A ceramic fiber composite brake pad
By using ceramic fiber composite materials and heat dissipation structures in brake pads, the problem of thermal decay of friction materials at high temperatures in brake pads has been solved, achieving high wear resistance and stable friction performance, extending service life and reducing costs.
Patent Information
- Application Number
- CN201910989635.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2039-10-17
AI Technical Summary
Existing brake pads are prone to thermal degradation of friction materials at high temperatures, resulting in unstable braking performance and insufficient wear resistance, which affects the safety and service life of the braking system.
The ceramic fiber composite brake pads incorporate PROMAXON®-D calcium silicate particles, ceramic fibers, diabase fibers, and other components into the friction layer. Drainage channels are also incorporated into the friction layer. Combined with a heat dissipation bonding layer made of basalt fibers, nano-silica modified phenolic resin, and other materials, a highly efficient heat dissipation structure is formed, ensuring that the material maintains good friction performance and wear resistance at high temperatures.
This technology achieves stable friction performance and good wear resistance in brake pads at high temperatures, extends service life, and reduces costs, thus meeting the requirements of high wear resistance, high speed, and safety in braking systems.
Smart Images

Figure CN110762145B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of automobile parts, in particular to a ceramic fiber composite brake pad. Background Art
[0002] In the braking system of a car, brake pads are the most critical safety parts. The brake pads play a decisive role in all braking effects. The working principle of the brake is mainly based on friction. The friction between the brake pads and the brake drum and the tires and the ground is used to convert the kinetic energy of the vehicle into heat energy after friction to stop the vehicle. A good and efficient braking system must be able to provide stable, sufficient and controllable braking force, and have good hydraulic transmission and heat dissipation capabilities to ensure that the force applied by the driver from the brake pedal can be fully and effectively transmitted to the master cylinder and each sub-cylinder, and to avoid hydraulic failure and brake decay caused by high heat. Summary of the invention
[0003] The object of the present invention is to provide a ceramic fiber composite brake pad to solve the problems raised in the above background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a ceramic fiber composite brake pad, comprising a friction layer and a heat dissipation adhesive layer, wherein the heat dissipation adhesive layer is located between the friction layer and the steel back, and the heat dissipation adhesive layer is made of the following components in proportion by weight: 14-15 parts of basalt fiber, 15-17 parts of phenolic resin modified with nano-silicon dioxide with epoxy groups, 1.5-2 parts of melamine, 3-4 parts of nano-alumina, 10-13 parts of copper fiber, 7-10 parts of steel fiber, 5-7 parts of polyimide, 4-5 parts of expanded vermiculite, 0.3-0.6 parts of sodium dodecyl sulfate, 0.3 parts of nano-zinc oxide, and 3-5 parts of nitrile rubber;
[0005] The friction layer is made of the following components in proportion by weight: 4 to 8 parts of PROMAXON ® -D calcium silicate particles, 9 to 11 parts of ceramic fibers, 10 to 15 parts of diabase fibers, 5 to 8 parts of iron yellow, 1 to 1.5 parts of tin bronze powder, 7 to 12 parts of carbon fibers, 5 to 8 parts of polyimide, 9 to 11 parts of needle-shaped wollastonite powder, 1 to 3 parts of zinc sulfide, 2 to 5 parts of tungsten disulfide, 2 to 5 parts of polytetrafluoroethylene, 15 to 17 parts of phenolic resin modified with nano-silicon dioxide with epoxy groups, 3 to 5 parts of nitrile rubber, and 1 to 1.5 parts of melamine.
[0006] Preferably, a drainage ditch is provided in the middle of the friction layer, and the bottom of the drainage ditch is flush with the heat dissipation adhesive layer.
[0007] PROMAXON ® -D basalt fiber particles (CAS registration number PROMAXON ® -D: 1344-95-2) are a high-porosity calcium silicate product. PROMAXON ® -D is produced by Promat International in Belgium, Europe, and LAPINUS Fibers Ltd. in the Netherlands is its sole agent in the global friction material market.
[0008] Diabase fiber does not contain asbestos inorganic substances, has good high temperature stability, extremely low non-fiber content, can reduce noise, and has good adaptability, good softness, excellent dispersibility, good bonding with resin, and little irritation to the skin.
[0009] Tungsten disulfide can be used as a lubricant, with better performance than molybdenum disulfide, lower friction coefficient and greater compressive strength. It is used alone in equipment operating at high temperature, high pressure, high speed, high load, and in chemically active media. It can be used as a filling material with polytetrafluoroethylene and nylon to make self-lubricating parts.
[0010] Needle-shaped wollastonite powder Needle-shaped wollastonite powder has the characteristics of high purity, good crystallization, strong fluidity, low linear expansion coefficient and corrosion resistance.
[0011] Tin bronze is a bronze with tin as the main alloying element. This alloy has high mechanical properties, anti-friction properties and corrosion resistance, is easy to cut, has good brazing and welding properties, a small shrinkage coefficient and is non-magnetic. Adding zinc can improve casting properties.
[0012] Polyimide has excellent mechanical properties, a decomposition temperature between 500-600°C, and can quickly diffuse the accumulated heat of the material, effectively preventing the friction material from entering the thermal decay stage.
[0013] Polytetrafluoroethylene has good lubrication properties. When combined with carbon fiber and aramid fiber, it can form a good friction-lubrication-friction relationship, which can improve friction performance and reduce the wear rate of the material.
[0014] The invention has the characteristics of good wear resistance, stable friction coefficient, long service life, low cost, etc. The heat dissipation area ensures that the advantages of each material are fully utilized in the friction material by reasonably matching multiple components. It has good temperature resistance, good thermal stability and low thermal conductivity, and meets the technical requirements of high wear resistance, high speed and safety of brake pads. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of the structure of the present invention;
[0016] Figure 2 This is a brake pad decay test curve diagram of Example 3 of the present invention;
[0017] Figure 3 It is a brake pad decay test curve diagram of comparative example 1 of the present invention. DETAILED DESCRIPTION
[0018] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Example 1
[0020] like Figure 1 As shown, the ceramic fiber composite brake pad includes a friction layer 1 and a heat dissipation adhesive layer 2. The heat dissipation adhesive layer 2 is located between the friction layer 1 and the steel back 3. A drainage ditch is provided in the middle of the friction layer 1. The bottom of the drainage ditch is flush with the heat dissipation adhesive layer, which is conducive to better heat dissipation of the heat dissipation adhesive layer. The heat dissipation adhesive layer is made of the following components in parts by weight: 14 parts of basalt fiber, 15 parts of nano-silicon dioxide modified phenolic resin with epoxy groups, 2 parts of melamine, 4 parts of nano-alumina, 10 parts of copper fiber, 7 parts of steel fiber, 5 parts of polyimide, 4 parts of expanded vermiculite, 0.6 parts of sodium dodecyl sulfate, 0.3 parts of nano-zinc oxide, and 3 parts of nitrile rubber;
[0021] The friction layer is made of the following components in weight: 4 parts of PROMAXON ® ~D calcium silicate particles, 9 parts of ceramic fiber, 15 parts of diabase fiber, 5 parts of iron yellow, 1 part of tin bronze powder, 9 parts of ceramic fiber, 7 parts of carbon fiber, 8 parts of polyimide, 11 parts of needle-shaped wollastonite powder, 1 part of zinc sulfide, 2 parts of tungsten disulfide, 5 parts of polytetrafluoroethylene, 17 parts of nano-silicon dioxide modified phenolic resin with epoxy group, 3 parts of nitrile rubber, and 1 part of melamine. The heat dissipation adhesive layer and the friction layer are mixed and poured into a high-speed disperser respectively, stirred into two uniformly dispersed powder compositions, and then each material composition is taken out and placed in two forming molds for pressing and forming, and then placed in the main mold, overlapped together, and compounded with the steel back, and then placed in a flat vulcanizer at a high temperature of 500°C and a pressure of 35MPa for 60 minutes. Finally, the brake pad is taken out and the burrs are removed to form a finished product (the same below).
[0022] Example 2
[0023] The ceramic fiber composite brake pad includes a friction layer 1 and a heat dissipation adhesive layer 2. The heat dissipation adhesive layer 2 is located between the friction layer 1 and the steel back 3. A drainage ditch is provided in the middle of the friction layer 1. The bottom of the drainage ditch is flush with the heat dissipation adhesive layer, which is conducive to better heat dissipation of the heat dissipation adhesive layer. The heat dissipation adhesive layer is made of the following components in parts by weight: 14 parts of basalt fiber, 16 parts of nano-silicon dioxide modified phenolic resin with epoxy groups, 1.5 parts of melamine, 3 parts of nano-alumina, 12 parts of copper fiber, 8 parts of steel fiber, 6 parts of polyimide, 4 parts of expanded vermiculite, 0.5 parts of sodium dodecyl sulfate, 0.3 parts of nano-zinc oxide, and 4 parts of nitrile rubber;
[0024] The friction layer is made of the following components in proportion by weight: 6 parts of PROMAXON ® ~D calcium silicate particles, 10 parts of ceramic fiber, 13 parts of diabase fiber, 6 parts of iron yellow, 1.5 parts of tin bronze powder, 10 parts of ceramic fiber, 8 parts of carbon fiber, 7 parts of polyimide, 10 parts of needle-shaped wollastonite powder, 2 parts of zinc sulfide, 3 parts of tungsten disulfide, 4 parts of polytetrafluoroethylene, 16 parts of phenolic resin modified with nano-silicon dioxide with epoxy groups, 4 parts of nitrile rubber, and 1 part of melamine.
[0025] Example 3
[0026] The ceramic fiber composite brake pad includes a friction layer 1 and a heat dissipation adhesive layer 2. The heat dissipation adhesive layer 2 is located between the friction layer 1 and the steel back 3. A drainage ditch is provided in the middle of the friction layer 1. The bottom of the drainage ditch is flush with the heat dissipation adhesive layer, which is conducive to better heat dissipation of the heat dissipation adhesive layer. The heat dissipation adhesive layer is made of the following components in parts by weight: 15 parts of basalt fiber, 17 parts of nano-silicon dioxide modified phenolic resin with epoxy groups, 2 parts of melamine, 4 parts of nano-alumina, 13 parts of copper fiber, 10 parts of steel fiber, 7 parts of polyimide, 5 parts of expanded vermiculite, 0.3 parts of sodium dodecyl sulfate, and 5 parts of nitrile rubber;
[0027] The friction layer is made of the following components in proportion by weight: 8 parts of PROMAXON ® ~D calcium silicate particles, 11 parts of ceramic fiber, 10 parts of diabase fiber, 8 parts of iron yellow, 1.5 parts of tin bronze powder, 11 parts of ceramic fiber, 12 parts of carbon fiber, 8 parts of polyimide, 11 parts of needle-shaped wollastonite powder, 3 parts of zinc sulfide, 5 parts of tungsten disulfide, 5 parts of polytetrafluoroethylene, 17 parts of phenolic resin modified with nano-silicon dioxide with epoxy groups, 5 parts of nitrile rubber, and 1.5 parts of melamine.
[0028] Comparative Example 1: 10 parts of aramid fiber, 8 parts of PROMAXON ® ~D calcium silicate particles, 11 parts of ceramic fiber, 7 parts of potassium hexatitanate whiskers, 4 parts of nano-alumina, 8 parts of molybdenum disulfide, 18 parts of atomized copper powder, 12 parts of carbonyl iron powder, 5 parts of barite, 6 parts of calcium oxide, 7 parts of magnesium oxide, 7 parts of talc, 5 parts of flake graphite, 10 parts of artificial graphite, 8 parts of triolein, 8 parts of dioctyl terephthalate, and 17 parts of nano-silica modified phenolic resin with epoxy groups. Production process: First, atomized copper powder, carbonyl iron powder, barite, calcium oxide, magnesium oxide, talcum powder, and calcium oxide are put into a ball mill and ground at 350r / min, with a ball milling ratio of 1:1 for 1h, then put into a mold and roughly pressed at 7MPa, and then dried in a drying furnace at 200℃. The composite powder block is taken out and poured into a high-speed disperser, stirred into a uniformly dispersed powder composition and mixed with PROMAXON ® ~D calcium silicate particles, ceramic fiber, triolein, dioctyl terephthalate, and nano-silica modified phenolic resin with epoxy groups. After being put into the mold and compounded with the blank, it is placed in a flat vulcanizer at a high temperature of 450℃ and a pressure of 40MPa for 60 minutes. The burrs are removed to become the finished product.
[0029] The specific embodiments 1, 2, 3 and the brake pad were compared and tested, and the results are as follows:
[0030]
[0031] Verification results show that this product has more excellent friction performance and good wear resistance, and has resistance to high temperature wear rate and thermal decay. During the heating process from 200°C to 350°C, the brake pad of Example 1 produced a large thermal decay, from 0.45 at 200°C to 0.29 at 300°C, a decrease of 35.5%. In terms of wear, before 200°C, the brake pads of Example 1 and the present invention are not much different, that is, the low-temperature wear of the two materials is similar; after 200°C, the present invention has excellent high-temperature bonding effect, which exponentially improves the wear resistance of the material. At 350°C, the wear rate of Example 1 is only 0.16, which is much lower than 0.25 of the comparative brake pad.
[0032] The following fading test was conducted on Example 3 and Comparative Example 1, with speeds of 50, 100, and 130 km / h, and brake line pressures of 2, 4, 6, 8, and 10 MPa, to examine the stability of the friction coefficient of the brake pad at different speeds and pressures.
[0033] like Figure 2-3As shown, the brake pad of Example 3 has a first decay of 6% and a second decay of 13%; the brake pad of Comparative Example 1 has a first decay of 29% and a second decay of 28%; it is obvious that the decay rate of the ceramic-based brake pad is much lower than that of the brake pad of Comparative Example 1, and its thermal stability is good. In the decay test, the first three braking times are the benchmark test, the first decay is 10 consecutive braking times at a speed of 100 km / h, and the recovery test is 12 braking times at a speed of 50 km / h and air cooling conditions. The second decay is the same as the first decay except that the continuous braking is 15 times at a speed of 100 km / h.
[0034] The friction coefficient of the brake pad shows insensitivity to the number of braking times, and the entire curve has no obvious "ups and downs". The friction coefficient fluctuates within 0.08, and the material has good heat resistance.
[0035] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0036] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A ceramic fiber composite brake pad, comprising a friction layer and a heat dissipation adhesive layer, wherein the heat dissipation adhesive layer is located between the friction layer and the steel back, characterized in that The heat dissipation adhesive layer is made of the following components in parts by weight: 14-15 parts of basalt fiber, 15-17 parts of nano-silicon dioxide modified phenolic resin with epoxy groups, 1.5-2 parts of melamine, 3-4 parts of nano-alumina, 10-13 parts of copper fiber, 7-10 parts of steel fiber, 5-7 parts of polyimide, 4-5 parts of expanded vermiculite, 0.3-0.6 parts of sodium dodecyl sulfate, 0.3 parts of nano-zinc oxide, and 3-5 parts of nitrile rubber; The friction layer is made of the following components in proportion by weight: 4-8 parts of PROMAXON ® ~D calcium silicate particles, 9-11 parts of ceramic fibers, 10-15 parts of diabase fibers, 5-8 parts of iron yellow, 1-1.5 parts of tin bronze powder, 7-12 parts of carbon fibers, 5-8 parts of polyimide, 9-11 parts of needle-shaped wollastonite powder, 1-3 parts of zinc sulfide, 2-5 parts of tungsten disulfide, 2-5 parts of polytetrafluoroethylene, 15-17 parts of phenolic resin modified with nano-silicon dioxide with epoxy groups, 3-5 parts of nitrile rubber, and 1-1.5 parts of melamine; a drainage ditch is provided in the middle of the friction layer, and the bottom of the drainage ditch is flush with the heat dissipation adhesive layer.
2. A ceramic fiber composite brake pad according to claim 1, characterized in that The heat dissipation adhesive layer is made of the following components in parts by weight: 15 parts of basalt fiber, 17 parts of nano-silicon dioxide modified phenolic resin with epoxy groups, 2 parts of melamine, 4 parts of nano-alumina, 13 parts of copper fiber, 10 parts of steel fiber, 7 parts of polyimide, 5 parts of expanded vermiculite, 0.3 parts of sodium lauryl sulfate, and 5 parts of nitrile rubber; The friction layer is made of the following components in proportion by weight: 8 parts of PROMAXON ® ~D calcium silicate particles, 11 parts of ceramic fiber, 10 parts of diabase fiber, 8 parts of iron yellow, 1.5 parts of tin bronze powder, 11 parts of ceramic fiber, 12 parts of carbon fiber, 8 parts of polyimide, 11 parts of needle-shaped wollastonite powder, 3 parts of zinc sulfide, 5 parts of tungsten disulfide, 5 parts of polytetrafluoroethylene, 17 parts of phenolic resin modified with nano-silicon dioxide with epoxy groups, 5 parts of nitrile rubber, and 1.5 parts of melamine.