Preparation method of ceramic sealing ring

By using the combination of hyperbranched epoxy resin and ceramic powder, the complex shape and uniformity problems in the preparation of ceramic sealing rings are solved, and the high density and good mechanical properties of ceramic sealing rings are achieved. It is suitable for the preparation of ceramic sealing rings with complex structures. .

CN119059802AActive Publication Date: 2024-12-03HUNAN MEICHENG NEW MATERIALS TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411559922.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
2044-11-04

AI Technical Summary

Technical Problem

During the preparation of existing ceramic seal rings, dry press molding methods are difficult to prepare samples of complex shapes, and the internal uniformity of the ceramics is poor, which limits the mechanical properties of the material.

Method used

The second generation of hyperbranched polyester was obtained by reacting trimethylolpropane and 2,2-dihydroxymethylolpropane acid, combined with epoxypropane and tetrabutyl ammonium bromide, and after treatment with aqueous sodium hydroxide solution, superbranching was formed epoxy resin and form a high solid content slurry with initiator and ceramic powder ball mill. The green body is obtained by vacuum degassing and mold curing, and then sintered under an inert atmosphere to form a ceramic sealing ring with high density and good mechanical properties. .

Benefits of technology

The rapid curing of ceramic sealing rings and the structural uniformity improvement are achieved, the slurry settlement is avoided, the density and mechanical properties of green body and sealing rings are improved, and special-shaped sealing rings of complex shapes can be prepared.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

The invention relates to the field of ceramic materials, in particular to a preparation method of a ceramic sealing ring, which comprises the following steps: adding an initiator and ceramic powder into ethanol for ball milling, adding hyperbranched epoxy resin, uniformly mixing to obtain slurry with the solid content of more than or equal to 60%, carrying out vacuum degassing on the slurry, pouring into a mold, curing to obtain a green body, drying the green body, and discharging glue to obtain the ceramic sealing ring. The preparation method comprises the following steps: heating to 1450-1600 DEG C in an inert gas atmosphere, carrying out isostatic pressing sintering for 1-5 hours, cooling to 1200-1300 DEG C, carrying out heat preservation annealing for 1-5 hours, and finally naturally cooling to room temperature. The method can be used for preparing a special-shaped sealing ring with a complex structure, and the prepared green body and ceramic sealing ring have high density and good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramic materials, and in particular to a method for preparing a ceramic sealing ring. Background Art

[0002] The power battery is the "heart" of electric vehicles, and its service life and safety are considered to be the key to whether electric vehicles can be widely popularized. Among them, the sealing of the end cover of the power battery is the key to determining the safety performance of the power battery. Ceramics have excellent electrical insulation and mechanical strength. In recent years, leading battery companies have gradually replaced common plastic seals with ceramic seals.

[0003] Ceramic sealing rings can give full play to the high insulation, high strength, high temperature resistance, aging resistance, corrosion resistance and other characteristics of ceramic materials. After metallization welding, they have good air tightness and are extremely resistant to high temperatures. They can withstand rapid temperature changes, have high mechanical strength, and have small dimensional tolerances at the sealing points, greatly improving their service life and safety.

[0004] Each step in the preparation process of ceramic sealing rings will affect its properties, among which the molding process is an important link, because the density and uniformity of the green body will directly affect the sintering performance of the material. The currently commonly used dry pressing molding method has the advantages of simple process and high efficiency, but dry pressing molding is difficult to prepare samples of complex shapes, and due to the poor uniformity inside the ceramic green body, the mechanical properties are limited. Summary of the invention

[0005] Purpose of the invention: In view of the above technical problems, the present invention proposes a method for preparing a ceramic sealing ring.

[0006] The technical solutions adopted are as follows: A method for preparing a ceramic sealing ring is as follows: S1: The second generation of hyperbranched polyester is obtained by reacting trimethylolpropane and 2,2-dimethylolpropionic acid; S2: Mix the second generation hyperbranched polyester, epichlorohydrin and tetrabutylammonium bromide, heat to 40-60°C and react for 1-5h, add sodium hydroxide aqueous solution, heat to 90-100°C and continue to react for 1-5h, return to room temperature and wash the reaction solution with water until it is neutral, and remove small molecules by vacuum distillation to obtain a hyperbranched epoxy resin; S3: firstly adding an initiator and a ceramic powder into ethanol for ball milling, then adding a hyperbranched epoxy resin and mixing well to obtain a slurry with a solid content of ≥60%, and then pouring the slurry into a mold for solidification after vacuum degassing to obtain a green body; S4: After the green body is dried and debinded, the temperature is raised to 1450-1600°C in an inert gas atmosphere for isostatic sintering for 1-5 hours, then the temperature is lowered to 1200-1300°C for annealing for 1-5 hours, and finally naturally cooled to room temperature.

[0007] Furthermore, the molar ratio of trimethylolpropane to 2,2-dimethylolpropionic acid is 1:9.

[0008] Furthermore, the molar ratio of the second generation hyperbranched polyester to epichlorohydrin is 1:12-20.

[0009] Furthermore, the amount of tetrabutylammonium bromide used is 0.1-1% of the mass of the second-generation hyperbranched polyester.

[0010] Further, the initiator is aliphatic amine disulfide and aromatic amine disulfide; The mass ratio of the aliphatic amine disulfide to the aromatic amine disulfide is 1-10:1-10.

[0011] Furthermore, the structural formula of the fatty amine disulfide is as follows: ; Wherein, n≥6, and can be 6, 7, 8, 9, 10, 11 or 12, and n is preferably 8.

[0012] Furthermore, the structural formula of the aromatic amine disulfide is as follows: .

[0013] Furthermore, the aromatic amine disulfide is preferably 4,4'-dithiodiphenylamine.

[0014] Further, the ceramic powder includes aluminum oxide powder, yttrium oxide, copper oxide and lanthanum oxide; The mass ratio of the aluminum oxide powder, yttrium oxide, copper oxide and lanthanum oxide is 95-100:1-5:0.1-1:0.1-1.

[0015] Furthermore, the mass ratio of the initiator, the ceramic powder and the hyperbranched epoxy resin is 0.1-0.5:60-80:1-5.

[0016] Furthermore, the pressure during isostatic sintering is 100-200 MPa.

[0017] Beneficial effects of the present invention: The invention provides a preparation method of a ceramic sealing ring. The hyperbranched epoxy resin prepared in the invention has a more dispersed molecular structure and more active groups, can form a three-dimensional gel network with a high cross-linking density, thereby realizing quick solidification of slurry faster, and can effectively avoid slurry sedimentation caused by too long curing time, thereby improving the uniformity of the internal structure of the green body and improving its strength. An initiator composed of aliphatic amine disulfide and aromatic amine disulfide can undergo a curing reaction with the hyperbranched epoxy resin, and the introduction of flexible aliphatic long chains can prevent the formation of microcracks in the green body caused by too high cross-linking density. Aromatic amine disulfide can improve the structural stability of the green body and improve the strength of the green body. Since disulfide bonds are prone to bond breaking reactions, they can be quickly broken and decomposed during debinding, and can be fully discharged in a short time, creating conditions for subsequent sintering densification. The method of the invention can be used to prepare special-shaped sealing rings with complex structures. The prepared green body and ceramic sealing rings have high density and good mechanical properties. DETAILED DESCRIPTION

[0018] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0019] Embodiment 1: This embodiment provides a method for preparing a ceramic sealing ring: ; S1: Under nitrogen protection, add 2,2-dimethylolpropionic acid (3 mol, 402 g), trimethylolpropane (1 mol, 134 g), and p-toluenesulfonic acid (1.5 g) as a catalyst into a flask, stir and heat to 140°C for reaction for 3 h, separate the water generated by the reaction with a water separator during the reaction, then add 2,2-dimethylolpropionic acid (6 mol, 804 g) and p-toluenesulfonic acid (8 g), keep the temperature unchanged and continue to react for 3 h, also separate the water generated by the reaction with a water separator during the reaction, stop introducing nitrogen, connect a vacuum pump to reduce pressure and remove water until no water is distilled out, cool to room temperature, dissolve with an appropriate amount of acetone, recrystallize in toluene, filter, and dry the obtained product to obtain the second generation hyperbranched polyester; S2: Add the second generation hyperbranched polyester (0.1 mol, 116.7 g), epichlorohydrin (2 mol, 185 g) and tetrabutylammonium bromide (0.6 g) into a flask with a condenser and stir to mix. After heating to 60°C for 5 h, add 10 ml of 10 wt% sodium hydroxide aqueous solution and heat to 100°C for further reaction for 5 h. After returning to room temperature, wash the reaction solution repeatedly with deionized water until it is neutral. Finally, remove small molecules by vacuum distillation to obtain a hyperbranched epoxy resin. S3: Using 4,4'-dithiodiphenylamine and 8,8-dithiodioctylamine in a mass ratio of 1:5 as initiators, and aluminum oxide powder, yttrium oxide, copper oxide, and lanthanum oxide in a mass ratio of 98:2:0.5:0.5 as ceramic powders, the initiator, ceramic powder, and ethanol are added into a ball mill, and after ball milling for 5 hours on a planetary ball mill, the hyperbranched epoxy resin is added, and the mixture is quickly stirred and mixed to obtain a slurry with a solid content of 80%, wherein the mass ratio of the initiator, ceramic powder, and hyperbranched epoxy resin is 0.5:65:3, and the slurry is poured into a mold after vacuum degassing and cured at room temperature for 60 minutes to obtain a green body; S4: After drying the green body in an oven at 80°C for 24 hours, heat it to 800°C at a rate of 1°C / min and keep it for 2 hours to debind, then introduce argon protection, heat it to 1550°C at a rate of 10°C / min, isostatically press sinter it at 150MPa for 4 hours, then cool it to 1250°C at a rate of 5°C / min and keep it for annealing for 2 hours, and finally cool it naturally to room temperature.

[0020] Embodiment 2: This embodiment provides a method for preparing a ceramic sealing ring: Wherein, S1 and S2 are the same as those in Example 1; S3: Using 4,4'-diphenyldisulfide and 8,8-dioctyldisulfide as initiators in a mass ratio of 1:10, and aluminum oxide powder, yttrium oxide, copper oxide, and lanthanum oxide as ceramic powders in a mass ratio of 98:2:0.5:0.5, the initiator, ceramic powder, and ethanol are added into a ball mill, and after ball milling for 5 hours on a planetary ball mill, the hyperbranched epoxy resin is added, and the mixture is quickly stirred and mixed to obtain a slurry with a solid content of 80%, wherein the mass ratio of the initiator, ceramic powder, and hyperbranched epoxy resin is 0.5:65:3, and the slurry is poured into a mold after vacuum degassing and cured at room temperature for 60 minutes to obtain a green body; S4: After drying the green body in an oven at 80°C for 24 hours, heat it to 800°C at a rate of 1°C / min and keep it for 2 hours to debind, then introduce argon protection, heat it to 1550°C at a rate of 10°C / min, isostatically press sinter it at 150MPa for 4 hours, then cool it to 1250°C at a rate of 5°C / min and keep it for annealing for 2 hours, and finally cool it naturally to room temperature.

[0021] Embodiment 3: This embodiment provides a method for preparing a ceramic sealing ring: Wherein, S1 and S2 are the same as those in Example 1; S3: Using 4,4'-dithiodiphenylamine and 8,8-dithiodioctylamine in a mass ratio of 5:1 as initiators, and aluminum oxide powder, yttrium oxide, copper oxide, and lanthanum oxide in a mass ratio of 98:2:0.5:0.5 as ceramic powders, the initiator, ceramic powder, and ethanol are added into a ball mill, and after ball milling for 5 hours on a planetary ball mill, the hyperbranched epoxy resin is added, and the mixture is quickly stirred and mixed to obtain a slurry with a solid content of 80%, wherein the mass ratio of the initiator, ceramic powder, and hyperbranched epoxy resin is 0.5:65:3, and the slurry is poured into a mold after vacuum degassing and cured at room temperature for 60 minutes to obtain a green body; S4: After drying the green body in an oven at 80°C for 24 hours, heat it to 800°C at a rate of 1°C / min and keep it for 2 hours to debind, then introduce argon protection, heat it to 1550°C at a rate of 10°C / min, isostatically press sinter it at 150MPa for 4 hours, then cool it to 1250°C at a rate of 5°C / min and keep it for annealing for 2 hours, and finally cool it naturally to room temperature.

[0022] Embodiment 4: This embodiment provides a method for preparing a ceramic sealing ring: Wherein, S1 and S2 are the same as those in Example 1; S3: Using 4,4'-diphenylene disulfide and 8,8-dioctyl disulfide as initiators in a mass ratio of 10:1, and aluminum oxide powder, yttrium oxide, copper oxide, and lanthanum oxide as ceramic powders in a mass ratio of 98:2:0.5:0.5, the initiator, ceramic powder, and ethanol are added into a ball mill, and after ball milling for 5 hours on a planetary ball mill, the hyperbranched epoxy resin is added, and the mixture is quickly stirred and mixed to obtain a slurry with a solid content of 80%, wherein the mass ratio of the initiator, ceramic powder, and hyperbranched epoxy resin is 0.5:65:3, and the slurry is poured into a mold after vacuum degassing and cured at room temperature for 60 minutes to obtain a green body; S4: After drying the green body in an oven at 80°C for 24 hours, heat it to 800°C at a rate of 1°C / min and keep it for 2 hours to debind, then introduce argon protection, heat it to 1550°C at a rate of 10°C / min, isostatically press sinter it at 150MPa for 4 hours, then cool it to 1250°C at a rate of 5°C / min and keep it for annealing for 2 hours, and finally cool it naturally to room temperature.

[0023] Comparative Example 1: The method is substantially the same as Example 1, except that the hyperbranched epoxy resin is replaced by ethylene glycol diglycidyl ether of the same mass.

[0024] Comparative Example 2: The method is substantially the same as Example 1, except that the hyperbranched epoxy resin is replaced by hydantoin epoxy resin of the same mass.

[0025] Comparative Example 3: The method is substantially the same as Example 1, except that ethylenediamine of the same mass is used as the initiator instead of the combination of 4,4'-diphenyldisulfide and 8,8-dioctyldisulfide.

[0026] Comparative Example 4: The method is basically the same as Example 1, except that the mass of the initiator remains unchanged and only 4,4'-dithiodiphenylamine is added.

[0027] Comparative Example 5: The method is basically the same as Example 1, except that the mass of the initiator remains unchanged and only 8,8-dioctyl disulfide is added.

[0028] Performance Test: According to the methods of Examples 1-4 and Comparative Examples 1-5 of the present invention, samples were prepared for performance testing; The bulk density (g / cm) was determined using the Archimedean displacement method. 3 The three-point bending strength (MPa) was tested by an electronic universal testing machine with a test interval of 30 mm and a rate of 0.5 mm / min. The fracture toughness (MPa·m 1 / 2 ); The test results are shown in Table 1 below: Table 1: ; As can be seen from Table 1 above, the green body and ceramic sealing ring prepared by the method of the present invention both have a high density and good mechanical properties; From the data comparison of Example 1 and Comparative Examples 1-2, it can be seen that the green body and ceramic sealing ring prepared by the hyperbranched epoxy resin in the present invention have higher density and better mechanical properties than those prepared by ethylene glycol diglycidyl ether and hydantoin epoxy resin; From the comparison of the data of Example 1 and Comparative Examples 3-5, it can be seen that the green body and the ceramic sealing ring prepared by using the combination of 4,4'-dithiodiphenylamine and 8,8-dithiodioctylamine as the initiator in the present invention have higher density and better mechanical properties.

[0029] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a ceramic sealing ring, characterized in that: The details are as follows: S1: The second generation of hyperbranched polyester is obtained by reacting trimethylolpropane and 2,2-dimethylolpropionic acid; S2: Mix the second generation hyperbranched polyester, epichlorohydrin and tetrabutylammonium bromide, heat to 40-60°C and react for 1-5h, add sodium hydroxide aqueous solution, heat to 90-100°C and continue to react for 1-5h, return to room temperature, wash the reaction solution with water until it is neutral, and remove small molecules by reduced pressure distillation to obtain a hyperbranched epoxy resin; S3: firstly adding an initiator and a ceramic powder into ethanol for ball milling, then adding a hyperbranched epoxy resin and mixing well to obtain a slurry with a solid content of ≥60%, and then pouring the slurry into a mold for solidification after vacuum degassing to obtain a green body; S4: After the green body is dried and debinded, the temperature is raised to 1450-1600°C in an inert gas atmosphere for isostatic sintering for 1-5 hours, then the temperature is lowered to 1200-1300°C for annealing for 1-5 hours, and finally naturally cooled to room temperature.

2. The method for preparing a ceramic sealing ring according to claim 1, characterized in that: The molar ratio of the trimethylolpropane to the 2,2-dimethylolpropionic acid is 1:

9.

3. The method for preparing a ceramic sealing ring according to claim 1, characterized in that: The molar ratio of the second generation hyperbranched polyester to epichlorohydrin is 1:12-20.

4. The method for preparing a ceramic sealing ring according to claim 1, characterized in that: The amount of tetrabutylammonium bromide used is 0.1-1% of the mass of the second-generation hyperbranched polyester.

5. The method for preparing a ceramic sealing ring according to claim 1, characterized in that: The initiator is aliphatic amine disulfide and aromatic amine disulfide; The mass ratio of the aliphatic amine disulfide to the aromatic amine disulfide is 1-10:1-10.

6. The method for preparing a ceramic sealing ring according to claim 5, characterized in that: The structural formula of the fatty amine disulfide is as follows: ; Among them, n≥6.

7. The method for preparing a ceramic sealing ring according to claim 5, characterized in that: The structural formula of the aromatic amine disulfide is shown below: 。 8. The method for preparing a ceramic sealing ring according to claim 1, characterized in that: The ceramic powder includes aluminum oxide powder, yttrium oxide, copper oxide and lanthanum oxide; The mass ratio of the aluminum oxide powder, yttrium oxide, copper oxide and lanthanum oxide is 95-100:1-5:0.1-1:0.1-1.

9. The method for preparing a ceramic sealing ring according to claim 1, characterized in that: The mass ratio of the initiator, the ceramic powder and the hyperbranched epoxy resin is 0.1-0.5:60-80:1-5.

10. The method for preparing a ceramic sealing ring according to claim 1, characterized in that: The pressure during isostatic sintering is 100-200MPa.

Citation Information

Patent Citations

  • Method for preparing aluminum oxide base ceramic core

    CN101077836A

  • Method for preparing Ba1-xSrxTiO3-MgO ferroelectric ceramic blank

    CN101870581A

  • Gel cast molding method for preparing shaped ceramic body

    CN105461310A

  • Preparation method of high-wear-resistance water seal ceramic wafer

    CN116874306A

  • Ceramic chopper and surface roughening treatment method thereof

    CN118545987A

Cited By

  • High-strength ceramsite proppant and preparation method thereof

    CN120943666A