Carbonaceous material dispersion and method for producing the same
By controlling the concentrations of amines and water in a high-purity non-aqueous solvent, a low-viscosity carbonaceous material dispersion was prepared, solving the problems of uneven dispersion and unstable viscosity of carbonaceous materials in lithium-ion secondary batteries, and improving the electrical properties and coating stability of the electrode.
Patent Information
- Application Number
- CN202110742418.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-03
- Filing Date
- 2021-07-01
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-07-01
AI Technical Summary
Existing carbonaceous material dispersions in lithium-ion secondary batteries suffer from problems such as unstable viscosity, uneven dispersion of carbonaceous materials, and difficulty in coating, and also contain impurities that lead to poor electrode performance.
By controlling the amine composition and water concentration in a high-purity non-aqueous solvent, a low-viscosity carbonaceous material dispersion is prepared. Specified amine compounds and dispersants are added to ensure the carbonaceous material concentration is between 15% and 30% by mass, and a multi-peak particle size distribution is formed through a specific dispersion process.
This method achieves high-concentration and uniform dispersion of carbonaceous materials in lithium-ion secondary batteries, reduces viscosity fluctuations, and improves the electrical properties and coating stability of the electrodes.
Smart Images

Figure CN113880075B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a carbonaceous material dispersion and a method for producing the same. Specifically, the present invention relates to a carbonaceous material dispersion suitable for use as a conductive aid in forming an electrode layer in the field of batteries, particularly in the manufacture of lithium ion secondary batteries, and a method for producing the same. Background Art
[0002] In recent years, lithium-ion secondary batteries with high capacity and high power have been widely used in many fields, such as electronic devices such as portable personal computers, smart phones, and mobile phones, or automobile fields such as electric vehicles and hybrid vehicles. In the further development of these fields, the high performance of lithium-ion secondary batteries and the efficiency of production processes are sought.
[0003] Electrodes used in lithium-ion secondary batteries are generally produced by applying an electrode slurry to a current collector, drying it, and then compressing it under pressure. The electrode slurry is prepared by mixing an electrode active material, a conductive additive, a binder, and the like in a solvent.
[0004] In order to prepare such electrode slurry efficiently, a scheme of using a carbonaceous material dispersion in which a carbonaceous material as a conductive aid is pre-dispersed in a solvent has been proposed (e.g., Patent Documents 1 to 3). When the carbonaceous material dispersion is used to prepare the electrode slurry, the mixing of the carbonaceous material dispersion and the electrode active material becomes easy, and an electrode with good conductivity in which the carbonaceous material is uniformly dispersed can be obtained.
[0005] For example, in the positive electrode for lithium ion secondary batteries, the material used as the positive electrode active material is a lithium transition metal composite oxide such as lithium cobalt oxide and lithium manganate, which itself lacks electronic conductivity, that is, electrical conductivity. Therefore, in order to give electrical conductivity to the lithium transition metal composite oxide, a carbonaceous material such as carbon black, graphite, carbon nanotubes, and carbon nanofibers is added to the electrode as a conductive additive.
[0006] As the properties required for the carbonaceous material dispersion, for example, Patent Document 4 describes that the dispersion state of the carbonaceous material such as carbon black in the carbonaceous material dispersion mixed in the positive electrode paste affects the battery performance.
[0007] When the carbonaceous material dispersion is paste-formed and mixed in the positive electrode active material, it is preferably low in viscosity for easy mixing. In addition, in order to prevent contamination of other metal particles in the battery material, the carbonaceous material dispersion is also preferably low in viscosity when performing pre-treatment such as filter removal of impurities. On the other hand, in order to manufacture the electrode, the solvent must be dried in the end, so the amount of solvent is preferably small.
[0008] In order to prepare the paste for the positive electrode, the positive electrode active material and the conductive auxiliary agent are evenly mixed and dispersed so that the conductive auxiliary agent maintains conductivity. Further, the binder components such as polyvinylidene fluoride resin (PVdF) in the bonding application of metal foil are dissolved. It should be noted that as a solvent, a non-aqueous solvent represented by N-methyl-2-pyrrolidone (NMP) is used.
[0009] Conventionally, an amine compound as a volatile pH adjuster has been added to the carbonaceous material dispersion in order to achieve the above-mentioned low viscosity. However, even when such an amine compound is added, the properties of the carbonaceous material dispersion are not stable and the viscosity does not become constant.
[0010] Therefore, in Patent Document 5, polyvinylidene fluoride is dissolved in a solvent of a nitrogen-containing heterocyclic amide compound such as 2-pyrrolidone or N-methyl-2-pyrrolidone, and the resin solution is applied to the surface of a substrate such as a metal plate or a resin molded body to form a coating that imparts water resistance and weather resistance to the substrate. The resin solution is colored by trace impurities contained in the solvent of the nitrogen-containing heterocyclic amide compound, and the coating formed using the resin solution is colored. For example, when a resin container having the coating is used as a transport container for precision components of LEDs and ICs, the presence of impurities contained in the coating causes malfunctions of electronic devices and automobile parts assembled with these precision components. The following solutions are proposed for solving the problem: (i) a nitrogen-containing heterocyclic amide compound is preliminarily brought into contact with a solid acidic substance; or (ii) a nitrogen-containing heterocyclic amide compound is preliminarily brought into contact with an acidic substance and then recovered by distillation. Furthermore, it is reported that even if the nitrogen-containing heterocyclic amide compound is simply treated with distillation, these impurities that cause coloration cannot be removed, but by using the compound treated by the above method, the problem of coloration can be eliminated.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Publication No. 2015-30777
[0014] Patent Document 2: Japanese Patent Application Publication No. 2016-46188
[0015] Patent Document 3: Japanese Patent Application Publication No. 2018-45820
[0016] Patent Document 4: International Publication No. WO2014 / 042266
[0017] Patent Document 5: Japanese Patent Application Laid-Open No. 10-310795 Summary of the invention
[0018] Problem that the invention aims to solve
[0019] As described above, conventional carbonaceous material dispersions are required to have stable performance, high-concentration and uniform dispersion of the carbonaceous material, and easy coating, but do not have characteristics that are sufficiently satisfactory for practical use.
[0020] Therefore, the subject of the present invention is to provide an improved carbonaceous material dispersion. The subject of the present invention is also to provide: a carbonaceous material dispersion suitable as a conductive aid dispersion for lithium ion secondary batteries and a method for producing the same. A further subject of the present invention is to provide: a carbonaceous material dispersion in which the carbonaceous material is highly concentrated and uniformly dispersed and can be easily coated and a method for producing the same. A further subject of the present invention is to provide: a carbonaceous material dispersion that can stably exhibit very excellent electrical properties when used as a conductive aid for lithium ion secondary batteries and a method for producing the same.
[0021] Solutions for solving problems
[0022] The present inventors have repeatedly conducted in-depth research on the manufacture of carbonaceous material dispersions that solve the above-mentioned problems, and have determined that nitrogen-containing heterocyclic amide compounds such as N-methyl-2-pyrrolidone contain a large amount of amine components as impurities. When using carbonaceous material dispersions to form electrodes for lithium-ion secondary batteries, the amine components as impurities sometimes cause adverse effects such as coating failures, and the viscosity of each batch is not fixed.
[0023] As mentioned above, in the paste for electrodes, for the purpose of bonding metal foil, a binder component such as polyvinylidene fluoride resin (PVdF) is added, and a nitrogen-containing heterocyclic amide compound such as N-methyl-2-pyrrolidone is a solvent that can dissolve the binder component such as the polyvinylidene fluoride resin. However, among the amine components contained as impurities in the nitrogen-containing heterocyclic amide compound, since the polyvinylidene fluoride resin is a fluorine-based resin, if there is moisture, it is believed that a dehydrofluoric acid reaction caused by an alkaline substance is generated. In fact, the stronger the amine component that affects the polyvinylidene fluoride resin, the more color tends to be present, and the change in the UV absorption spectrum is also determined to be greater. The UV absorption spectrum was used as an indicator for investigation, and the results also showed that in our investigation, the degree of influence on the polyvinylidene fluoride resin was different depending on the type of amine.
[0024] Based on these aspects, the present inventors discovered that in the manufacture of a carbonaceous material dispersion, the concentration of the amine component and the water concentration in a nitrogen-containing heterocyclic amide compound such as N-methyl-2-pyrrolidone used as a non-aqueous solvent are managed so as to be below specified conditions, and a non-aqueous solvent satisfying these specified conditions is used to prepare the carbonaceous material dispersion. As a result, even if the carbonaceous material concentration is increased to 15 to 30% by mass, the viscosity is low. Moreover, when the obtained carbonaceous material dispersion is used, for example, in the manufacture of electrode slurry for lithium-ion secondary batteries, the viscosity of each batch of slurry is fixed, and an electrode that stably exhibits very excellent electrical properties can be formed, thereby completing the present invention.
[0025] It should be noted that in the present invention, in order to achieve low viscosity, a prescribed amine compound as a volatile pH adjuster is added as needed, but the prescribed amine compound has little effect on polyvinylidene fluoride resins and the like as binders, and after excluding the amine compound with high dispersion effect on carbonaceous materials and non-specific amine compounds contained as impurities in non-aqueous solvents such as N-methyl-2-pyrrolidone, the prescribed amine compound is added, so that when further kneading in the positive electrode active material and the binder during the preparation of the electrode slurry, it also becomes a stable kneading state, and the original function of the binder is successfully maintained. As a result, when the positive electrode paste is finally manufactured, the concentration of the amine component is always managed, so that the fluctuation of the viscosity of each batch is suppressed, and the failure during manufacturing is sharply reduced.
[0026] That is, the present invention for solving the above-mentioned problems is a method for producing a carbonaceous material dispersion liquid, characterized in that it is a method for producing a carbonaceous material dispersion liquid in which a carbonaceous material is dispersed in a non-aqueous solvent containing a nitrogen-containing heterocyclic amide compound having a solvent purity of 99.9% or more, and the production method comprises the following steps:
[0027] Amine management concentration confirmation step: confirm that the amine component concentration in the non-aqueous solvent is less than 3×10 -6 ;
[0028] The water management concentration confirmation step is to confirm that the water concentration in the non-aqueous solvent is less than 5×10 -4 ;and,
[0029] In the dispersing step, a carbonaceous material is added to the non-aqueous solvent satisfying the conditions in the above-mentioned amine management concentration confirmation step and water management concentration confirmation step so that the carbonaceous material concentration becomes 15 to 30% by mass based on the total mass, and the mixture is stirred and mixed.
[0030] In one embodiment of the method for producing a carbonaceous material dispersion of the present invention, a method for producing a carbonaceous material dispersion in which the nitrogen-containing heterocyclic amide compound is a 2-pyrrolidone is described.
[0031] In one embodiment of the method for producing a carbonaceous material dispersion of the present invention, a method for producing a carbonaceous material dispersion in which the nitrogen-containing heterocyclic amide compound is N-methyl-2-pyrrolidone is described.
[0032] In one embodiment of the method for producing a carbonaceous material dispersion of the present invention, a method for producing a carbonaceous material dispersion characterized in that a resin-based dispersant is added as a dispersant is described.
[0033] In one embodiment of the method for producing a carbonaceous material dispersion of the present invention, a method for producing a carbonaceous material dispersion characterized by adding a predetermined amine compound as a dispersant is described.
[0034] In one embodiment of the method for producing a carbonaceous material dispersion of the present invention, a method for producing a carbonaceous material dispersion characterized in that the carbonaceous material is carbon black is described.
[0035] In one embodiment of the method for producing a carbonaceous material dispersion of the present invention, a method for producing a carbonaceous material dispersion is described in which a dispersion treatment is performed so that two or more particle size peaks are formed when the dispersion is measured with a laser diffraction particle size distribution analyzer.
[0036] The present invention for solving the above-mentioned problems is also a carbonaceous material dispersion obtained by the above-mentioned method for producing a carbonaceous material dispersion, wherein the carbonaceous material concentration is 15 to 30% by mass relative to the total mass, and the concentration of the amine component in the dispersion other than the predetermined amine compound added as required is less than 3×10 -6 , the water concentration in the dispersion is less than 1×10 -3 .
[0037] In one embodiment of the carbonaceous material dispersion of the present invention, a carbonaceous material dispersion in which the carbonaceous material is carbon black and the nitrogen-containing heterocyclic amide compound is N-methyl-2-pyrrolidone is shown.
[0038] One embodiment of the carbonaceous material dispersion of the present invention shows a carbonaceous material dispersion characterized by having a viscosity of 50 to 500 mPa·s.
[0039] One embodiment of the carbonaceous material dispersion of the present invention shows a carbonaceous material dispersion having two or more particle size peaks when measured with a laser diffraction particle size distribution analyzer.
[0040] In one embodiment of the carbonaceous material dispersion of the present invention, there is shown a carbonaceous material dispersion having two or more particle size peaks when measured by a laser diffraction particle size distribution meter, wherein the height ratio (P1:P2) of at least two main peaks P1 and P2 among these peaks is 1:0.7 to 0.7:1.
[0041] Effects of the Invention
[0042] According to the present invention, it is possible to obtain a carbonaceous material dispersion liquid which is highly dispersed at a relatively low solvent content, has a low viscosity, and can exhibit excellent electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a graph showing the particle size distribution in one embodiment of the carbonaceous material dispersion of the present invention. DETAILED DESCRIPTION
[0044] Hereinafter, the present invention will be described in more detail based on specific embodiments.
[0045] <Method for producing carbonaceous material dispersion>
[0046] The method for producing a carbonaceous material dispersion of the present invention is characterized in that it is a method for producing a carbonaceous material dispersion in which a carbonaceous material is dispersed in a non-aqueous solvent containing a nitrogen-containing heterocyclic amide compound having a solvent purity of 99.9% or more, and the method comprises the following steps:
[0047] Amine management concentration confirmation step: confirm that the amine component concentration in the non-aqueous solvent is less than 3×10 -6 ;
[0048] The water management concentration confirmation step is to confirm that the water concentration in the non-aqueous solvent is less than 5×10 -4 ;and,
[0049] In the dispersing step, a carbonaceous material is added to the non-aqueous solvent satisfying the conditions in the above-mentioned amine management concentration confirmation step and water management concentration confirmation step so that the carbonaceous material concentration becomes 15 to 30% by mass based on the total mass, and the mixture is stirred and mixed.
[0050] (Nitrogen-containing heterocyclic amide compound)
[0051] Examples of the nitrogen-containing heterocyclic amide compound used in the present invention include 2-pyrrolidones represented by the general formula (I).
[0052]
[0053] 〔In the formula, R 1 and R 2 Each is independently hydrogen or an alkyl group having 1 to 4 carbon atoms.]
[0054] Specifically, as 2-pyrrolidones, for example, 2-pyrrolidones, N-methyl-2-pyrrolidones, N-ethyl-2-pyrrolidones, N-propyl-2-pyrrolidones, N-butyl-2-pyrrolidones, 5-methyl-2-pyrrolidones, 5-ethyl-2-pyrrolidones, 5-propyl-2-pyrrolidones, etc. can be enumerated, and they can be used alone or mixed with two or more. Among these 2-pyrrolidones, N-methyl-2-pyrrolidones is particularly preferred.
[0055] There are no particular limitations on the synthesis method and supply route of the nitrogen-containing heterocyclic amide compound, particularly N-methyl-2-pyrrolidone, used in the present invention. The compound may be synthesized by any synthesis method and supply route, but it is desirable that the synthesis method and supply route be such that amine components and water are not easily mixed in as impurities.
[0056] For example, N-methyl-2-pyrrolidone is not particularly limited, and one produced by the synthesis method shown below and subjected to a purification treatment such as adsorption or distillation as necessary (newly produced product) can be used.
[0057] As a method for producing N-methyl-2-pyrrolidone (NMP), for example, the following method can be mainly exemplified by way of non-limiting example:
[0058] A method for producing γ-butyrolactone (GBL) by reacting methylamine in an axial reaction tower at 200 to 350° C. and about 10 MPa (Ullmann's Encyclopedia of Industrial chemistry, 5th Ed., Vol. A22, pages 458 to 459);
[0059] A method for producing γ-butyrolactam (2-pyrrolidone, γ-BL) from GBL (selectivity: 94 mol %) by complete reaction with liquid ammonia at 270° C. and about 120 bar, for example in a series of three stirred reactors, and forming NMP in the same manner as methylamine (Winnacker, Kuechler "Chemische Technologie", 4th edition, 1982, Vol. 6, p. 99, lines 5-9);
[0060] For example, as described in Japanese Patent Application Laid-Open No. 10-158238, γ-BL is reacted with excess monomethylamine (MMA) in the presence of water at 250 to 300° C. to form NMP;
[0061] As described in Japanese Patent Application Laid-Open No. 1-190667, a method for producing NMP based on the reaction of γ-BL with excess MMA;
[0062] As described in Japanese Patent Application Laid-Open No. 7-218751, a method for synthesizing NMP is based on heating γ-BL or its open-chain derivatives with dimethylamine (DMA) and / or trimethylamine (TMA) at 200° C. or above;
[0063] As described in Japanese Patent Application Laid-Open No. 1-186864, in the presence of water, a corresponding lactone is reacted with a secondary amine to produce an N-alkylated lactam via a corresponding N,N-dialkyl-ω-hydroxyformamide as an intermediate (it should be noted that according to Example 1 described in the patent publication, NMP was obtained at a yield of 60% by reacting γ-BL with aqueous DMA, and methylamide of γ-hydroxybutyric acid was additionally formed. In another example based on the publication, a 60% yield of NMP was also reported in the corresponding reaction of γ-BL with DMA.);
[0064] As described in Japanese Patent Laid-Open No. 1-186863, a method for producing N-alkylated lactam by reacting the corresponding lactone with a tertiary amine or a tertiary or quaternary ammonium compound in the presence of water and removing the corresponding alcohol (it should be noted that according to Example 1 of the patent gazette, NMP was obtained in a yield of 8% by reacting γ-BL with aqueous TMA, and a large amount of by-products such as methylamide of γ-hydroxybutyric acid, 2-pyrrolidone and γ-hydroxybutyric acid were formed.);
[0065] As described in Japanese Patent Publication No. 4-47021420, a method for synthesizing NMP is based on reacting GBL with MeNH2 in the presence of water;
[0066] As described in Chem.Abstracts 124:145893 (CN-A-1104635), a method for synthesizing NMP based on reacting GBL with MeNH2 at 220-290°C and ≥6MPa (a mixture of GBL, 30% aqueous MeNH2 and water was reacted in batches at a ratio of 1:1.4:5.6 at 280°C and 6MPa to obtain NMP in a yield of 97%);
[0067] As described in International Patent Publication No. WO99 / 52867, a method for continuously producing NMP by reacting GBL with MMA in three consecutive reaction steps in a liquid phase (in this case, the first stage is operated at a temperature of 150 to 220° C., the second stage is operated at a temperature of 220 to 270° C., and the third stage is operated at a temperature of 250 to 310° C. The pressure of all three steps is 30 to 90 ATE (30.4 and 91.2 bar), preferably 40 to 60 ATE (40.5 and 60.8 bar). The molar ratio of GBL to MMA is 1:1.05 to 1:1.4);
[0068] As described in Chem. Abstract 82:13994, a method for producing the same is to react 1 part of GBL with 2 parts of MMA and 2 to 4 parts of water (= molar ratio 1:5.5:9.6 to 19.1) at 200 to 300°C, particularly 230 to 300°C (2 hours);
[0069] As described in Chem. Abstract 87:5802, a mixture of 1:1.4:4 (molar ratio = 1:3.9:19.1) was heated at 250°C and at 45-50 kg / cm 2 A method for reacting GBL with MMA and water;
[0070] A purification method for NMP based on treatment with an alkali metal hydroxide in aqueous solution followed by distillation, as shown in U.S. Pat. No. 2,964,535; and
[0071] As shown in Japanese Patent Publication No. 2006-503793, it is a method for continuously producing NMP by reacting GBL and MMA in a liquid phase, in which GBL and MMA are used in a molar ratio of 1:1.08 to 1:2, and the reaction is carried out at a temperature of 320 to 380° C. and an absolute pressure of 70 to 120 bar; etc.
[0072] Alternatively, for example, any recycled product obtained by a distillation purification process may be used, such as a lithium-ion secondary battery manufacturing process, a coating process of applying a polyvinylidene fluoride resin solution to the surface of a substrate such as a metal plate or a resin molded body, or a waste liquid of N-methyl-2-pyrrolidone used in any other process.
[0073] Among them, from the aspect that any one of the amine component concentration and the water concentration is easily and well controlled, it is particularly preferred to use a regenerated product obtained from a waste liquid from a lithium ion secondary battery manufacturing process. In particular, a regenerated product obtained from a waste liquid from a manufacturing process such as a carbonaceous material dispersion liquid manufactured by the manufacturing method of the present invention, a lithium ion secondary battery manufacturing process, etc. is the most ideal. That is, it is preferred to use a regenerated product obtained from a waste liquid from a manufacturing process using a carbonaceous material dispersion liquid manufactured by the manufacturing method of the present invention for use in the manufacturing method of the present invention again.
[0074] The nitrogen-containing heterocyclic amide compound used as the non-aqueous solvent in the present invention is assumed to be mainly an amine compound and water as described below as impurities, but it is desirable that other components are not contained as much as possible. From this point of view, it is ideal to have a purity of at least 99.9% or more, and more preferably a purity of 99.95% or more. It should be noted that the purity is measured by a Karl Fischer moisture meter and a gas chromatograph.
[0075] (Carbonaceous materials)
[0076] As the carbonaceous material used, there is no particular limitation as long as it has conductivity and can be in a powdery form, and examples thereof include carbon black (CB), carbon nanotubes (CNT), carbon nanofibers (CNF), graphene, fullerene, natural graphite, artificial graphite, difficult graphitization carbon, coke, graphite, etc., which can be used alone or in combination of two or more. As a carbonaceous material, CB is particularly preferred. Further as CB, for example, furnace black, Ketjen black, channel black, acetylene black, thermal black, etc. can be cited, and any one of them can be used. Among them, for example, acetylene black has a low metal component content in its preparation method, so it is preferred.
[0077] It should be noted that as carbon black, carbon black that has been subjected to a conventional oxidation treatment, carbon black that has been subjected to a graphitization treatment, etc. may also be used. The oxidation treatment of carbon black is a treatment in which carbon black is subjected to a high-temperature treatment in air, or subjected to a secondary treatment with nitric acid, nitrogen dioxide, ozone, etc., so that oxygen-containing polar functional groups such as phenolic groups, quinone groups, carboxyl groups, and carbonyl groups are directly introduced (covalently bonded) to the surface of carbon black to improve the dispersibility of carbon black.
[0078] If necessary, the carbonaceous material may be subjected to dry magnetic separation to remove mixed metal impurities before the preparation of the carbonaceous material dispersion, and / or dispersed in a non-aqueous solvent as the carbonaceous material dispersion and then subjected to wet magnetic separation.
[0079] In this specification, the "powdered particulate" form of the carbonaceous material as a raw material dispersed in the non-aqueous solvent is not limited as long as it can at least be dispersed in the above-mentioned non-aqueous solvent. Furthermore, its shape is not particularly limited, and is not limited to a roughly spherical shape, and can include an elliptical shape, a thin sheet shape, a needle shape, a short fiber shape, an amorphous shape, etc.
[0080] It should be noted that, regarding carbon black, as described on the website of the Carbon Black Association (https: / / carbonblack.biz / index.html), the smallest unit that cannot be decomposed into carbon black is an aggregate (primary aggregate), and a part of it (domain) is generally referred to as a particle. The particles are considered to belong to the particles defined as the smallest unit in nanomaterials, but they are only a part of the aggregate. The aggregate forms an agglomerate (secondary aggregate) through physical forces such as van der Waals forces. Furthermore, most carbon black products are transported and sold in the form of pellets, and the pellets are processed into beads by compression and granulation to prevent scattering and improve operability.
[0081] For example, it may include: primary aggregates with an average particle size of about 10 to 100 nm, secondary aggregates formed by agglomerating such primary aggregates to have an average particle size of about 0.1 to 100 μm, or particles processed into an average particle size of about 500 to 5000 μm by compression treatment or granulation treatment in consideration of operability.
[0082] It should be noted that, from the viewpoint of carbon black conductivity, as conductive carbon fine particles, it is preferred that primary particles are connected to some extent to form a collection of structures such as chains or house-like structures. The connector of the primary particles in the collection is also called a structure, and its degree of development can be observed by particle size distribution measurement (dynamic light scattering method or laser diffraction / light scattering method) and electron microscopy (both scanning type and transmission type can be used.) This structure can effectively form a conductive path between the positive electrode active material particles. Therefore, it is possible to give the positive electrode active material layer excellent conductivity with less dosage.
[0083] (Amine management concentration confirmation process and water management concentration confirmation process)
[0084] In the production method of the present invention, first, an amine management concentration confirmation step and a water management concentration confirmation step are performed for confirming the amine component concentration and water concentration of the non-aqueous solvent having a purity of 99.9% or more.
[0085] The amine management concentration confirmation step and the water management concentration confirmation step may be performed for each batch of the non-aqueous solvent used, or may be performed at fixed intervals or arbitrary intervals in a continuous production plant, for example, on non-aqueous solvent samples taken out through a sample collection line.
[0086] The amine management concentration confirmation step and the water management concentration confirmation step may be separate steps or may be steps performed simultaneously.
[0087] The amine management concentration confirmation step is usually performed using an ion chromatograph. It can be performed by a method of quantitatively analyzing all peaks of the amine substances that are expected to be mixed in advance using a standard curve, an internal standard method, a standard addition method, etc. In this way, it is confirmed whether the amine component concentration in the non-aqueous solvent is less than 3×10 mass fraction. -6 , more preferably less than 2×10 -6 , further expected to be less than 1×10 -6 Here, when setting such an amine management concentration, if the amine component concentration in the non-aqueous solvent is 3×10 -6If the above is exceeded, there is a concern that the carbonaceous material dispersion may become unstable. Furthermore, when the binder component described later is added to the prepared carbonaceous material dispersion, the viscosity of each batch of the carbonaceous material dispersion may fluctuate, and there is a concern that workability may be reduced. It should be noted that, as impurities, a part of non-specific amine substances contained in the non-aqueous solvent is not particularly limited, for example, when it contains ethylenediamine, cyclohexylamine, dipropylamine, 2-ethylpiperidine, morpholine, etc., it is believed that the possibility of affecting the viscosity of the above-mentioned carbonaceous material dispersion becomes higher, but by performing concentration management, that is, the concentration of the amine component in the above-mentioned non-aqueous solvent is less than 3×10 -6 Even if amines that are considered to have such a high influence are contained as impurities, the desired improvement effect can be exerted.
[0088] It should be noted that, when a prescribed amine compound is added as a dispersant when preparing a carbonaceous material dispersion as described later, the amine component concentration, i.e., the amine management concentration, here does not include the concentration of the prescribed amine compound, and is the total amount of amine components other than these (assuming that the non-aqueous solvent used originally contains the same compound as the prescribed amine compound as an impurity, the total amount of the amount later added as a dispersant and the amount originally present as an impurity is excluded from the calculation of the amine management concentration).
[0089] In addition, the water management concentration confirmation step can be carried out using, for example, a Karl Fischer water concentration meter, a near-infrared absorbance type micro-water concentration meter, a refractive index concentration meter, etc. Or it can be carried out more accurately by using a gas chromatograph using an ion liquid phase column. Thus, it is confirmed whether the water concentration in the non-aqueous solvent is less than 5×10 mass fraction. -4 , and more expected to be less than 2×10 -4 , further expected to be less than 1×10 -4 Here, when such a moisture management concentration is set, in the carbonaceous material dispersion of the present invention, the solvent (including water) in the dispersion is usually finally removed when the carbonaceous material dispersion is used to manufacture products. Therefore, when the amount of water in the solvent increases, there is a concern that an adverse condition will occur in the manufacturing process of such a product. Furthermore, when the binder component described later is mixed into the prepared carbonaceous material dispersion, there is a concern that the presence of water in the non-aqueous solvent will have a significant impact on the fluctuation of the viscosity in the above-mentioned mixture.
[0090] When it is determined that the non-aqueous solvent used satisfies the criteria in either the amine management concentration confirmation step or the water management concentration confirmation step, the process proceeds to the dispersion step of dispersing the carbonaceous material in the non-aqueous solvent.
[0091] On the other hand, in either the amine management concentration confirmation step or the water management concentration confirmation step, when it is determined that the non-aqueous solvent does not satisfy the criteria, the non-aqueous solvent is not used directly in the dispersion treatment.
[0092] The non-aqueous solvent is subjected to purification treatments such as (1) distillation purification, (2) contact with an acidic substance such as an inorganic acid such as sulfuric acid, nitric acid, phosphoric acid, and hydrochloric acid, a water-soluble inorganic acid such as isopolyacid, heteropolyphosphoric acid, tungstosilicic acid, and molybdosilicic acid, a water-insoluble inorganic solid acid such as zeolite, alumina, silica-alumina, silica-magnesia, and silica-zirconia, activated carbon that has been pre-treated with an acid, a water-insoluble acidic cation exchange resin such as a strongly acidic cation exchange resin, or an organic carboxylic acid such as acetic acid, propionic acid, butyric acid, succinic acid, lactic acid, malic acid, and oxalic acid, or (3) contact with an acidic substance followed by distillation purification, and then is again subjected to the amine management concentration confirmation step and the water management concentration confirmation step.
[0093] Of course, instead of using the non-aqueous solvent, another new non-aqueous solvent may be used in the amine management concentration confirmation step and the water management concentration confirmation step.
[0094] (Dispersion process)
[0095] For the non-aqueous solvent, if it is judged that the criteria are met in either the amine management concentration confirmation process or the water management concentration confirmation process, a carbonaceous material is added to the non-aqueous solvent and stirred and mixed to disperse it, thereby preparing a carbonaceous material dispersion having a carbonaceous material concentration of 15 to 30 mass % relative to the total mass of the dispersion.
[0096] As the carbonaceous material concentration relative to the total mass of the dispersion, 16 to 28 mass % is further preferred, and 18 to 25 mass % is particularly preferred. When the concentration of the carbonaceous material is less than the above, the energy required for solvent removal in product manufacturing, the transportation cost of the dispersion, and the cost of the solvent increase. On the other hand, if the concentration of the carbonaceous material is more than the above, it becomes difficult to obtain sufficient fluidity and the operability deteriorates.
[0097] The dispersing device is not particularly limited, and a disperser commonly used for pigment dispersion or the like can be used. For example, mixers such as dispersers, homomixers, and planetary mixers, homogenizers (such as "Claire Mix" manufactured by M Technique Co., Ltd., "Fill Mix" manufactured by PRIMIX, and "Abramix" manufactured by Silberson), paint conditioners (manufactured by Red Devil), colloid mills (such as "PUC Colloid Mill" manufactured by PUC and "Colloid Mill MK" manufactured by IKA), mills (such as "Corn Mill MKO" manufactured by IKA), ball mills, sand mills (such as "Dynomill" manufactured by Simmal Enterprises), attritors, bead mills (such as "DCP Mill" manufactured by Erich), media dispersers such as CoBall Mill, wet jet mills (such as "Genus PY" manufactured by Genus, "Starburst" manufactured by Sugino Machine Limited, and "Nanomizer" manufactured by Nanomizer), "Claire Mill" manufactured by M Technique Co., Ltd., and "Dyno Mill" manufactured by Simmal Enterprises). SS-5", "MICROS" manufactured by Nara Machinery Co., Ltd. and other media-free dispersers, other roll mills, etc., but are not limited to these.
[0098] Preferably, the carbonaceous material is finally dispersed in a grinder, particularly preferably a grinder using beads having an average particle size of 0.05 to 2 mm. It is further preferred that the dispersion treatment is performed using a shearing type dispersion device described in detail below before the dispersion treatment using the grinder, and then the dispersion treatment using the grinder is performed to prepare the carbonaceous material.
[0099] It should be noted that if the particle size of the beads used in the grinder is too small, there is a concern that the carbonaceous materials such as the primary aggregates of carbon black will be crushed very finely, and the dispersion process requires too much energy. In addition, due to the difficulty in operation, the average particle size of the beads is preferably above 0.05 mm, and particularly preferably above 0.5 mm. On the other hand, if the beads are too large, the number of beads per unit volume decreases, so the dispersion efficiency decreases, the pulverization of the carbonaceous materials becomes insufficient, and the particles of the carbonaceous materials exist in a state with a large aspect ratio, and there is a concern that the liquid properties as a coating or coating agent cannot be obtained. Therefore, the average diameter of the beads is preferably below 2 mm, and particularly preferably below 1.5 mm.
[0100] The material of the beads used as a dispersion medium in the grinder is not particularly limited, and examples thereof include alumina, zirconia, steel, chrome steel, glass, etc. Among them, zirconia beads are preferably used if contamination of the product and the size of the kinetic energy caused by specific gravity are taken into consideration.
[0101] The shape of the beads is not particularly limited, but spherical beads are generally used.
[0102] The structure of the grinder is not particularly limited, and various known grinders can be applied. Specifically, various known attritors, sand mills, bead mills, etc. can be mentioned.
[0103] It should be noted that the filling ratio of beads to the container can be determined according to the container, stirring mechanism, structure, etc., and is not particularly limited. If the ratio is too low, there is a concern that the carbonaceous material cannot be fully crushed or cut. On the other hand, if the ratio is too high, a large driving force is required for rotation, and there is a concern that the wear of the beads will cause an increase in the contamination of the treated medium. Therefore, the filling ratio of the beads is preferably set to about 70 to 85 volume % of the effective volume of the container.
[0104] In addition, operating conditions such as processing time, shaft speed, container internal pressure, engine load, etc. are determined by the blending amount of the carbonaceous material and the properties of the resin to be dispersed, especially the viscosity, compatibility with the carbonaceous material, etc., and can be appropriately set according to the purpose.
[0105] Before the dispersion treatment using the grinder, a preliminary dispersion treatment may be performed using other stirring apparatuses, for example, a shearing type agitator such as a disperser or a homomixer.
[0106] By performing the dispersion treatment in this manner, a dispersion having a viscosity of about 50 to 500 mPa·s, more preferably 100 to 400 mPa·s, and even more preferably 150 to 300 mPa·s is prepared.
[0107] In addition, in the preparation of the carbonaceous material dispersion, it is desirable to disperse the carbonaceous material in the obtained dispersion so that the carbonaceous material is dispersed as shown in FIG. Figure 1 As shown, two or more particle size peaks are formed. Since two or more particle size peaks are formed in this way, good dispersibility and fluidity can be exhibited, and the aggregation structure of carbon black and the like can be appropriately maintained to a certain extent, for example, when forming an electrode, good conductive properties can be exhibited.
[0108] It is particularly desired that primary particles or primary aggregates and secondary aggregates of carbon black, etc. exist in a sufficient proportion, and that at least two particle size peaks are formed when measured by a laser diffraction particle size distribution meter, and that the height ratio (P1:P2) of at least two main peaks P1 and P2 among these peaks is 1:0.7 to 0.7:1.
[0109] (Dispersant)
[0110] When the carbonaceous material dispersion of the present invention is prepared as described above, it is preferable to add a resinous dispersant and / or a predetermined amine compound as a dispersant in order to obtain the above-mentioned high fluidity. In particular, it is preferable to add both a resinous dispersant and a predetermined amine compound.
[0111] Examples of the resin dispersant include polyvinyl alcohols, methyl cellulose, ethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl acetals, polyvinyl pyrrolidones, etc., among which polyvinyl alcohol and methyl cellulose are particularly preferred. The amount of the resin dispersant added is about 0.01 to 5% by mass, more preferably 0.05 to 3% by mass, and even more preferably about 0.1 to 2% by mass relative to the total amount of the dispersion.
[0112] As the prescribed amine compound, for example, tertiary amine, secondary amine, primary amine, cyclic amine, and compounds having an amino group and a hydroxyl group in an alkane skeleton, i.e., alkanolamine or amino alcohol, or other amines such as diglycolamine, tris(hydroxymethyl)aminomethane (THAM), and morpholine can be exemplified. It should not be particularly limited, and among them, for example, 2-methylaminoethanol, 2-amino-1-butanol, 4-ethylamino-1-butanol, triethylamine, 2-amino-2-ethyl-1,3-propanediol (AEPD), 2-amino-2-methyl-1-propanol (AMP), THAM, etc. are particularly preferred. Moreover, the addition amount of the prescribed amine compound is about 0.01 to 5%, more preferably 0.05 to 3%, and even more preferably about 0.1 to 2% relative to the total amount of the dispersion.
[0113] (Binder)
[0114] The carbonaceous material dispersion of the present invention may further contain a binder. Alternatively, when the carbonaceous material dispersion of the present invention is used to prepare, for example, a slurry for an electrode, such a binder may be used in combination.
[0115] As the binder used, there can be cited: polymers or copolymers containing ethylene, propylene, vinyl chloride, vinyl acetate, vinyl alcohol, maleic acid, acrylic acid, acrylate, methacrylic acid, methacrylate, acrylonitrile, styrene, vinyl butyral, vinyl acetal, vinyl pyrrolidone, etc. as structural units; polyurethane resin, polyester resin, phenolic resin, epoxy resin, phenoxy resin, urea resin, melamine resin, alkyd resin, acrylic resin, formaldehyde resin, silicone resin, fluororesin; rubbers such as styrene-butadiene rubber and fluororubber; conductive resins such as polyaniline and polyacetylene, etc. In addition, it can also be a modified body, mixture and copolymer of these resins. In the use of lithium ion secondary batteries, it is particularly preferred to use polymer compounds having fluorine atoms in the molecule, such as polyvinylidene fluoride, polyvinyl fluoride, tetrafluoroethylene, etc.
[0116] In addition, the weight average molecular weight of these resins as binders is preferably 10,000 to 2,000,000, more preferably 100,000 to 1,000,000, and particularly preferably 200,000 to 1,000,000. If the molecular weight is small, the resistance and adhesion of the binder are sometimes reduced. If the molecular weight becomes large, although the resistance and adhesion of the binder are improved, the viscosity of the binder itself becomes high, the workability is reduced, and it acts as an aggregating agent, and the dispersed particles sometimes aggregate significantly.
[0117] From the perspective of the industrial applicability of the present invention, the binder preferably contains a polymer compound having fluorine atoms, preferably a polymer compound having fluorine atoms, more preferably a vinylidene fluoride copolymer, and particularly preferably polyvinylidene fluoride.
[0118] <Carbonaceous material dispersion>
[0119] The carbonaceous material dispersion of the present invention is a carbonaceous material dispersion obtained by the method for producing a carbonaceous material dispersion of the present invention, wherein the carbonaceous material concentration is 15 to 30% by mass relative to the total mass, and the concentration of the amine component in the dispersion excluding the specified amine compound added as required is less than 3×10 -6 , the water concentration in the dispersion is less than 1×10 -3 .
[0120] As for the amine component concentration of the carbonaceous material dispersion, it is desirable that it is less than 3×10 mass fraction, similarly to the amine management concentration in the production method. -6 , more preferably less than 2×10 -6 , further expected to be less than 1×10 -6 .
[0121] On the other hand, the water concentration of the carbonaceous material dispersion is less than 1×10 -3 , more preferably less than 5×10 -4 , further expected to be less than 2×10 -4 The moisture management concentration in the manufacturing method is less than 5×10 -4 , and more expected to be less than 2×10 -4 , further expected to be less than 1×10 -4 , while the water concentration of the carbonaceous material dispersion as a product is slightly increased within the allowable range. This is because, even if the water concentration of the non-aqueous solvent used for manufacturing is managed within the above range, the product will absorb moisture from the air during the manufacturing process or during subsequent storage, and there is a possibility that the moisture content will increase. However, even if the moisture content in the product is slightly higher than the moisture management concentration during manufacturing, there is no particular problem in the product characteristics. On the contrary, with regard to the moisture management concentration during manufacturing, the product will absorb moisture from the air, and even if the moisture concentration increases, it will not affect the product characteristics, and the result is preset to be low.
[0122] It should be noted that, regarding the carbonaceous material dispersion of the present invention, as described in the description of the above-mentioned manufacturing method, it is desirable that the carbonaceous material is carbon black and the nitrogen-containing heterocyclic amide compound is N-methyl-2-pyrrolidone. Similarly, as described above, it is desirable that when measured with a laser diffraction particle size distribution meter, two or more particle size peaks are formed, and further, the height ratio (P1: P2) of at least two main peaks P1 and P2 among these peaks is 1: 0.7 to 0.7: 1.
[0123] The carbonaceous material dispersion of the present invention is not particularly limited, but its viscosity is preferably 50 to 500 mPa·s, more preferably 100 to 400 mPa·s, and even more preferably 150 to 300 mPa·s.
[0124] (Application of Carbonaceous Material Dispersion Liquid)
[0125] The carbonaceous material dispersion of the present invention further contains the above-mentioned binder and the following electrode active material, and can be prepared as an electrode paste. It is particularly preferred that the carbonaceous material dispersion containing the above-mentioned dispersant, carbon black as a carbonaceous material, and N-methyl-2-pyrrolidone as a non-aqueous solvent is used as an electrode paste containing a binder and an electrode active material.
[0126] (Electrode Active Material)
[0127] The positive electrode active material for lithium ion secondary batteries is not particularly limited, and metal compounds such as metal oxides and metal sulfides, and conductive polymers that can be doped or intercalated with lithium ions can be used.
[0128] For example, inorganic compounds such as oxides of transition metals such as Fe, Co, Ni, and Mn, composite oxides with lithium, and transition metal sulfides can be cited. Specifically, MnO, V2O5, V6O 13 , transition metal oxide powders such as TiO2, composite oxide powders of lithium and transition metals such as lithium nickelate, lithium cobaltate, lithium manganate, and lithium manganate with a spinel structure, phosphate compounds with an olivine structure, i.e., lithium iron phosphate-based materials, transition metal sulfide powders such as TiS2 and FeS, etc. In addition, conductive polymers such as polyaniline, polyacetylene, polypyrrole, and polythiophene can also be used. In addition, the above-mentioned inorganic compounds and organic compounds can be mixed and used.
[0129] There are no particular limitations on the negative electrode active material for lithium ion secondary batteries as long as it can be doped or embedded with lithium ions. Examples include metal Li, alloys thereof such as tin alloys, silicon alloys, and lead alloys, and Li X Fe2O3、Li X Fe3O4、Li X WO2, metal oxides such as lithium titanate, lithium vanadate, lithium silicate, conductive polymers such as polyacetylene, polyparaphenylene, amorphous carbonaceous materials such as soft carbon and hard carbon, artificial graphite such as highly graphitized carbon materials, or carbonaceous powders such as natural graphite, carbon black, mesophase carbon black, resin-baked carbon materials, vapor-deposited carbon fibers, carbon fibers, etc. These negative electrode active materials can be used alone or in combination.
[0130] The average particle size of these electrode active materials is preferably in the range of 0.05 to 100 μm, more preferably in the range of 0.1 to 50 μm. The average particle size of the electrode active material in this specification refers to the average value of the particle size measured with an electron microscope.
[0131] The electrode paste can be prepared by mixing the above-mentioned carbonaceous material dispersion, a binder and an electrode active material. There is no limitation on the order of adding the components, and for example, the following methods can be cited: a method of mixing all the components at the same time; a method of adding the remaining components to the carbonaceous material dispersion prepared in advance by the above method and mixing; a method of adding a binder to the carbonaceous material dispersion prepared in advance by the above method, kneading, and then adding the electrode active material to the kneaded product and mixing; etc.
[0132] As an apparatus for producing the electrode paste, the same apparatus as that used in producing the carbonaceous material dispersion of the present invention can be used.
[0133] Example
[0134] Hereinafter, the present invention will be described in detail based on Examples, but the present invention is not limited to the following Examples unless the gist thereof is exceeded. In the present examples, "part" represents part by mass, and "%" represents % by mass.
[0135] Carbon black (sometimes abbreviated as "CB"), a dispersant, a binder, etc. used in Examples and Comparative Examples are shown below.
[0136] <Carbon black>
[0137] Denka Black granular product (manufactured by Denka Company Limited): acetylene black, specific surface area 69m 2 / g.
[0138] <Non-aqueous solvent>
[0139] As the non-aqueous solvent, the following were used.
[0140] N-Methyl-2-pyrrolidone (NMP).
[0141] As the non-aqueous solvent NMP, various substances were prepared, and their compositions were as follows.
[0142] NMP-A: A product produced by Japan Refine Co., Ltd. and purified by distillation from waste liquid from the lithium-ion secondary battery manufacturing process.
[0143] NMP-B: a new liquid of commercially available NMP.
[0144] NMP-C1: a mixture of 16.67 parts by mass of the above-mentioned NMP-B and 483.33 parts by mass of the above-mentioned NMP-A.
[0145] NMP-C2: a mixture of 50.00 parts by mass of the above-mentioned NMP-B and 450.00 parts by mass of the above-mentioned NMP-A.
[0146] NMP-AW1: A comparative product obtained by adding 0.01% of purified water to the above-mentioned NMP-A.
[0147] NMP-AW2: A comparative product obtained by adding 0.05% of purified water to the above-mentioned NMP-A.
[0148] NMP-AW3: A comparative product obtained by adding 0.10% of purified water to the above-mentioned NMP-A.
[0149] NMP-AA1: Add 2-ethylpiperidine to the above NMP-A to make the mass fraction 3×10 -6 And the accomplished ones.
[0150] NMP-AA2: Add morpholine to the above NMP-A to make the mass fraction 3×10 -6 .
[0151] NMP-AA3: Add triethylamine to the above NMP-A to make the mass fraction 3×10 -6 .
[0152] <Dispersant>
[0153] Polyvinyl alcohol 500 (Kanto Chemical): degree of polymerization 500, degree of saponification 86.5 to 89.0%, hereinafter referred to as PVA.
[0154] <Specified amine compounds>
[0155] AEPD: 2-amino-2-ethyl-1,3-propanediol.
[0156] <Binder>
[0157] KF Polymer W9100 (manufactured by KUREHA CORPORATION): polyvinylidene fluoride (PVDF), weight average molecular weight of about 280000. Hereinafter, it is abbreviated as W9100.
[0158] <Evaluation of Carbonaceous Material Dispersion Liquid>
[0159] The carbonaceous material dispersions obtained in Examples 1 to 14 and Comparative Examples 1 to 9 were evaluated by measuring the initial viscosity value and the viscosity change rate. The evaluation method is as follows.
[0160] <Initial viscosity value and viscosity change rate>
[0161] The dispersion stability that is the subject of the present invention can be evaluated based on the viscosity change rate of the obtained carbonaceous material dispersion over time. The viscosity change rate is evaluated as follows: it is evaluated based on the change rate of the viscosity measurement value after standing at 25°C for 10 days, 17 days or 30 days when the viscosity measurement value after dispersion (initial viscosity value) is used as a reference. The smaller the change, the better the stability. The viscosity value is measured as follows: using a B-type viscometer ("BL" manufactured by Toki Sangyo Co., Ltd.), the dispersion composition is fully stirred with a scraper at a temperature of 25°C and a rotor speed of 60rpm, and then the measurement is performed immediately. The rotors used in the measurement are: No. 20 when the viscosity value is less than 100mPa·s, No. 21 when it is greater than 100mPa·s and less than 500mPa·s, No. 22 when it is greater than 500mPa·s and less than 2000mPa·s, and No. 23 when it is greater than 2000mPa·s and less than 10000mPa·s.
[0162] <Concentration of amine components, water content, and impurities in NMP>
[0163] [Preliminary test 1]
[0164] The amine component concentration (mass fraction), water content (mass fraction), and solvent purity of each of NMP as the above-mentioned non-aqueous solvent were measured using an ion chromatograph, a Karl Fischer moisture meter, and a gas chromatograph.
[0165] As a result, the following analysis values were shown.
[0166] NMP-A: Amine component concentration 0.05×10 -6 , moisture 3×10 -5 , Solvent purity 99.95%
[0167] NMP-C1: Amine component concentration 1.0×10 -6 , moisture 3×10 -5 , Solvent purity 99.95%
[0168] NMP-C2: Amine component concentration 3.0×10 -6 , moisture 3×10 -5 , Solvent purity 99.95%
[0169] NMP-AW1: Amine component concentration 0.05×10 -6 , moisture 1.3×10 -4 , Solvent purity 99.95%
[0170] NMP-AW2: Amine component concentration 0.05×10 -6 , moisture 5.3×10 -4 , Solvent purity 99.95%
[0171] NMP-AW3: Amine component concentration 0.05×10 -6 , moisture 1×10 -3 , Solvent purity 99.94%
[0172] NMP-B: Amine component concentration 3.0×10 -5 , moisture 3×10 -5 , Solvent purity 99.95%
[0173] NMP-AA1: Amine component (2-ethylpiperidine) concentration 3.0×10 -6 , moisture 3×10 -5 , Solvent purity 99.95%
[0174] NMP-AA2: Amine component (morpholine) concentration 3.0×10 -6 , moisture 3×10 -5, Solvent purity 99.95%
[0175] NMP-AA3: Amine component (triethylamine) concentration 3.0×10 -6 , moisture 3×10 -5 , Solvent purity 99.95%
[0176] In addition, except for NMP-A, NMP-C1, and NMP-AW1, at least one of the allowable ranges of the amine management concentration and the water management concentration specified in the present invention was exceeded.
[0177] <Preparation of Carbonaceous Material Dispersion>
[0178] [Example 1]
[0179] In a glass bottle, 77.5 parts of NMP-A as N-methyl-2-pyrrolidone, 1 part of PVA as a dispersant, and 0.5 parts of AEPD as a specified amine are placed, and after being fully mixed and dissolved or dispersed, 21 parts of carbon black granules are added, and zirconium oxide beads are used as a medium, and dispersed in a bead mill until the viscosity becomes less than 250 mPa·s. The carbonaceous material dispersion D-1 is obtained. The initial viscosity value of the carbonaceous material dispersion D-1 is 174 mPa·s. Moreover, the peak of the particle size measured by the laser diffraction particle size distribution meter is as follows: Figure 1 As shown, it exists at 1.01μm and 0.25μm, and the peak ratio is 1.0:0.9.
[0180] After standing at 25°C for 10 days, the viscosity of the dispersion was 166 mPa·s, with a viscosity change rate of 5%. After standing at 25°C for 17 days, the viscosity of the dispersion was 160 mPa·s, with a viscosity change rate of 8%. After standing at 25°C for 30 days, the viscosity of the dispersion was 161 mPa·s, with a viscosity change rate of 8%.
[0181] [Example 2]
[0182] Carbonaceous material dispersion D-C1 was obtained in the same manner except that NMP-C1 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 212 mPa·s, and the viscosity of the dispersion after standing at 25°C for 30 days was 192 mPa·s, with a viscosity change rate of 9%.
[0183] [Comparative Example 1]
[0184] Carbonaceous material dispersion D-C2 was obtained in the same manner except that NMP-C2 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 217 mPa·s, and the viscosity of the dispersion after standing at 25°C for 30 days was 183 mPa·s, with a viscosity change rate of 16%.
[0185] [Comparative Example 2]
[0186] Carbonaceous material dispersion DB was obtained in the same manner except that NMP-B was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 211 mPa·s, and the viscosity of the dispersion after standing at 25°C for 30 days was 180 mPa·s, with a viscosity change rate of 15%.
[0187] [Example 3]
[0188] Carbonaceous material dispersion D-AW1 was obtained in the same manner except that NMP-AW1 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 210 mPa·s. The viscosity of the dispersion after standing at 25°C for 10 days was 191 mPa·s, and the viscosity change rate was 10%.
[0189] [Comparative Example 3]
[0190] Carbonaceous material dispersion D-AW2 was obtained in the same manner except that NMP-AW2 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 220 mPa·s. The viscosity of the dispersion after standing at 25°C for 10 days was 183 mPa·s, and the viscosity change rate was 16%.
[0191] [Comparative Example 4]
[0192] Carbonaceous material dispersion D-AW3 was obtained in the same manner except that NMP-AW3 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 223 mPa·s. The viscosity of the dispersion after standing at 25°C for 10 days was 183 mPa·s, and the viscosity change rate was 18%.
[0193] [Reference Example 1]
[0194] Carbonaceous material dispersion D-AA1 was obtained in the same manner except that NMP-AA1 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 190 mPa·s. The viscosity of the dispersion after standing at 25° C. for 17 days was 158 mPa·s, and the viscosity change rate was 17%.
[0195] [Reference Example 2]
[0196] Carbonaceous material dispersion D-AA2 was obtained in the same manner except that NMP-AA2 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 205 mPa·s. The viscosity of the dispersion after standing at 25° C. for 17 days was 175 mPa·s, and the viscosity change rate was 15%.
[0197] [Reference Example 3]
[0198] Carbonaceous material dispersion D-AA3 was obtained in the same manner except that NMP-AA3 was used instead of NMP-A as N-methyl-2-pyrrolidone. The initial viscosity of the prepared dispersion was 207 mPa·s. The viscosity of the dispersion after standing at 25° C. for 17 days was 179 mPa·s, and the viscosity change rate was 14%.
[0199] [Example 4]
[0200] To 24.5 parts of the carbonaceous material dispersion prepared in Example 1, 70.5 parts of NMP-A and 5 parts of binder W9100 were added, and the mixture was mixed and dispersed in a stirrer at 60°C for 1 hour to prepare a coating paste. The initial viscosity of the prepared coating paste was 155 mPa·s, and the viscosity of the paste after standing at 45°C for 7 days was 599 mPa·s, indicating sufficient workability during coating and appropriate curability thereafter.
[0201] [Example 5]
[0202] To 24.5 parts of the carbonaceous material dispersion prepared in Example 2, 0.5 parts of NMP-C17 and 5 parts of the binder W9100 were added, and the mixture was fully mixed and dispersed in a stirrer at 60°C for 1 hour to prepare a coating paste. The initial viscosity of the prepared coating paste was 165 mPa·s, and the viscosity of the paste after standing at 45°C for 7 days was 550 mPa·s, indicating sufficient workability during coating and appropriate curability thereafter.
[0203] [Comparative Example 6]
[0204] To 24.5 parts of the carbonaceous material dispersion prepared in Comparative Example 1, 0.5 parts of NMP-C27 and 5 parts of the binder W9100 were added, and the mixture was fully mixed and dispersed in a stirrer at 60°C for 1 hour to prepare a coating paste. The initial viscosity of the prepared coating paste was 135 mPa·s, and the viscosity of the paste after standing at 45°C for 7 days was 403 mPa·s, indicating sufficient workability during coating, but the subsequent curability was significantly reduced compared to Example 4.
[0205] [Comparative Example 7]
[0206] To 24.5 parts of the carbonaceous material dispersion prepared in Comparative Example 2, 70.5 parts of NMP-B and 5 parts of binder W9100 were added, and the mixture was mixed and dispersed in a stirrer at 60°C for 1 hour to prepare a coating paste. The initial viscosity of the prepared coating paste was 128 mPa·s, and the viscosity of the paste after standing at 45°C for 7 days was 402 mPa·s, indicating sufficient workability during coating, but the subsequent curability was significantly reduced compared to Example 4.
[0207] [Reference Example 4]
[0208] To 24.5 parts of the carbonaceous material dispersion prepared in Reference Example 1, 170.5 parts of NMP-AA and 5 parts of binder W9100 were added, and the mixture was mixed and dispersed in a stirrer at 60°C for 1 hour to prepare a coating paste. The initial viscosity of the prepared coating paste was 140 mPa·s, and the viscosity of the paste after standing at 45°C for 7 days was 356 mPa·s, indicating that the workability during coating was insufficient, and the subsequent curability was significantly reduced compared to Example 4.
[0209] [Reference Example 5]
[0210] To 24.5 parts of the carbonaceous material dispersion prepared in Reference Example 2, 270.5 parts of NMP-AA and 5 parts of binder W9100 were added, and the mixture was mixed and dispersed in a stirrer at 60°C for 1 hour to prepare a coating paste. The initial viscosity of the prepared coating paste was 136 mPa·s, and the viscosity of the paste after standing at 45°C for 7 days was 320 mPa·s, indicating that the workability during coating was insufficient, and the subsequent curability was significantly reduced compared to Example 4.
[0211] [Reference Example 6]
[0212] To 24.5 parts of the carbonaceous material dispersion prepared in Reference Example 3, 370.5 parts of NMP-AA and 5 parts of binder W9100 were added, and the mixture was mixed and dispersed in a stirrer at 60°C for 1 hour to prepare a coating paste. The initial viscosity of the prepared coating paste was 131 mPa·s, and the viscosity of the paste after standing at 45°C for 7 days was 316 mPa·s, indicating that the workability during coating was insufficient, and the subsequent curability was significantly reduced compared to Example 4.
Claims
1. A method for producing a carbonaceous material dispersion, characterized in that: The present invention relates to a method for producing a carbonaceous material dispersion liquid in which a carbonaceous material is dispersed in a non-aqueous solvent containing a nitrogen-containing heterocyclic amide compound having a solvent purity of 99.9 mass % or more, and the method comprises the following steps: Amine management concentration confirmation step, confirming that the amine component concentration in the non-aqueous solvent is less than 3×10 -6 ; The water management concentration confirmation step is to confirm that the water concentration in the non-aqueous solvent is less than 5×10 -4 ; and, In the dispersing step, a carbonaceous material is added to the non-aqueous solvent satisfying the conditions in the amine management concentration confirmation step and the water management concentration confirmation step so that the carbonaceous material concentration becomes 15 to 30% by mass based on the total mass, and the mixture is stirred and mixed.
2. The method for producing a carbonaceous material dispersion according to claim 1, wherein: The nitrogen-containing heterocyclic amide compound is a 2-pyrrolidone.
3. The method for producing a carbonaceous material dispersion according to claim 1 or 2, wherein: The nitrogen-containing heterocyclic amide compound is N-methyl-2-pyrrolidone.
4. The method for producing a carbonaceous material dispersion according to claim 1 or 2, characterized in that: A resin-based dispersant is added as a dispersant.
5. The method for producing a carbonaceous material dispersion according to claim 1 or 2, characterized in that: A prescribed amine compound is added as a dispersant.
6. The method for producing a carbonaceous material dispersion according to claim 1 or 2, characterized in that: The carbonaceous material is carbon black.
7. The method for producing a carbonaceous material dispersion according to claim 1 or 2, wherein: The dispersion treatment is performed so that two or more particle size peaks are formed when the dispersion liquid is measured with a laser diffraction particle size distribution analyzer.
8. A carbonaceous material dispersion, characterized in that it is a carbonaceous material dispersion obtained by the method for producing a carbonaceous material dispersion according to any one of claims 1 to 7, wherein the carbonaceous material concentration is 15 to 30% by mass relative to the total mass, and the concentration of amine components in the dispersion excluding a predetermined amine compound added as required is less than 3×10 -6 , the water concentration in the dispersion is less than 1×10 -3 .
9. The carbonaceous material dispersion according to claim 8, wherein The carbonaceous material is carbon black, and the nitrogen-containing heterocyclic amide compound is N-methyl-2-pyrrolidone.
10. The carbonaceous material dispersion according to claim 8 or 9, characterized in that: The viscosity is 50 to 500 mPa·s. 11 . The carbonaceous material dispersion according to claim 8 , which forms two or more particle size peaks when measured using a laser diffraction particle size distribution analyzer.
12. The carbonaceous material dispersion according to claim 8 or 9, wherein When measured by a laser diffraction particle size distribution analyzer, two or more particle size peaks are formed, and the height ratio P1:P2 of at least two main peaks P1 and P2 among these peaks is 1:0.7 to 0.7:1.