method for preparing silicon nitride according to claim 1, characterized in that: The flow rate of argon in S21 is 0.8L / min-1.2L / min; and / or, the flow rate of argon gas in S22 is 0.8 L / min-1.2 L / min; and / or, the flow rate of argon gas in S23 is 1.8 L / min-2.2 L / min; and / or, the flow rate of argon gas in S24 is 0.8 L / min-1.2 L / min; And / or, the flow rate of argon gas in S25 is 0.4L / min-0.6L / min.
3. The method for preparing silicon nitride according to claim 1, characterized in that: At least one of the steps S21 to S26 further includes at least one emptying process, and the relative pressure of the system at the end of each emptying is 20 kPa±5 kPa, and the relative pressure of the system before and after the emptying is maintained at 80 kPa±5 kPa; And / or, at least one of steps S24 to S26 further comprises introducing an auxiliary gas, wherein the auxiliary gas comprises helium and / or neon, and the flow rate of the auxiliary gas is 0.4 L / min-0.6 L / min.
4. The method for preparing silicon nitride according to claim 1, characterized in that: During the first stage of sintering, the vacuum is evacuated to below 50 Pa, the temperature is raised from room temperature to 600°C-650°C at a rate of 40°C / h-50°C / h, and the vacuum is stopped after the temperature is kept for 3h-5h.
5. The method for preparing silicon nitride according to claim 1, characterized in that: The compression molding includes using a pressure of 0.1 MPa-0.5 MPa and maintaining the pressure for 10s-30s.
6. A silicon nitride powder, prepared by the method for preparing silicon nitride according to any one of claims 1 to 5.
7. Use of the silicon nitride powder according to claim 6 in the preparation of ceramic products.