Polyaniline-based composite material as well as preparation method and application thereof
Through alkaline pretreatment and freeze-drying of PANI-based materials combined with rapid plasma sintering, bulk composite materials are prepared, which solves the problems of complex processes and unstable performance in the existing technology, and achieves efficient electromagnetic wave absorption performance and Good mechanical properties.
Patent Information
- Application Number
- CN202411062927.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-11
AI Technical Summary
The preparation process of existing PANI-based electromagnetic absorbing materials is complex, the molding processability is poor, and the performance is unstable in extreme environments.
The preparation method of polyaniline-based composite materials includes reacting aniline monomer with an initiator in an acidic solution, followed by pretreatment in an alkaline solution, followed by dispersion with magnetic metal nanopowder and freeze-drying and rapid plasma sintering. Forming bulk composite materials.
It improves the density and mechanical properties of the material, maintains the nanoscale microstructure, and enhances the wave absorption performance. The process is simple and stable, and is suitable for large-scale production.
Smart Images

Figure CN118755263A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wave absorbing materials, and in particular to a polyaniline-based composite material and a preparation method and application thereof. Background Art
[0002] With the rapid development of the fifth generation of wireless systems and electronic communication equipment, potential electromagnetic interference and radiation pollution have brought many adverse effects on sensitive precision electronic products and human health. Therefore, in recent years, the research on high-performance absorbing materials to eliminate the negative impact of electromagnetic waves has been booming. Polyaniline (PANI) is a typical conductive polymer, which is widely studied due to its advantages such as easy synthesis, excellent thermal stability, low cost, and good redox performance. Magnetic metal materials such as Co, Ni and their alloys have large saturation magnetization and high Snoke limit, and the resonance frequency is in the GHz band, and are widely used in the field of absorbing waves. Good impedance matching is a key factor in consuming incident microwaves. The composite of PANI and magnetic materials can provide a prerequisite for the smooth entry of electromagnetic waves into the material for attenuation. At the same time, the introduction of magnetic materials can produce a magneto-dielectric synergistic effect while playing their own absorbing role, achieving an effect of one plus one greater than two. Therefore, the preparation of PANI and magnetic material composites and their dissipation mechanism have attracted widespread attention from researchers.
[0003] At present, most of the research on PANI-based electromagnetic absorbing materials is based on powdered PANI composite materials. However, powdered composite materials have complex preparation processes, the raw materials of the composite functional enhanced second phase are expensive, and the molding processability is poor in the subsequent practical application process, and the performance is unstable in extreme service environments such as high temperature. Therefore, it is of great significance to develop a new PANI-based absorbing material with simple process, which can be used in extreme environments and is easy to process and use in subsequent processing. Summary of the invention
[0004] In view of the problems of existing powdery composite materials such as complex preparation process, poor molding processability, and unstable performance that cannot be used in extreme environments, the present invention provides a polyaniline-based composite material and a preparation method and application thereof.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] In a first aspect, the present invention provides a method for preparing a polyaniline-based composite material, comprising the following steps:
[0007] Step a, adding aniline monomer and initiator into an acidic solution, reacting, solid-liquid separation, washing, and obtaining PANI material;
[0008] Step b, adding the PANI material into an alkaline solution, reacting, solid-liquid separation, and washing to obtain a pretreated PANI material;
[0009] Step c, dispersing the pretreated PANI material and magnetic metal nanopowder into water to obtain a dispersion; freeze-drying the dispersion, and then performing rapid discharge plasma sintering to obtain a polyaniline-based composite material.
[0010] Compared with the prior art, the preparation method of the polyaniline-based composite material provided by the present invention firstly pre-treats the PANI material with alkali to improve the formability of the material in subsequent sintering, avoids the problem of pores on the surface of the material during the sintering process, improves the compactness of the sintered body, and further improves the mechanical properties of the material; then, the pre-treated PANI material and the magnetic metal nano-powder are freeze-dried and then subjected to discharge plasma sintering to obtain a bulk PANI-based composite material, wherein freeze-drying can avoid the agglomeration of the magnetic metal nano-powder during the drying process, maintain the uniform dispersion of the magnetic nano-metal powder in the PANI matrix, thereby facilitating the formation of a uniform conductive network in the PANI matrix; and the powder after freeze-drying has a regular porous structure inside, which is conducive to the escape of gas in the subsequent sintering process, thereby helping to obtain a dense sintered body; and rapid plasma sintering can effectively inhibit the excessive growth of grains during the sintering process, maintain the nano-scale microstructure of the material, retain the microporous structure in the material while ensuring the compactness of the material, and improve the wave absorption performance of the material.
[0011] The preparation method of the polyaniline-based composite material provided by the present invention is simple to operate, has a stable process, high production efficiency, can achieve high automation, and the prepared composite material has good density, uniformity and stability. In addition, the prepared block material is more conducive to actual processing and use than traditional powder materials, and has high practical value.
[0012] Furthermore, in step a, the mass ratio of the aniline monomer to the initiator is 1:1.5 to 1:2.5.
[0013] Furthermore, in step a, the mass volume ratio of the aniline monomer to the acidic solution is 10 g: (350-450) mL.
[0014] Furthermore, in step a, the concentration of the acidic solution is 1 mol / L to 2 mol / L.
[0015] Furthermore, in step a, the initiator is ammonium persulfate.
[0016] Furthermore, in step a, the acidic solution is a hydrochloric acid solution.
[0017] Furthermore, in step a, the reaction temperature is 0°C to 5°C, and the reaction time is 4h to 8h.
[0018] Furthermore, in step b, the mass volume ratio of the PANI material to the alkaline solution is 4 g:1 L to 6 g:1 L.
[0019] Furthermore, in step b, the alkaline solution is 0.1 mol / L to 0.2 mol / L ammonia water or sodium hydroxide solution.
[0020] Furthermore, in step b, the reaction temperature is 25° C. to 40° C., and the reaction time is 18 h to 30 h.
[0021] Pre-treating the prepared PANI material with an alkaline solution can avoid the appearance of pores on the material surface during the subsequent sintering process, which would lead to poor stability and formability of the material, and is beneficial to improving the mechanical properties of the molded material.
[0022] It should be noted that in step b, a drying step is also included after washing, and the drying can be carried out by freeze-drying. The specific freeze-drying process parameters can be routinely adjusted by those skilled in the art, and the present invention does not make any special limitations.
[0023] Furthermore, in step c, the magnetic nano-metal powder is nickel powder, and its particle size is 80nm to 120nm.
[0024] Furthermore, in step c, the mass ratio of the pretreated PANI material to the magnetic metal nanopowder is 7:1 to 20:1.
[0025] Furthermore, in step c, the concentration of the pretreated PANI material in the dispersion is 8 g / L to 12 g / L.
[0026] Magnetic metal nanoparticles with high conductivity are used to form a good conductive network structure inside the PANI material. At the same time, magnetic metals have strong magnetic loss capabilities, which is beneficial to improving the attenuation ability of electromagnetic waves in the material and improving the material's wave absorption ability.
[0027] Furthermore, in step c, the freeze-drying temperature is -70°C to -50°C, and the freeze-drying time is 48h to 96h.
[0028] By freeze-drying followed by rapid spark plasma sintering and controlling the spark plasma sintering process, an appropriate amount of microporous structure can be introduced into the dense PANI-based material to increase the dielectric loss and polarization loss, thereby improving the material's microwave absorption performance.
[0029] Furthermore, in step c, the rapid discharge plasma sintering temperature is 130° C. to 150° C., the heating rate is 30° C. / min to 50° C. / min, the pressure is 60 MPa to 80 MPa, and the holding time is 3 min to 5 min.
[0030] By controlling the above-mentioned rapid sintering plasma process, the excessive growth of grains during the sintering process can be effectively suppressed, and the nano-scale microstructure of the material can be maintained. At the same time, by controlling the parameters such as the heating rate, sintering temperature and pressure, it is also beneficial to obtain a PANI-based composite material with uniform and fine structure and moderate density, and obtain a PANI-based composite material with excellent microwave absorption and mechanical properties. The block material obtained by rapid plasma sintering is conducive to subsequent processing and use, and has higher practicality.
[0031] In a second aspect, the present invention further provides a polyaniline-based composite material, which is prepared by any of the above-mentioned methods for preparing the polyaniline-based composite material.
[0032] In a third aspect, the present invention also provides the use of the above-mentioned polyaniline-based composite material as an absorbing material in aircraft stealth, electromagnetic absorption, electromagnetic protection or microwave darkroom.
[0033] The present invention provides a method for preparing a novel bulk absorbing material. The PANI matrix material is pretreated and combined with a freeze-drying and rapid discharge plasma sintering method to composite the PANI matrix material with a magnetic metal material. The prepared bulk absorbing material has excellent electromagnetic absorbing performance, and the best absorbing efficiency can reach about 28.55 dB in the X-band (8.2-12.4 GHz), and can cover the entire X-band. At the same time, the preparation method of the PANI-based composite material provided by the present invention has a simple and easy process, can be produced in large specifications, and has opened up a new way for the structural design and optimization of high-performance absorbing materials. It has broad application prospects in the fields of electromagnetic absorption, electromagnetic safety protection, etc. of communication equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 XRD diagram of the Ni / PANI composite material prepared in Example 1 of the present invention;
[0035] Figure 2 This is a SEM image of the Ni / PANI composite material prepared in Example 1 of the present invention;
[0036] Figure 3 The three-dimensional reflection loss spectrum of the Ni / PANI composite material prepared in Example 1 of the present invention as a function of frequency and thickness;
[0037] Figure 4A two-dimensional reflection loss spectrum of the Ni / PANI composite material prepared in Example 1 of the present invention as a function of frequency and thickness;
[0038] Figure 5 A three-dimensional reflection loss spectrum of the Ni / PANI composite material prepared in Example 2 of the present invention as a function of frequency and thickness;
[0039] Figure 6 A two-dimensional reflection loss spectrum of the Ni / PANI composite material prepared in Example 2 of the present invention as a function of frequency and thickness;
[0040] Figure 7 A three-dimensional reflection loss spectrum of the Ni / PANI composite material prepared in Comparative Example 1 of the present invention as the frequency and thickness change;
[0041] Figure 8 A two-dimensional reflection loss spectrum of the Ni / PANI composite material prepared in Comparative Example 1 of the present invention as a function of frequency and thickness;
[0042] Fig. 9 Optical photographs of the Ni / PANI bulk composite materials prepared in Example 1 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0044] In order to better illustrate the present invention, further examples are given below.
[0045] Unless otherwise specified, the raw materials and reagents used in the following examples and comparative examples are commercially available products.
[0046] The nickel powder used in the following examples and comparative examples is a spherical nickel powder with a diameter of about 100 nm, and the manufacturer is Qinghe County Top Metal Materials Co., Ltd.
[0047] Example 1
[0048] A method for preparing a Ni / PANI bulk composite material comprises the following steps:
[0049] Step a, adding 10 mL of aniline to 200 mL of 1 mol / L hydrochloric acid solution to obtain an aniline solution; adding 20 g of ammonium persulfate to 200 mL of 1 mol / L hydrochloric acid solution and stirring to dissolve to obtain an ammonium persulfate solution; adding the aniline solution and the ammonium persulfate solution to a three-necked flask, stirring and reacting at 0° C. for 5 hours, filtering after the reaction, washing with water until the liquid is colorless, and then adding the above sample to 0.1 mol / L ammonia water at a solid-liquid ratio of 5 g:1 L, stirring and reacting at room temperature for 24 hours, filtering with suction, washing with water and ethanol, and freeze-drying to obtain PANI powder;
[0050] Step b, dispersing PANI powder in water to obtain a PANI dispersion with a concentration of 10 mg / mL; adding nickel powder to the PANI dispersion, wherein the mass ratio of nickel powder to PANI powder is 1:7, ultrasonically dispersing for 30 minutes, and then magnetically stirring for 3 hours, and then freeze-drying the dispersion at -70°C for 48 hours to obtain Ni / PANI composite material powder;
[0051] Step c, subjecting the Ni / PANI composite material powder to rapid discharge plasma sintering, wherein the sintering temperature is 150° C., the heating rate is 50° C. / min, the pressure is 60 MPa, and the insulation time is 3 min, to obtain a Ni / PANI bulk composite material.
[0052] The XRD patterns of the PANI powder and Ni / PANI bulk composite material prepared in step a of this embodiment are shown in FIG. Figure 1 As shown in the figure, it can be seen that 25.7° corresponds to the characteristic peak of PANI powder; when compounded with nickel nanoparticles, additional characteristic diffraction peaks of Ni appear, which are 44.507°, 51.846°, and 76.37°, respectively, corresponding to the standard PDF card of nickel (04-0850), which proves that the bulk Ni / PANI composite material was successfully synthesized.
[0053] The SEM image of the Ni / PANI bulk composite material prepared in this example is shown in Figure 2 As shown in the figure, it can be seen that PANI is a cluster morphology formed by short rods, and the Ni nanoparticles are spherical and evenly distributed in the PANI matrix.
[0054] The Ni / PANI bulk composite material prepared in the example was tested for electromagnetic parameters in the range of 8.2 to 12.4 GHz (X band) using the waveguide method. The test mold size was 22.84 mm × 10.14 mm. The wave absorption efficiency values of the test samples at different thicknesses were calculated based on the measured S scattering parameters, dielectric constant (ε) and magnetic permeability (μ). Figure 3-4The three-dimensional reflection loss diagram and two-dimensional reflection loss diagram of the Ni / PANI bulk composite material vary with frequency and thickness. The strongest absorption reflection loss of this material is -28.55dB at a thickness of 1.61mm, and full coverage of the X-band can be achieved at 1.78mm.
[0055] The mechanical properties of the Ni / PANI bulk composite material prepared above were tested using a mechanical testing machine, model EM6.103-T, 1KN. Each sample was tested at least three times at room temperature. Among them, the flexural strength was tested using a three-point bending test method. The sample was cut into strips of 10mm×2mm×2mm and polished with sandpaper. The loading rate was 0.6mm / min and the support span was 7.75mm. The fracture toughness was tested using the single-edge notched beam (SENB) method. The sample (10mm×2mm×2mm) was cut to about half the width using a low-speed diamond saw. The test was carried out at a loading rate of 0.06mm / min and the support span was 7.75mm. The final test sample had a flexural strength of 173.4MPa and a fracture toughness of 5.1MPa m 1 / 2 .
[0056] It is proved that the electromagnetic absorbing material of the present invention can have stronger electromagnetic absorbing performance at a thinner thickness. Compared with the powdered PANI-based electromagnetic absorbing material, the block-shaped electromagnetic absorbing material of the present invention has good mechanical properties and strong processability.
[0057] Example 2
[0058] A method for preparing a Ni / PANI bulk composite material comprises the following steps:
[0059] Step a, adding 10 mL of aniline to 200 mL of 2 mol / L hydrochloric acid solution to obtain an aniline solution; adding 15 g of ammonium persulfate to 150 mL of 2 mol / L hydrochloric acid solution and stirring to dissolve to obtain an ammonium persulfate solution; adding the aniline solution and the ammonium persulfate solution to a three-necked flask, stirring and reacting at 5° C. for 4 hours, filtering after the reaction is completed, washing with water until the liquid is colorless, and then adding the above sample to 0.1 mol / L ammonia water at a solid-liquid ratio of 6 g:1 L, stirring and reacting at room temperature for 18 hours, filtering, washing with water and ethanol, and freeze-drying to obtain PANI powder;
[0060] Step b, dispersing PANI powder in water to obtain a PANI dispersion with a concentration of 12 mg / mL; adding nickel powder to the PANI dispersion, wherein the mass ratio of nickel powder to PANI powder is 1:15, ultrasonically dispersing for 30 minutes, and then magnetically stirring for 3 hours, and then freeze-drying the dispersion at -50°C for 96 hours to obtain a Ni / PANI composite material powder;
[0061] Step c, subjecting the Ni / PANI composite material powder to rapid discharge plasma sintering, wherein the rapid discharge plasma sintering temperature is 130°C, the heating rate is 30°C / min, the pressure is 80MPa, and the insulation time is 5min, to obtain a Ni / PANI bulk composite material.
[0062] The electromagnetic parameters of the samples prepared in this embodiment were tested in the range of 8.2 to 12.4 GHz (X band) using the waveguide method. Figure 5-6 The three-dimensional reflection loss diagram and two-dimensional reflection loss diagram of the Ni / PANI bulk composite material vary with frequency and thickness. At a thickness of 1.65mm, the strongest absorption reflection loss of this material can reach -26.41dB, and full coverage of the X-band can be achieved at 1.80mm.
[0063] The flexural strength of the tested sample is 232.6MPa and the fracture toughness is 5.6MPa m 1 / 2 .
[0064] Example 3
[0065] A method for preparing a Ni / PANI bulk composite material comprises the following steps:
[0066] Step a, adding 10 mL of aniline to 200 mL of 1.5 mol / L hydrochloric acid solution to obtain an aniline solution; adding 25 g of ammonium persulfate to 250 mL of 1.5 mol / L hydrochloric acid solution and stirring to dissolve to obtain an ammonium persulfate solution; adding the aniline solution and the ammonium persulfate solution to a three-necked flask, stirring and reacting at 2° C. for 6 hours, filtering after the reaction, washing with water until the liquid is colorless, and then adding the above sample to 0.2 mol / L ammonia water at a solid-liquid ratio of 4g:1L, stirring and reacting at room temperature for 30 hours, filtering, washing with water and ethanol, and freeze-drying to obtain PANI powder;
[0067] Step b, dispersing PANI powder in water to obtain a PANI dispersion with a concentration of 8 mg / mL; adding nickel powder to the PANI dispersion, wherein the mass ratio of nickel powder to PANI powder is 1:20, ultrasonically dispersing for 30 minutes, and then magnetically stirring for 3 hours, and then freeze-drying the dispersion at -60°C for 72 hours to obtain a Ni / PANI composite material powder;
[0068] Step c, subjecting the above-mentioned Ni / PANI composite material powder to rapid discharge plasma sintering, wherein the discharge frequency is 500kHz, the pulse current is 100A~500A, the pulse voltage is 1V~6V, the temperature is 140°C, the heating rate is 40°C / min, the pressure is 70MPa, and the insulation time is 4min to obtain a Ni / PANI bulk composite material.
[0069] The electromagnetic parameters of the sample prepared in this embodiment were tested by waveguide method in the range of 8.2-12.4 GHz (X band). The strongest absorption reflection loss of the material was -24.1 dB at a thickness of 1.71 mm, and full coverage of the X band was achieved at 1.84 mm.
[0070] The flexural strength of the tested sample is 282MPa and the fracture toughness is 6.1MPa m 1 / 2 .
[0071] Comparative Example 1
[0072] This comparative example provides a method for preparing a Ni / PANI bulk composite material, which is different from Example 1 only in that the mass ratio of nickel powder to PANI powder is replaced with 1:100, and the remaining steps and conditions are exactly the same as those in Example 1, which will not be repeated here.
[0073] See also Figure 7 and Figure 8 The minimum reflection loss of the Ni / PANI bulk composite material prepared in this comparative example is -11.22 dB, while the minimum reflection losses of the Ni / PANI bulk composite materials prepared in Examples 1 to 3 are all lower than -25 dB, which proves that the mass ratio of Ni to polyaniline selected within a specific range in the present invention can effectively improve the wave absorbing performance of the composite material.
[0074] Comparative Example 2
[0075] This comparative example provides a method for preparing a Ni / PANI bulk composite material, which is different from Example 1 only in that the alkali treatment step is omitted. The specific steps are as follows:
[0076] Step a, adding 10 mL of aniline to 200 mL of 1 mol / L hydrochloric acid solution to obtain an aniline solution; adding 20 g of ammonium persulfate to 200 mL of 1 mol / L hydrochloric acid solution and stirring to dissolve to obtain an ammonium persulfate solution; adding the aniline solution and the ammonium persulfate solution to a three-necked flask, stirring and reacting at 0° C. for 5 hours, filtering after the reaction is completed, washing with water until the liquid is colorless, and freeze-drying to obtain PANI powder;
[0077] Step b, dispersing PANI powder in water to obtain a PANI dispersion with a concentration of 10 mg / mL; adding nickel powder to the PANI dispersion, wherein the mass ratio of nickel powder to PANI powder is 1:9, ultrasonically dispersing for 30 minutes, and then magnetically stirring for 3 hours, and then freeze-drying the dispersion at -70°C for 48 hours to obtain Ni / PANI composite material powder;
[0078] Step c, subjecting the Ni / PANI composite material powder to rapid discharge plasma sintering, wherein the sintering temperature is 150° C., the heating rate is 50° C. / min, the pressure is 60 MPa, and the insulation time is 3 min, to obtain a Ni / PANI bulk composite material.
[0079] See also Fig. 9 The comparison of the optical photographs of the block samples of Example 1 and Comparative Example 2 shows that the surface of the block sample prepared in Example 1 is smoother ( Fig. 9 (a)), while the surface of the block sample prepared in Comparative Example 2 has obvious bulging phenomenon ( Fig. 9 (b)), which will have a serious impact on the mechanical properties of the samples.
[0080] In summary, the NI / PANI-based composite material provided by the present invention has a maximum absorption intensity of -28.55dB at 1.61mm; the effective absorption bandwidth covers the entire X-band at 1.78mm, and the maximum absorption intensity reaches -20dB. In addition, the preparation process of the material of the present invention is simple, and the block material has the advantages of good stability, good mechanical properties, and strong processability, and has higher practical application value.
[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a polyaniline-based composite material, characterized in that: The steps include: Step a, adding aniline monomer and initiator into an acidic solution, reacting, solid-liquid separation, washing, and obtaining PANI material; Step b, adding the PANI material into an alkaline solution, reacting, solid-liquid separation, and washing to obtain a pretreated PANI material; Step c, dispersing the pretreated PANI material and magnetic metal nanopowder into water to obtain a dispersion; freeze-drying the dispersion, and then performing rapid discharge plasma sintering to obtain a polyaniline-based composite material.
2. The method for preparing the polyaniline-based composite material according to claim 1, characterized in that: In step a, the mass ratio of the aniline monomer to the initiator is 1:1.5 to 1:2.5; and / or In step a, the mass volume ratio of the aniline monomer to the acidic solution is 10 g: (350-450) mL; and / or In step a, the concentration of the acidic solution is 1 mol / L to 2 mol / L.
3. The method for preparing the polyaniline-based composite material according to claim 1, characterized in that: In step a, the initiator is ammonium persulfate; and / or In step a, the acidic solution is a hydrochloric acid solution.
4. The method for preparing the polyaniline-based composite material according to any one of claims 1 to 3, characterized in that: In step a, the reaction temperature is 0°C to 5°C, and the reaction time is 4h to 8h.
5. The method for preparing the polyaniline-based composite material according to claim 1, characterized in that: In step b, the mass volume ratio of the PANI material to the alkaline solution is 4 g:1 L to 6 g:1 L; and / or In step b, the alkaline solution is 0.1 mol / L to 0.2 mol / L ammonia water or sodium hydroxide solution.
6. The method for preparing the polyaniline-based composite material according to claim 1 or 5, characterized in that: In step b, the reaction temperature is 25° C. to 40° C., and the reaction time is 18 h to 30 h.
7. The method for preparing a polyaniline-based composite material according to claim 1, characterized in that: In step c, the mass ratio of the pretreated PANI material to the magnetic metal nanopowder is 7:1 to 20:1; and / or In step c, the concentration of the pretreated PANI material in the dispersion is 8 g / L to 12 g / L; and / or In step c, the magnetic nano-metal powder is nickel powder, and its particle size is 80nm to 120nm.
8. The method for preparing the polyaniline-based composite material according to claim 1, characterized in that: In step c, the freeze-drying temperature is -70°C to -50°C, and the freeze-drying time is 48h to 96h; and / or In step c, the rapid discharge plasma sintering temperature is 130° C. to 150° C., the heating rate is 30° C. / min to 50° C. / min, the pressure is 60 MPa to 80 MPa, and the insulation time is 3 min to 5 min.
9. A polyaniline-based composite material, characterized in that: The polyaniline-based composite material is prepared by the preparation method of any one of claims 1 to 8.
10. Use of the polyaniline-based composite material according to claim 9 as an absorbing material in aircraft stealth, electromagnetic absorption, electromagnetic protection or microwave darkroom.