Iron-silicon magnetic powder composite material and preparation thereof, iron-silicon magnetic powder core and preparation and application of iron-silicon magnetic powder core

By coating and passivating the insulating powder of ferrosilicon magnetic powder, the problem of high loss of ferrosilicon magnetic powder composite materials in the prior art is solved, better insulation and magnetic properties are achieved, and the loss of ferrosilicon magnetic powder core is reduced. , improving the energy-saving efficiency of the device.

CN119049823APending Publication Date: 2024-11-29HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411246898.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29

Smart Images

  • Figure BDA0005031038970000151
    Figure BDA0005031038970000151
  • Figure BDA0005031038970000161
    Figure BDA0005031038970000161
Patent Text Reader

Abstract

The invention provides an iron-silicon magnetic powder composite material and preparation thereof, an iron-silicon magnetic powder core and preparation and application thereof, and the preparation method comprises the following steps: coating iron-silicon magnetic powder with insulating powder to obtain an intermediate, and passivating the obtained intermediate for at least one time to obtain the iron-silicon magnetic powder composite material. According to the preparation method provided by the invention, after the iron-silicon magnetic powder is coated with the insulating powder to form the insulating coating layer, passivation is carried out, and the passivation filler is formed in the gap in the insulating coating layer, so that the gap in the insulating coating layer can be fully insulated, and the insulativity between the iron-silicon magnetic powder composite materials is better; moreover, the content of the non-magnetic insulating powder coated in the iron-silicon magnetic powder composite material obtained by the preparation method is relatively low, and the magnetic performance of the iron-silicon magnetic powder composite material is improved, so that the loss of an iron-silicon magnetic powder core prepared from the iron-silicon magnetic powder composite material is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of technical magnetic powder cores, and relates to a method for preparing an iron-silicon magnetic powder composite material, and in particular to an iron-silicon magnetic powder composite material and its preparation, an iron-silicon magnetic powder core and its preparation and application. Background Art

[0002] With the development of science and technology, various types of soft magnetic powder cores are widely used in new energy, electrical, communication and automotive industries, requiring various types of soft magnetic powder cores to develop in the direction of miniaturization, intelligence, high integration and low loss. At present, there are mainly various types of soft magnetic powder cores on the market, such as iron powder cores and metal magnetic powder cores. Among them, iron powder cores have higher saturation magnetic induction intensity, but lower resistivity. They are usually used in low frequency bands and have large eddy current losses at high frequencies. Although the loss of metal magnetic powder cores is greatly reduced compared to iron powder cores, the DC superposition characteristics and high-frequency losses still limit their large-scale application. At present, the main metal magnetic powder cores used are iron silicon magnetic powder cores. Although iron silicon magnetic powder cores have lower costs and high DC superposition performance, they have higher losses and serious heat generation, which is not conducive to energy saving and high efficiency of devices.

[0003] CN113035541A discloses a method for coating iron silicon powder with modified silica sol, which mainly comprises the following steps: uniformly mixing 80% silica sol by mass, 10% sodium silicate solution by mass and 10% water by mass to prepare a modified silica sol coating liquid, placing the iron silicon powder in the modified silica sol coating liquid for 1 to 3 minutes and then drying to prepare the iron silicon powder coated with the modified silica sol, and subsequently uniformly mixing and stirring the iron silicon powder coated with the modified silica sol, kaolin, FK glue, phenolic resin and zinc stearate to obtain a mixture, which is then pressed to obtain a magnetic powder core.

[0004] CN102294475A discloses a method for preparing an iron silicon material and a μ60 iron silicon magnetic powder core. The method for preparing the magnetic powder core includes the steps of particle size classification (mainly a particle size ratio of 200 mesh, 100 mesh, and 60 mesh magnetic powder), passivation, insulation coating, compression molding, and heat treatment to obtain the magnetic powder core.

[0005] CN113744988A discloses a coating method for magnetic powder core powder, modified magnetic powder core powder and its use. The coating method comprises the following steps: (1) uniformly mixing magnetic powder core powder, insulating agent and passivation liquid, drying to obtain a first coating material; (2) mixing a binder with the first coating material obtained in step (1), drying to obtain a second coating material with a moisture content of 0.6-0.7%; (3) granulating and drying the second coating material obtained in step (2), and then uniformly mixing it with a release agent to complete the coating of the magnetic powder core powder; steps (1) and (2) are performed in a fully enclosed environment.

[0006] The preparation methods of iron-silicon magnetic powder composite materials disclosed in the prior art all have certain defects, such as high loss and severe heat generation, which is not conducive to energy saving and high efficiency of devices. Therefore, it is very important to develop and design a new type of iron-silicon magnetic powder composite material and preparation method, iron-silicon magnetic powder core and preparation process. Summary of the invention

[0007] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an iron-silicon magnetic powder composite material and its preparation, an iron-silicon magnetic powder core and its preparation and application. The preparation method provided by the present invention first coats the iron-silicon magnetic powder with insulating powder to form an insulating coating layer, and then passivates it to form a passivation filler in the gaps in the insulating coating layer, so that the gaps in the insulating coating layer can be fully insulated, thereby making the insulation between the iron-silicon magnetic powder composite materials better; moreover, the content of coated non-magnetic insulating powder in the iron-silicon magnetic powder composite material obtained by the preparation method is low, which improves the magnetic properties of the iron-silicon magnetic powder composite material, thereby reducing the loss of the iron-silicon magnetic powder core prepared with the iron-silicon magnetic powder composite material.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing an iron-silicon magnetic powder composite material, the preparation method comprising:

[0010] The iron silicon magnetic powder is coated with insulating powder to obtain an intermediate, and the intermediate is passivated at least once to obtain an iron silicon magnetic powder composite material.

[0011] The preparation method provided by the present invention first coats the iron silicon magnetic powder with insulating powder to form an insulating coating layer, and then performs passivation to form a passivation filler in the gaps in the insulating coating layer, so that the gaps in the insulating coating layer can be fully insulated, thereby improving the insulation between the iron silicon magnetic powder composite materials; moreover, the content of the coated non-magnetic insulating powder in the iron silicon magnetic powder composite material obtained by the preparation method is low, the magnetic properties of the iron silicon magnetic powder composite material are improved, and thus the loss of the iron silicon magnetic powder core prepared with the iron silicon magnetic powder composite material is reduced.

[0012] Preferably, the ferrosilicon magnetic powder is pretreated before coating, and the pretreatment includes: heat treating the ferrosilicon magnetic powder in a vacuum environment, a reducing atmosphere, a nitrogen atmosphere or an inert atmosphere.

[0013] The preparation method of the present invention comprises pre-treating the iron silicon magnetic powder, wherein the pre-treatment can eliminate the stress in the iron silicon magnetic powder, improve the plastic deformation ability of the iron silicon magnetic powder, reduce the hardness of the iron silicon magnetic powder, thereby increasing the density of the iron silicon magnetic powder composite material, and further increasing the comprehensive magnetic properties of the iron silicon magnetic powder core prepared with the iron silicon magnetic powder composite material.

[0014] Preferably, the heat treatment comprises heating, keeping warm and cooling down in sequence, the heating rate is 1-15°C / min, and the terminal temperature is 650-800°C.

[0015] The heating rate described in the present invention is 1 to 15°C / min, for example, it can be 1°C / min, 3°C / min, 5°C / min, 7°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 14°C / min or 15°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] The terminal temperature of the heating in the present invention is 650-800°C, for example, it can be 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, the insulation time is 2 to 3 hours, for example, it can be 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the cooling rate is less than 30°C / h, and the terminal temperature is 10-40°C.

[0019] The cooling rate described in the present invention is not more than 30°C / h, for example, it can be 30°C / h, 29°C / h, 28°C / h, 27°C / h, 26°C / h, 25°C / h, 24°C / h, 23°C / h, 22°C / h, 21°C / h, 20°C / h, 18°C / h, 16°C / h, 14°C / h, 12°C / h or 10°C / h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] The terminal temperature of the cooling described in the present invention is 10-40°C, for example, it can be 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, 23°C, 25°C, 27°C, 30°C, 32°C, 35°C, 37°C or 40°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the reducing atmosphere comprises any one of hydrogen, methane or carbon monoxide or a combination of at least two thereof, typical but non-limiting combinations include a combination of hydrogen and methane, a combination of methane and carbon monoxide, or a combination of hydrogen, methane and carbon monoxide.

[0022] Preferably, the inert atmosphere comprises any one of argon, helium or neon or a combination of at least two of them, typical but non-limiting combinations being a combination of argon and helium, a combination of helium and neon, or a combination of argon, helium and neon.

[0023] Preferably, the iron silicon magnetic powder includes iron silicon magnetic powder prepared by a gas atomization method.

[0024] Preferably, the coating method includes mixing the insulating powder and the iron silicon magnetic powder by stirring.

[0025] Preferably, the stirring time is 10 to 40 min, for example, it can be 10 min, 12 min, 15 min, 17 min, 20 min, 22 min, 25 min, 27 min, 30 min, 32 min, 35 min, 37 min or 40 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the insulating powder comprises any one of SiO2 powder, Al2O3 powder, TiO2 powder, MgO powder or CaO powder, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of SiO2 powder and Al2O3 powder, a combination of Al2O3 powder and TiO2 powder, a combination of MgO powder and CaO powder, or a combination of SiO2 powder, Al2O3 powder and TiO2 powder, preferably SiO2 powder.

[0027] The Si in the SiO2 powder of the present invention is a semiconductor material and has a better insulation effect than other powders.

[0028] Preferably, the average particle size of the insulating powder is not greater than 100 nm, for example, it may be 100 nm, 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, 20 nm, 18 nm, 15 nm, 10 nm, 8 nm, 5 nm or 3 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably not greater than 20 nm.

[0029] In the present invention, the average particle size of the insulating powder is not greater than 100 nm, in order to ensure that the insulating particles can be well adsorbed on the surface of the iron silicon magnetic powder, increase the insulation effect of the iron silicon magnetic powder, and reduce the loss of the iron silicon magnetic powder core prepared from the iron silicon magnetic powder composite material.

[0030] Preferably, the insulating powder is prepared by a gas phase method.

[0031] Preferably, the average particle size of the iron silicon magnetic powder is 10 to 40 μm, for example, it can be 10 μm, 12 μm, 15 μm, 17 μm, 20 μm, 22 μm, 25 μm, 27 μm, 30 μm, 32 μm, 35 μm, 37 μm or 40 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the mass ratio of insulating powder to ferrosilicon magnetic powder in the mixture is (0.1-2):100, for example, it can be 0.1:100, 0.3:100, 0.5:100, 0.7:100, 0.9:100, 1:100, 1.2:100, 1.4:100, 1.6:100, 1.8:100 or 2:100, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the preparation method comprises a first passivation and a second passivation performed sequentially.

[0034] The invention adopts a secondary passivation process to improve the insulation between the iron-silicon magnetic powder composite materials, thereby improving the loss of the iron-silicon magnetic powder core prepared with the iron-silicon magnetic powder composite materials.

[0035] The insulation between magnetic powders further improves the loss characteristics of the magnetic core

[0036] The insulation between magnetic powders further improves the loss characteristics of the magnetic core

[0037] Preferably, the first passivation comprises first immersing the intermediate in a passivating agent solution.

[0038] Preferably, the passivator in the passivator solution comprises a water-soluble inorganic material, and the water-soluble inorganic material comprises phosphoric acid and / or aluminum dihydrogen phosphate.

[0039] In the present invention, phosphoric acid and / or aluminum dihydrogen phosphate are used as passivators, and phosphate passivation fillers are generated in the gaps within the insulating coating layer during the first passivation process.

[0040] The mass concentration of the passivating agent solution in the present invention is 80-99wt%, for example, it can be 80wt%, 82wt%, 84wt%, 86wt%, 88wt%, 90wt%, 92wt%, 94wt%, 96wt% or 98wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0041] Preferably, the solvent in the passivator solution includes any one of water, acetone or anhydrous ethanol or a combination of at least two of them. Typical but non-limiting combinations include a combination of water and acetone, a combination of acetone and anhydrous ethanol, or a combination of water, acetone and anhydrous ethanol.

[0042] Preferably, during the first passivation, the mass ratio of the passivator in the passivator solution to the iron silicon magnetic powder in the intermediate is (0.1-1):100, for example, it can be 0.1:100, 0.2:100, 0.3:100, 0.4:100, 0.5:100, 0.6:100, 0.7:100, 0.8:100, 0.9:100 or 1:100, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the first soaking time is 10 to 30 min, for example, it can be 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, during the first passivation, the intermediate is completely immersed in the passivating agent solution.

[0045] Preferably, drying is further included between the first passivation and the second passivation.

[0046] Preferably, the drying method includes any one of natural drying, heated drying and vacuum drying, or a combination of at least two of them. Typical but non-limiting combinations include a combination of natural drying and heated drying, a combination of heated drying and vacuum drying, or a combination of natural drying, heated drying and vacuum drying.

[0047] Preferably, the second passivation comprises secondly immersing the first passivated intermediate in liquid nitrogen.

[0048] In the present invention, the intermediate after the first passivation is secondly immersed in liquid nitrogen to form a nitride film, thereby achieving the second passivation.

[0049] Preferably, the second soaking time is not less than 20 min, for example, it can be 20 min, 22 min, 25 min, 27 min, 30 min, 32 min, 35 min, 37 min or 40 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] In a second aspect, the present invention provides an iron-silicon magnetic powder composite material, wherein the iron-silicon magnetic powder composite material is obtained by the preparation method described in the first aspect.

[0051] In a third aspect, the present invention provides an iron-silicon magnetic powder core, wherein the iron-silicon magnetic powder core is prepared from the iron-silicon magnetic powder composite material described in the second aspect.

[0052] In a fourth aspect, the present invention provides a process for preparing the iron-silicon magnetic powder core according to the third aspect, the preparation process comprising:

[0053] The iron-silicon magnetic powder composite material is pressed and formed, and then sintered in a protective atmosphere to obtain the iron-silicon magnetic powder core.

[0054] Preferably, the compression molding comprises: mixing the iron-silicon magnetic powder composite material with a release agent and then molding in a press.

[0055] Preferably, the release agent comprises zinc stearate.

[0056] Preferably, the mass ratio of the release agent to the iron-silicon magnetic powder composite material in the mixture is (0.2-0.6):100, for example, it can be 0.2:100, 0.25:100, 0.3:100, 0.35:100, 0.4:100, 0.45:100, 0.5:100, 0.55:100 or 0.6:100, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] Preferably, the molding pressure is 1500-2000 MPa, for example, it can be 1500 MPa, 1550 MPa, 1600 MPa, 1650 MPa, 1700 MPa, 1750 MPa, 1800 MPa, 1850 MPa, 1900 MPa, 1950 MPa or 2000 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] Preferably, the sintering includes a heating process, a heat preservation process and a cooling process performed sequentially.

[0059] Preferably, the rate of the heating process is 1-15°C / min, and the terminal temperature is 680-720°C.

[0060] The rate of the heating process described in the present invention is 1 to 15°C / min, for example, it can be 1°C / min, 3°C / min, 5°C / min, 7°C / min, 10°C / min, 12°C / min or 15°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] Preferably, the insulation process lasts for 1 to 2 hours, for example, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] Preferably, the cooling process includes cooling with the furnace to 10-35°C, for example, it can be 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C or 35°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] Preferably, the protective atmosphere comprises nitrogen and / or an inert gas, preferably nitrogen.

[0064] In a fifth aspect, the present invention provides an application of the iron-silicon magnetic powder core described in the third aspect, wherein the iron-silicon magnetic powder core is used in new energy, electrical, communication and automotive industries.

[0065] Compared with the prior art, the present invention has the following beneficial effects:

[0066] The preparation method provided by the present invention first coats the iron silicon magnetic powder with insulating powder to form an insulating coating layer, and then performs passivation to form a passivation filler in the gaps in the insulating coating layer, so that the gaps in the insulating coating layer can be fully insulated, thereby improving the insulation between the iron silicon magnetic powder composite materials; moreover, the content of the coated non-magnetic insulating powder in the iron silicon magnetic powder composite material obtained by the preparation method is low, the magnetic properties of the iron silicon magnetic powder composite material are improved, and thus the loss of the iron silicon magnetic powder core prepared with the iron silicon magnetic powder composite material is reduced. DETAILED DESCRIPTION

[0067] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0068] Example 1

[0069] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, the preparation method comprising:

[0070] (1) In a vacuum environment, the iron silicon magnetic powder is heated to 740° C. at a rate of 5° C. / min, then kept at this temperature for 2 hours, and then cooled to 25° C. at a rate of 30° C. / h to obtain pretreated iron silicon magnetic powder with an average particle size of 25 μm;

[0071] (2) mixing SiO2 powder having an average particle size of 20 nm with the pretreated iron silicon magnetic powder obtained in step (1) by stirring for 20 minutes to obtain an intermediate, wherein the mass ratio of SiO2 powder to the pretreated iron silicon magnetic powder in the mixture is 0.8:100;

[0072] (3) soaking the intermediate obtained in step (2) in a phosphoric acid acetone solution for 20 minutes, wherein the mass ratio of phosphoric acid in the phosphoric acid acetone solution to the iron silicon magnetic powder in the intermediate is 0.2:100, to obtain a first passivated intermediate;

[0073] (4) The first passivated intermediate obtained in step (3) is immersed in liquid nitrogen for 30 minutes for a second passivation to obtain a second iron-silicon magnetic powder composite material.

[0074] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, the preparation process comprising:

[0075] Zinc stearate and iron silicon magnetic powder composite materials with a mass ratio of 0.4:100 are mixed, and then formed in a press at a pressure of 1900 MPa, and then heated to 700°C at a rate of 5°C / min in a nitrogen atmosphere, and then kept warm for 1 hour, and then cooled to 25°C in the furnace to obtain the iron silicon magnetic powder core.

[0076] Example 2

[0077] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, the preparation method comprising:

[0078] (1) In a hydrogen atmosphere, the iron silicon magnetic powder is heated to 650° C. at a rate of 1° C. / min, then kept at this temperature for 3 hours, and then cooled to 10° C. at a rate of 10° C. / h, to obtain pretreated iron silicon magnetic powder having an average particle size of 10 μm;

[0079] (2) mixing SiO2 powder having an average particle size of 10 nm with the pretreated iron silicon magnetic powder obtained in step (1) by stirring for 40 minutes to obtain an intermediate, wherein the mass ratio of SiO2 powder to the pretreated iron silicon magnetic powder in the mixture is 0.1:100;

[0080] (3) soaking the intermediate obtained in step (2) in an anhydrous ethanol solution of aluminum dihydrogen phosphate for 10 minutes, wherein the mass ratio of aluminum dihydrogen phosphate in the anhydrous ethanol solution of aluminum dihydrogen phosphate to the iron silicon magnetic powder in the intermediate is 1:100, to obtain a first passivated intermediate;

[0081] (4) The first passivated intermediate obtained in step (3) is immersed in liquid nitrogen for 20 minutes for a second passivation to obtain a second iron-silicon magnetic powder composite material.

[0082] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, the preparation process comprising:

[0083] Zinc stearate and iron silicon magnetic powder composite materials with a mass ratio of 0.2:100 are mixed, and then formed in a press at a pressure of 2000 MPa, and then heated to 720°C at a rate of 15°C / min in a nitrogen atmosphere, and then kept warm for 1.5 hours, and then cooled to 35°C in the furnace to obtain the iron silicon magnetic powder core.

[0084] Example 3

[0085] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, the preparation method comprising:

[0086] (1) In a nitrogen atmosphere, the iron silicon magnetic powder is heated to 800° C. at a rate of 15° C. / min, then kept at this temperature for 2.5 hours, and then cooled to 40° C. at a rate of 20° C. / h to obtain pretreated iron silicon magnetic powder having an average particle size of 40 μm;

[0087] (2) mixing SiO2 powder having an average particle size of 100 nm with the pretreated iron silicon magnetic powder obtained in step (1) by stirring for 10 minutes to obtain an intermediate, wherein the mass ratio of the SiO2 powder to the pretreated iron silicon magnetic powder in the mixture is 2:100;

[0088] (3) soaking the intermediate obtained in step (2) in a phosphoric acid acetone solution for 30 minutes, wherein the mass ratio of phosphoric acid in the phosphoric acid acetone solution to the iron silicon magnetic powder in the intermediate is 0.1:100, to obtain a first passivated intermediate;

[0089] (4) The first passivated intermediate obtained in step (3) is immersed in liquid nitrogen for 40 minutes for a second passivation to obtain a second iron-silicon magnetic powder composite material.

[0090] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, the preparation process comprising:

[0091] Zinc stearate and iron silicon magnetic powder composite materials with a mass ratio of 0.6:100 are mixed, and then formed in a press at a pressure of 1500MPa, and then heated to 680°C at a rate of 1°C / min in an argon atmosphere, and then kept warm for 2h, and then cooled to 10°C in the furnace to obtain the iron silicon magnetic powder core.

[0092] Example 4

[0093] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the average particle size of the SiO2 powder in step (2) is 50 nm.

[0094] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0095] Example 5

[0096] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the average particle size of the SiO2 powder in step (2) is 100 nm.

[0097] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0098] Example 6

[0099] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the SiO2 powder in step (2) is replaced by Al2O3 powder of the same mass and particle size.

[0100] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0101] Example 7

[0102] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the MgO powder in step (2) is replaced by MgO powder of the same mass and particle size.

[0103] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0104] Example 8

[0105] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the TiO2 powder in step (2) is replaced by TiO2 powder of the same mass and particle size.

[0106] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0107] Example 9

[0108] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the CaO powder in step (2) is replaced by CaO powder of the same mass and particle size.

[0109] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0110] Example 10

[0111] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the average particle size of the SiO2 powder in step (2) is 200 nm.

[0112] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0113] Embodiment 11

[0114] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as Embodiment 1 except that step (1) is omitted, that is, in step (2), iron-silicon magnetic powder with an average particle size of 25 μm is directly mixed with SiO2 powder with an average particle size of 20 nm.

[0115] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0116] Example 12

[0117] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the mass ratio of SiO2 powder to pretreated iron-silicon magnetic powder in the mixture in step (2) is 0.05:100.

[0118] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0119] Example 13

[0120] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the mass ratio of SiO2 powder to pretreated iron-silicon magnetic powder in the mixture in step (2) is 3:100.

[0121] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0122] Embodiment 14

[0123] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the mass ratio of phosphoric acid in the phosphoric acid acetone solution to the iron-silicon magnetic powder in the intermediate in step (3) is 0.05:100.

[0124] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0125] Embodiment 15

[0126] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that the mass ratio of phosphoric acid in the phosphoric acid acetone solution to the iron-silicon magnetic powder in the intermediate is 2:100 in step (3).

[0127] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0128] Example 16

[0129] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that step (3) is omitted.

[0130] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0131] Embodiment 17

[0132] This embodiment provides a method for preparing an iron-silicon magnetic powder composite material, which is the same as that of Embodiment 1 except that step (4) is omitted.

[0133] This embodiment also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Embodiment 1.

[0134] Comparative Example 1

[0135] This comparative example provides a method for preparing an iron-silicon magnetic powder composite material, the preparation method comprising:

[0136] (1) In a hydrogen atmosphere, the iron silicon magnetic powder is heated to 650° C. at a rate of 1° C. / min, then kept at this temperature for 3 hours, and then cooled to 10° C. at a rate of 10° C. / h, to obtain pretreated iron silicon magnetic powder having an average particle size of 10 μm;

[0137] (2) soaking the pretreated iron silicon magnetic powder obtained in step (1) in an anhydrous ethanol solution of aluminum dihydrogen phosphate for 20 minutes, wherein the mass ratio of aluminum dihydrogen phosphate in the anhydrous ethanol solution of aluminum dihydrogen phosphate to the pretreated iron silicon magnetic powder is 1:100, to obtain a first passivated iron silicon magnetic powder;

[0138] (3) The first passivated iron silicon magnetic powder obtained in step (2) is immersed in liquid nitrogen for 20 minutes for a second passivation to obtain a second passivated iron silicon magnetic powder.

[0139] (4) mixing Al2O3 powder having an average particle size of 10 nm with the second passivated iron silicon magnetic powder obtained in step (2) by stirring for 40 minutes to obtain an intermediate, wherein the mass ratio of Al2O3 powder to the second passivated iron silicon magnetic powder in the mixture is 0.1:100, to obtain a second iron silicon magnetic powder composite material

[0140] This comparative example also provides a preparation process of an iron-silicon magnetic powder core, and the preparation process is the same as that of Example 1.

[0141] An annular iron-silicon magnetic powder core with an outer diameter of 12.7 mm, an inner diameter of 7.6 mm, and a height of 3 mm was prepared by the preparation method provided in the above embodiments and comparative examples, and the density ρ of the annular iron-silicon magnetic powder core was tested by the drainage method; subsequently, the annular iron-silicon magnetic powder core was wound, and the inductance L was tested by an LCR meter, and the effective magnetic permeability μ of the annular iron-silicon magnetic powder core was calculated as shown in Table 1, and the test frequency was 100 kHz. The AC loss of the annular iron-silicon magnetic powder core was tested by a Japanese Iwasaki SY-8218 soft magnetic BH analyzer as shown in Table 1, and the test conditions were: 50 kHz, 100 mT, and a temperature of 25°C.

[0142] Table 1

[0143]

[0144]

[0145] From Table 1, we can get:

[0146] (1) The iron-silicon magnetic powder composite material is prepared by the preparation method of the iron-silicon magnetic powder composite material provided in Examples 1 to 9, and the iron-silicon magnetic powder core prepared by the preparation process in Examples 1 to 9 has a higher density, a higher effective magnetic permeability and a lower AC loss;

[0147] (2) By comparing Example 1 with Example 10, it can be seen that the average particle size of the insulating powder in the present invention affects the performance of the prepared iron-silicon magnetic powder composite material, thereby affecting the performance of the iron-silicon magnetic powder core; the average particle size of the insulating powder in the present invention is not greater than 100nm, the purpose of which is to ensure that the insulating particles can be well adsorbed on the surface of the iron-silicon magnetic powder, increase the insulation effect of the iron-silicon magnetic powder, and reduce the loss of the iron-silicon magnetic powder core prepared by the iron-silicon magnetic powder composite material; when the average particle size of the insulating powder is greater than 100nm, it cannot be well adsorbed on the surface of the iron-silicon magnetic powder, thereby failing to effectively reduce the loss of the iron-silicon magnetic powder core;

[0148] (3) By comparing Example 1 with Example 11, it can be seen that the present invention further includes pre-treatment of the iron silicon magnetic powder before coating, and the pre-treatment can eliminate the stress in the iron silicon magnetic powder, improve the plastic deformation ability of the iron silicon magnetic powder, and reduce the hardness of the iron silicon magnetic powder, thereby increasing the density of the iron silicon magnetic powder composite material, and further improving the comprehensive magnetic properties of the iron silicon magnetic powder core prepared with the iron silicon magnetic powder composite material;

[0149] (4) By comparing Example 1 with Examples 12 and 13, it can be seen that the mass ratio of the insulating powder to the iron silicon magnetic powder in the mixture of the present invention will affect the performance of the obtained iron silicon magnetic powder composite material, thereby affecting the performance of the iron silicon magnetic powder core; when the mass ratio of the insulating powder to the iron silicon magnetic powder is low, the loss of the iron silicon magnetic powder core will increase, because the reduction of the insulating powder content will lead to uneven coating of the magnetic powder surface, and the eddy current loss will increase, thereby increasing the loss; when the mass ratio of the insulating powder to the iron silicon magnetic powder is high, the density of the iron silicon magnetic powder core will decrease, the effective magnetic permeability will decrease, and the loss will increase. This is because the non-magnetic insulating powder increases, so the magnetic permeability decreases, the density change decreases, and the insulating powder content increases. Increased hysteresis loss also increases, thereby increasing the loss;

[0150] (5) By comparing Example 1 with Examples 14 and 15, it can be seen that the mass ratio of the passivator in the passivator solution of the present invention to the iron silicon magnetic powder in the intermediate will affect the performance of the obtained iron silicon magnetic powder composite material, thereby affecting the performance of the iron silicon magnetic powder core; when the mass ratio of the passivator to the iron silicon magnetic powder is low, the density of the iron silicon magnetic powder core will be reduced and the loss will be increased. This is because too little passivator will reduce the passivation layer on the surface of the magnetic powder, making the insulation effect between the magnetic powders worse, the eddy current loss increased, and the loss increased; when the mass ratio of the passivator to the iron silicon magnetic powder is high, the density of the iron silicon magnetic powder core will be reduced, the effective magnetic permeability will be reduced, and the loss will be increased. This is because too much passivator will cause the passivation layer on the surface of the magnetic powder to be thicker, the non-magnetic material will also increase, the magnetic permeability will be reduced, and the loss will increase;

[0151] (6) By comparing Example 1 with Examples 16 and 17, it can be seen that the first passivation of the two passivations in the present invention will affect the performance of the obtained iron-silicon magnetic powder composite material, thereby affecting the performance of the iron-silicon magnetic powder core; when the first passivation is omitted, the density of the iron-silicon magnetic powder core will become lower and the loss will become higher. This is because the first step of passivation agent treatment is lacking. Only the second step of nitrogen passivation will cause the coating layer on the surface of the magnetic powder to be uneven, the insulation effect to be poor, the insulation effect between the magnetic powders to be poor, the eddy current loss to be increased, and the loss to be increased; when the second passivation is omitted, the density of the iron-silicon magnetic powder core will become lower and the loss to be higher. This is because the second step of passivation is lacking, resulting in the coating layer on the surface of the magnetic powder to be uneven, the insulation effect to be poor, the insulation effect between the magnetic powders to be poor, the eddy current loss to be increased, and the loss to be increased;

[0152] (7) By comparing Example 1 with Comparative Example 1, it can be seen that the preparation method provided by the present invention first coats the iron silicon magnetic powder with insulating powder to form an insulating coating layer, and then passivates it to form a passivation filler in the gaps in the insulating coating layer, so that the gaps in the insulating coating layer can be fully insulated, thereby making the insulation between the iron silicon magnetic powder composite materials better; moreover, the content of coated non-magnetic insulating powder in the iron silicon magnetic powder composite material obtained by the preparation method is relatively low, thereby improving the magnetic properties of the iron silicon magnetic powder composite material, thereby reducing the loss of the iron silicon magnetic powder core prepared with the iron silicon magnetic powder composite material.

[0153] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an iron-silicon magnetic powder composite material, It is characterized in that The preparation method comprises: The iron silicon magnetic powder is coated with insulating powder to obtain an intermediate, and the intermediate is passivated at least once to obtain an iron silicon magnetic powder composite material.

2. The preparation method according to claim 1, It is characterized in that The method further includes pre-treating the iron silicon magnetic powder before coating, wherein the pre-treatment includes: heat-treating the iron silicon magnetic powder in a vacuum environment, a reducing atmosphere, a nitrogen atmosphere or an inert atmosphere; Preferably, the heat treatment includes heating, keeping warm and cooling down in sequence; Preferably, the heating rate is 1-15°C / min, and the terminal temperature is 650-800°C; Preferably, the insulation time is 2 to 3 hours; Preferably, the cooling rate is no more than 30°C / h, and the terminal temperature is 10-40°C.

3. The preparation method according to claim 1 or 2, It is characterized in that The coating method includes mixing the insulating powder and the iron silicon magnetic powder by stirring; Preferably, the stirring time is 10 to 40 minutes; Preferably, the insulating powder comprises SiO 2 Powder, Al 2 O 3 Powder, TiO 2 Powder, MgO powder or CaO powder, any one or a combination of at least two thereof, preferably SiO 2 powder; Preferably, the average particle size of the insulating powder is not greater than 100 nm, preferably not greater than 20 nm; Preferably, the average particle size of the iron silicon magnetic powder is 10 to 40 μm; Preferably, the mass ratio of the insulating powder to the iron silicon magnetic powder in the mixture is (0.1-2):

100.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The preparation method comprises a first passivation and a second passivation performed sequentially; Preferably, the first passivation comprises first immersing the intermediate in a passivating agent solution; Preferably, the passivator in the passivator solution comprises a water-soluble inorganic material, and the water-soluble inorganic material comprises phosphoric acid and / or aluminum dihydrogen phosphate; Preferably, during the first passivation, the mass ratio of the passivator in the passivator solution to the iron silicon magnetic powder in the intermediate is (0.1-1):100; Preferably, the first soaking time is 10 to 30 minutes; Preferably, the second passivation comprises secondly immersing the first passivated intermediate in liquid nitrogen; Preferably, the second soaking time is not less than 20 minutes.

5. An iron-silicon magnetic powder composite material, It is characterized in that The iron-silicon magnetic powder composite material is obtained by the preparation method according to any one of claims 1 to 4.

6. An iron silicon magnetic powder core, It is characterized in that The iron-silicon magnetic powder core is prepared from the iron-silicon magnetic powder composite material according to claim 5.

7. A process for preparing the iron-silicon magnetic powder core according to claim 6, It is characterized in that The preparation process comprises: The iron-silicon magnetic powder composite material is pressed and formed, and then sintered in a protective atmosphere to obtain the iron-silicon magnetic powder core.

8. The preparation process according to claim 7, It is characterized in that The compression molding comprises: mixing the iron-silicon magnetic powder composite material with a release agent and molding it in a press; Preferably, the release agent comprises zinc stearate; Preferably, the mass ratio of the release agent to the iron-silicon magnetic powder composite material in the mixture is (0.2-0.6):100; Preferably, the molding pressure is 1500-2000 MPa.

9. The preparation process according to claim 7 or 8, It is characterized in that The sintering includes a heating process, a heat preservation process and a cooling process which are carried out in sequence; Preferably, the rate of the heating process is 1-15°C / min, and the terminal temperature is 680-720°C; Preferably, the insulation process lasts for 1 to 2 hours; Preferably, the cooling process includes cooling to 10-35°C with the furnace; Preferably, the protective atmosphere comprises nitrogen and / or an inert gas, preferably nitrogen.

10. An application of the iron-silicon magnetic powder core according to claim 6, It is characterized in that The iron silicon magnetic powder core is used in new energy, electrical, communication and automobile industries.