A method for preparing a corrosion-resistant lightweight piston for a fuel tank

Through the liquid phase oxidation, epoxidation and hot pressing molding process of polyether ether ketone, inorganic short fiber and carbon nanoparticle composite materials, the corrosiveness and insufficient strength of the fuel tank piston material were solved, and hydroxylamine perchlorate fuel was realized. Improved corrosion resistance and sealing performance.

CN114770838BActive Publication Date: 2024-10-29LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210529181.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-16
Publication Date
2024-10-29
Estimated Expiration
2042-05-16

AI Technical Summary

Technical Problem

Existing fuel tank piston materials have problems such as low corrosivity, insufficient strength, and easy cracking during long-term storage and use, making it difficult to meet the corrosion resistance and sealing requirements of hydroxylamine perchlorate fuel.

Method used

A composite material composed of polyether ether ketone (PEEK) powder, inorganic short fibers and carbon nanoparticles is used to form a piston material with high strength and corrosion resistance through liquid phase oxidation, epoxidation, mechanical mixing and hot pressing molding processes. .

Benefits of technology

The tensile breaking strength, tensile modulus, compressive strength and impact strength of the piston are improved, the corrosion resistance of hydroxylamine perchlorate fuel is enhanced, the dead weight and the risk of jamming are reduced, and the yield and sealing performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114770838B_ABST
    Figure CN114770838B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a corrosion-resistant lightweight piston for a fuel tank, the method comprising the following steps: (1) weighing the following components by weight percentage: 40% to 90% polyetheretherketone (PEEK) powder, 5% to 45% inorganic short fibers, and 0.1% to 5% carbon nanoparticles; (2) fiber liquid phase oxidation; (3) fiber epoxidation; (4) carbon nanoparticle dispersion; (5) mechanical mixing; (6) material kneading; (7) piston hot pressing molding; (8) heat treatment of the piston blank; (9) mechanical processing of the piston blank. The present invention can effectively improve the yield rate and make the product less prone to cracking. The obtained polymer composite material piston can greatly reduce the dead weight of the fuel supply tank, has good corrosion resistance, is particularly suitable for hydroxylamine perchlorate and its mixed fuel, has a significant improvement in the sealing reliability during the fuel extrusion process, and can meet the piston structural strength and operation reliability under low pressure difference conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of underwater turbine engines, and in particular to a method for preparing a corrosion-resistant lightweight piston for a fuel tank. Background Art

[0002] The turbine engine has the characteristics of low gas consumption, large enthalpy drop and simple structure, and is one of the main propulsion systems for improving the speed of underwater vehicles. The sealing of static storage fuel and the stability of fuel supply are related to the reliability of the turbine engine; therefore, as an important device for storing and supplying fuel, the fuel supply tank has become an integral part of the underwater turbine engine propulsion system. At present, there is an urgent need to develop compact and space-saving alternative fuel supply devices and technologies.

[0003] Reactive fuel with hydroxylamine perchlorate (HAP) as the oxidant is the main fuel for the tank supply system. It can overcome the shortcomings of traditional fuels such as oxygen deficiency, incomplete combustion, and low energy and specific impulse. It has high energy density and safety in use, and has become an important reactive fuel for future underwater propulsion systems. The corrosion resistance, lightweight and sealing reliability of the fuel supply tank have become the future development direction of the fuel supply device. In view of the physical and chemical properties of the above fuels, the use of metal pistons in the long-term storage of fuel tanks has the following disadvantages: (1) The large mass of the fuel itself causes the deformation of the conduit, which causes a gap between the piston and the tank wall and causes fuel leakage. (2) Reactive fuels are highly corrosive to the metal materials of the tank during static long-term storage. The use of traditional metal storage tanks and pistons will cause problems such as reduced fuel safety. Reinforced polymer materials have light weight, high strength and excellent chemical corrosion resistance. Therefore, the development of corrosion-resistant and high-strength non-metallic pistons is the technical development trend of future fuel tanks.

[0004] US Patent USP5104514 reported a technical method for applying protective materials on the surface of aluminum alloy shells and pistons to the fuel tank of underwater propulsion system. The specific method is as follows: first, the aluminum alloy shell is sandblasted, then immersed in sodium sulfate solution and anodized by applying current to form an anodic oxide film with a thickness of 60 to 70 μm, then immersed in sodium dichromate solution, rinsed and air-dried, and electrostatically sprayed with epoxy resin powder. After curing, an epoxy resin coating of about 120 μm is generated on the surface of the aluminum alloy anodized film. Experiments have shown that the protective coating has good corrosion resistance and wear resistance, and has good bonding strength with the aluminum alloy shell.

[0005] Chinese patent CN112175346A discloses a preparation method of carbon fiber composite material for piston, firstly, the carbon fiber is surface treated, then graphene modified phenolic resin, carbon fiber, hexamethylenetetramine, wollastonite, carbon black, and calcium hydroxide are mixed in a mixer, dried, plasticized in an open mill, the plasticized material is cooled to room temperature, crushed, and then pressed into shape in a hot press, and then placed in an oven for natural cooling. The tensile strength of the composite material for piston formed by this method is 75-85MPa, which cannot meet the structural design requirements of the fuel tank for piston parts. In addition, the compatibility of phenolic resin-based composite materials with HAP three-component fuel is poor, and long-term use will lead to a further reduction in the mechanical strength of the material.

[0006] Chinese patent CN113024993A relates to a polyetheretherketone composite material and its preparation method and application. The specific material is composed of PEEK powder, surface sulfonated PEEK powder, mineral fiber, molybdenum disulfide, and polytetrafluoroethylene powder. It is prepared by cold pressing-sintering-hot pressing. The prepared material has the characteristics of high temperature resistance, wear resistance, low friction resistance, low leakage and long life, and is suitable for use in the field of high-speed reciprocating seals. The composite material involved in this patent still has low mechanical strength, with a tensile strength of 95 to 105 MPa, and shows insufficient strength as a load-bearing structural part.

[0007] Chinese patent CN111440342B designs a CF / PEEK composite material with a strong chemical bond interface and a preparation method thereof. The specific method steps include: (1) high temperature decomposition of the original sizing agent on the surface of CF; (2) simultaneous microwave radiation and ultraviolet light irradiation of CF in a saturated water vapor environment; (3) immersing the irradiated CF in an aminated PEEK / dimethylformamide / carbon nanotube suspension and heating it to allow the aminated PEEK to react with the irradiated CF; (4) laminating and hot pressing the product with the PEEK material to prepare a CF / PEEK composite material with a strong chemical interface, with a bending strength of 900-1100MPa, a bending modulus of 57-65GPa, an interface shear strength of 100-120MPa, and a residual compressive strength after impact of 210-250MPa. Although the laminated composite material involved in this technology has a high interface shear strength, it is a non-homogeneous molding. The piston used in the fuel supply tank is a large-sized thin-walled piston. During operation, the fuel pressure and conveying displacement force applied to the piston are coaxial with the carbon fiber layers. Under high pressure, liquid fuel will penetrate into the interlayer gaps of the carbon fiber fabric, greatly reducing the interfacial shear strength of the composite material. During long-term storage, problems such as interlayer delamination may even occur, seriously affecting the reliability of the fuel tank.

[0008] Chinese patent CN112694712A relates to a lightweight and high-strength piston for a fuel supply tank and its preparation method, the main components of which include: polyetheretherketone, fiber powder, carbon nanoparticles, and active slurry. The piston material is prepared by hot pressing, which not only reduces the dead weight of the fuel supply tank, but also significantly improves the sealing and reliability during the fuel extrusion process. However, the yield rate during the manufacturing process is only 50%, and problems such as product cracking are prone to occur. Summary of the invention

[0009] The technical problem to be solved by the present invention is to provide a method for preparing a corrosion-resistant lightweight piston for a fuel tank which is not prone to cracking and has a high yield.

[0010] In order to solve the above problems, a method for preparing a corrosion-resistant lightweight piston for a fuel tank according to the present invention comprises the following steps:

[0011] (1) Weigh the following components by weight percentage: 40% to 90% of polyetheretherketone (PEEK) powder, 5% to 45% of inorganic short fibers, and 0.1% to 5% of carbon nanoparticles;

[0012] (2) Liquid phase oxidation of fibers: Soak the inorganic short fibers in mixed acid at a temperature of 50-80°C, stir and react for more than 60 minutes, then cool and stand for centrifugation, wash the precipitate with distilled water, adjust the pH to 7, and then dry at 100°C;

[0013] ⑶ Fiber epoxidation: dissolve m-chloroperbenzoic acid (mCPBA) in chloroform solvent to form a chloroform solution with a concentration of 15% to 30%; then immerse the inorganic short fibers that have undergone surface oxidation treatment in the chloroform solution for more than 4 hours, and stir the materials intermittently during this process; after the reaction is completed, let it stand, centrifuge and filter, and dry it;

[0014] (4) Carbon nanoparticle dispersion: adding carbon nanoparticles to a polyethyleneimine (PEI) aqueous solution with a mass concentration of more than 60%, and obtaining a polyethyleneimine aqueous solution containing carbon nanoparticles with a mass concentration of 2-5% by ultrasonic dispersion;

[0015] (5) Mechanical mixing: The short fibers subjected to surface epoxidation treatment are dispersed at high speed in a high-speed stirring disperser, and at the same time, the polyethyleneimine (PEI) solution containing carbon nanoparticles is sprayed into the stirring disperser, and stirring and dispersing is continued until the fiber bundles are completely dispersed, and the material is taken out; the material is dried to obtain a dried material;

[0016] (6) Material kneading: knead the polyetheretherketone (PEEK) powder at 150±10°C using a vacuum kneader until a sticky mass appears on the surface, add the dried material in batches according to proportion, increase the kneading speed to 200~500RPM, turn on the vacuum, increase the temperature to 200℃~240℃, continue mixing for 1 hour, take out the mixed material in a hot state, and crush the mixed material after it is completely cooled to obtain a crushed mixed material;

[0017] (7) Piston hot pressing molding: the crushed mixed material is taken out and hot pressed in a mold, the temperature is lowered after molding, and the pressure is released after the temperature is lower than 150° C., and the mixture is cooled to room temperature in the furnace, and the piston blank is taken out after demolding;

[0018] ⑻Heat treatment of the piston blank;

[0019] ⑼ The piston blank is obtained by machining.

[0020] The weight average molecular weight of the polyetheretherketone (PEEK) powder in step (1) is 65000-80000 g / mol.

[0021] In the step (1), the inorganic short fibers are glass fibers or carbon fibers; the glass fibers are alkali-free fibers, which are short fibers with a length of more than 1 mm, a fiber size of 2000-4000 Denier, a single fiber diameter of 10-15 μm, and an optimal fiber length of 4.5-6.0 mm; the carbon fibers are short fibers with a fiber length of 3.0-6.0 mm and a single fiber diameter of 5-10 μm.

[0022] In step (1), the carbon nanoparticles are graphene or carbon nanotubes; the graphene is mainly industrial-grade graphene oxide, with a sheet thickness of ≤5nm, an oxygen content of 20% to 30%, and a sheet diameter of 5 to 20μm; the carbon nanotubes are multi-walled carbon nanotubes with a tube diameter of 5 to 30nm and a length of 5 to 30μm, and the surface of the carbon nanotubes is carboxylated, wherein the carboxyl content is 2 to 5%.

[0023] The mixed acid in step (2) refers to an acid solution obtained by uniformly mixing nitric acid having a volume concentration of 68% and sulfuric acid having a volume concentration of 70% in a volume ratio of 1:3.

[0024] In the step (4), the molecular weight of the polyethyleneimine is less than 1000 and the viscosity is less than 3000 mPa·s.

[0025] The conditions for hot pressing in step (7) are that the temperature is 380°C to 400°C, the pressing pressure is 5 to 20 MPa, and the holding time is 50 min to 90 min.

[0026] The process of heat treatment in step (8) is as follows:

[0027] ① Dry the piston blank in an oven at 150℃ for more than 3 hours;

[0028] ② Gradually heat the piston blank to 200°C at a heating rate of 10°C / hour;

[0029] ③Keep warm at 200℃ for 6~10 hours;

[0030] ④ Gradually cool the piston blank to 140°C at a cooling rate of 10°C / hour;

[0031] ⑤ Close the oven and cool the piston blank to room temperature in the oven.

[0032] The piston prepared by the method described above has a tensile fracture strength greater than 250 MPa, a tensile modulus greater than 27 GPa, a compressive strength greater than 350 MPa, and an impact strength greater than 9.0 KJ / m 2 .

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] 1. In the present invention, the short fibers are treated by liquid phase oxidation method, especially soaking in a mixed acid with a volume ratio of HNO3:H2SO4=1:3, which has a significant chemical etching effect on the fiber surface, can obtain the best fiber surface activity, and the surface contains abundant oxygen-containing functional groups such as carboxyl, hydroxyl and carbonyl, which can improve the bonding strength between the short fibers and the PEEK resin matrix. At the same time, since the stirring reaction time has a significant effect on the content of the fiber surface active groups, the surface activity of the fiber cannot be stimulated in a short time, and too long stirring time will cause transitional etching or even cracking of the fiber surface, so the stirring time is limited to 60~90 minutes, and a large number of oxygen-containing groups are obtained.

[0035] 2. In the present invention, the fiber surface is subjected to epoxidation treatment. The chloroform solution containing mCPBA can make the fiber surface contain abundant epoxy groups. The epoxy group content on the fiber surface can be increased by appropriately increasing the concentration of mCPBA and the fiber soaking time. The increase in the epoxy group content can greatly improve the interfacial bonding strength between the fiber and the carbon nanoparticles and the PEEK resin matrix, and can also greatly improve the corrosion resistance of the piston material in HAP fuel. This treatment method is simple and easy to implement, and has significant effects.

[0036] 3. In the present invention, the short fibers and carbon nanoparticles are mechanically mixed. In this process, the carbon nanoparticles need to be uniformly dispersed in the PEI solution, wherein the PEI molecular weight involved is required to be less than 1000 and the viscosity is less than 3000 mPa·s; a smaller molecular weight has a higher molecular chain activity, which can promote the chemical cross-linking of the amino groups in polyethyleneimine with the epoxy groups and hydroxyl groups on the surface of the short fibers, thereby improving the chemical adhesion of the carbon nanoparticles on the surface of the short fibers. In addition, the chemical adhesion of the PEI solution can further improve the enrichment of carbon nanoparticles on the surface of the fiber filaments, forming an effective chemical bond, which has a better interface bonding strength than the mechanical pinning effect. In addition, the PEI sprayed on the fiber surface can form a layer of PEI film after removing water. The formation of the PEI film greatly improves the interface compatibility of the short fibers, carbon nanoparticles and the PEEK resin matrix, which is an important basis for improving the mechanical strength of the piston material.

[0037] 4. In the present invention, the double rotor vacuum kneading of PEEK, short fibers and carbon nanoparticles is used. Under the shearing action of the double rotor, the short fibers, carbon nanoparticles and PEEK resin can be fully dispersed and mixed, and the optimal kneading temperature is 200°C to 240°C. PEEK resin undergoes plastic flow under mechanical shearing, and the viscosity change of the polymer itself causes the surface of the short fibers and carbon nanoparticles with active functional groups to be fully infiltrated in the resin matrix, thereby promoting the grafting and cross-linking reaction between the active functional groups such as epoxy groups and carboxyl groups and the PEEK molecular chains, thereby improving the dispersibility of the fibers and carbon nanoparticles in the resin. In addition, the shearing action of the double rotor will not cause the short fibers to break, but will further axially disperse the fiber bundles, so that the dispersion uniformity is greatly improved.

[0038] 5. The hot pressing molding method is adopted in the present invention, and the molding temperature control and pressing pressure are crucial to improving the mechanical properties of the piston. The optimal pressing process parameters involved in the present invention are: temperature of 380°C~400°C, and pressing pressure of 5~20MPa. In this process, PEEK will flow at a temperature above the melting point, and the PEI film formed on the fiber surface can undergo a cross-linking reaction with the molecular chain of PEEK, further improving the interfacial binding energy between PEEK and the fiber, thereby greatly improving the mechanical strength of the piston material. If the hot pressing temperature is low, the insufficient fluidity of PEEK will cause defects or gaps.

[0039] 6. The present invention adopts the heat treatment technology of the piston blank to eliminate the internal stress of the PEEK composite material, avoid the stress concentration of the short fiber in the PEEK, and effectively improve the toughness and impact resistance of the piston material; at the same time, it can also effectively prevent the cracking of the pressed piston product, thereby ensuring the quality of the piston product and the dimensional stability of the thin-walled parts during machining.

[0040] 7. The present invention makes full use of the synergistic effect of inorganic short fibers and carbon nanoparticles. At the same time, the introduction of surface active functional groups can have good interface compatibility with PEEK. The surface-treated inorganic short fibers have a rough microscopic surface, and carbon nanoparticles with chemical bonding can be attached to the fiber surface, which greatly improves the physical and mechanical properties of the PEEK composite material.

[0041] 8. The tensile fracture strength of the piston for the fuel supply tank obtained by the present invention is greater than 250MPa, the tensile modulus is greater than 27GPa, the compressive strength is greater than 350MPa, and the impact strength is greater than 9.0KJ / m 2 Compared with the preparation method involved in Chinese patent CN112694712A, the mechanical performance indexes of the piston material are more than 10%, and the specific strength can reach the same level as 7A04 aluminum alloy. The density is much lower than that of traditional metal pistons, which greatly reduces the deadweight of the fuel supply tank and avoids the problem of stuck due to the deadweight of the piston during operation. Compared with the preparation method involved in Chinese patent CN112694712A, the finished product rate of the piston for the fuel supply tank obtained by the present invention can be increased by more than 30%, the surface of the product is smooth and crack-free, and after ultrasonic non-destructive testing, the proportion of voids and defects inside the piston is less than 1%.

[0042] 9. The lightweight piston for the fuel tank obtained by the present invention has good machining properties, and can be processed into a high-precision thin-walled piston with a complex structure. After the static sealing test, the piston has good static pressure sealing performance, the damping value is less than 1600N, and can meet the piston structural strength and operation reliability in the low pressure difference range of 0.1MPa~2.3MPa, and there is no sticking phenomenon during the operation process.

[0043] 10. After soaking the lightweight piston for fuel supply tank obtained by the present invention in HAP for one year, there is no obvious dimensional expansion phenomenon, and the decrease of its tensile strength after soaking in hydroxylamine perchlorate (HAP) three-component fuel is less than 5%. Compared with the preparation method involved in Chinese patent CN112694712A, it has more excellent corrosion resistance, is particularly suitable for hydroxylamine perchlorate and its mixed fuel, and can meet the technical requirements of static storage of fuel tanks. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0045] Figure 1 A flow chart was prepared for the present invention.

[0046] Figure 2 It is a three-dimensional view of the lightweight piston blank of the present invention.

[0047] Figure 3It is a schematic diagram of the structure of the lightweight piston blank of the present invention.

[0048] Figure 4 It is the AA cross-sectional view of the present invention.

[0049] Figure 5 It is a schematic diagram of a lightweight piston according to the present invention.

[0050] Figure 6 It is the BB cross-sectional view of the present invention.

[0051] Figure 7 It is the volume change rate of the lightweight piston of the present invention when immersed in HAP fuel.

[0052] Figure 8 It is the pressure change stored by the lightweight piston of the present invention through a static low pressure difference. DETAILED DESCRIPTION

[0053] like Figure 1 As shown, a method for preparing a corrosion-resistant lightweight piston for a fuel tank comprises the following steps:

[0054] (1) Weigh the following components by weight percentage: 40% to 90% of polyetheretherketone (PEEK) powder, 5% to 45% of inorganic short fibers, and 0.1% to 5% of carbon nanoparticles.

[0055] Among them: the weight average molecular weight of polyetheretherketone (PEEK) powder is 65000~80000g / mol. The molecular weight of the resin matrix will affect the physical and mechanical properties and molding process of the piston. A lower molecular weight will make the molecular chain entanglement ability weaker and the mechanical strength of the piston will be reduced; too high a molecular weight will lead to too high a molding temperature and reduced fluidity after the resin is melted.

[0056] Inorganic short fibers are glass fibers or carbon fibers. Glass fibers are alkali-free fibers with a length of more than 1 mm, a fiber size of 2000-4000 Denier, a single fiber diameter of 10-15 μm, and an optimal fiber length of 4.5-6.0 mm; carbon fibers are short fibers with a fiber length of 3.0-6.0 mm and a single fiber diameter of 5-10 μm. Inorganic short fibers need to be subjected to surface liquid phase oxidation and epoxidation treatment to increase surface activity and have a good chemical interface bond with the polyetheretherketone resin matrix.

[0057] The carbon nanoparticles are graphene or carbon nanotubes. Graphene is mainly industrial-grade graphene oxide, with a sheet thickness of ≤5nm, an oxygen content of 20%~30%, and a sheet diameter of 5~20μm; the use of industrial-grade graphene oxide can reduce the cost of polymer composite materials. The carbon nanotubes are multi-walled carbon nanotubes, with a tube diameter of 5~30nm and a length of 5~30μm. The surface of the carbon nanotubes is carboxylated, and the carboxyl content is 2~5%. The surface carboxylation of carbon nanotubes can significantly increase the surface activity of carbon nanoparticles, thereby greatly improving the interface bonding strength between carbon nanotubes and PEEK resin matrix, and between carbon nanotubes and fibers. After surface treatment, carbon nanoparticles can be effectively loaded on the fiber surface, or grafted on the PEEK molecular chain, which can play a good toughening role on polymer composite materials.

[0058] ⑵Fiber liquid phase oxidation: Soak the inorganic short fibers in a mixed acid, which refers to an acid solution obtained by mixing nitric acid with a volume concentration of 68% and sulfuric acid with a volume concentration of 70% in a volume ratio of 1:3. Control the soaking temperature to 50-80°C, stir the reaction for more than 60 minutes, then cool and stand it for centrifugation, wash the precipitate with distilled water, adjust it to pH 7, and then dry it at 100°C.

[0059] ⑶ Fiber epoxidation: dissolve meta-chloroperbenzoic acid (mCPBA) in chloroform solvent to form a chloroform solution with a concentration of 15%~30%; then immerse the inorganic short fibers that have been surface-oxidized in the chloroform solution for more than 4 hours, and stir the materials intermittently during this process; after the reaction is completed, let it stand, centrifuge and dry it.

[0060] (4) Carbon nanoparticle dispersion: Add carbon nanoparticles to a polyethyleneimine (PEI) aqueous solution with a mass concentration of more than 60%, and obtain a polyethyleneimine aqueous solution containing carbon nanoparticles with a mass concentration of 2-5% by ultrasonic dispersion. The molecular weight of polyethyleneimine is less than 1000 and the viscosity is less than 3000 mPa·s.

[0061] ⑸ Mechanical mixing: The short fibers with surface epoxidation treatment are dispersed at high speed in a high-speed stirring disperser, and at the same time, the polyethyleneimine (PEI) solution containing carbon nanoparticles is sprayed into the stirring disperser, and the stirring and dispersion is continued until the fiber bundles are completely dispersed, and the material is taken out; the material is dried to remove moisture to obtain a dried material.

[0062] (6) Material kneading: Use a twin-rotor vacuum kneader at 150±10℃ to knead the polyetheretherketone (PEEK) powder until a sticky mass appears on the surface, then add the dried material in batches according to proportion, increase the kneading speed to 200~500RPM, turn on the vacuum, raise the temperature to 200℃~240℃, continue mixing for 1 hour, take out the mixed material in a hot state, and crush the mixed material after it is completely cooled to obtain a crushed mixed material.

[0063] ⑺ Piston hot pressing molding: After the crushed mixed material is taken out, it is hot pressed in the mold. The conditions for hot pressing molding are that the temperature is 380℃~400℃ and the pressing pressure is 5~20MPa. During the initial pressing process, multiple pressurization and pressure relief are performed to ensure the density of the product. The pressure holding time is 50min~90min. After molding, the temperature is lowered. When the temperature is lower than 150℃, the pressure is relieved, and the piston blank is cooled to room temperature with the furnace. After demolding, the piston blank is taken out.

[0064] ⑻ Heat treatment of the piston blank can eliminate the internal stress of the PEEK composite material and avoid the stress concentration of short fibers in PEEK. The heat treatment process is as follows:

[0065] ① Dry the piston blank in an oven at 150℃ for more than 3 hours;

[0066] ② Gradually heat the piston blank to 200°C at a heating rate of 10°C / hour;

[0067] ③Keep warm at 200℃ for 6~10 hours;

[0068] ④ Gradually cool the piston blank to 140°C at a cooling rate of 10°C / hour;

[0069] ⑤ Close the oven and cool the piston blank to room temperature in the oven.

[0070] ⑼Machining the piston blank:

[0071] According to the drawing requirements, the piston blank is precision machined to ensure the piston outer diameter size and tolerance requirements, inner diameter tolerance requirements, and meet the corresponding groove size processing requirements.

[0072] The piston obtained is Figures 2 to 6 As shown, its tensile strength is greater than 250MPa, tensile modulus is greater than 27GPa, compressive strength is greater than 350MPa, and impact strength is greater than 9.0KJ / m 2 .

[0073] Example 1 A method for preparing a corrosion-resistant lightweight piston for a fuel tank comprises the following steps:

[0074] ⑴ Weigh the following components: polyetheretherketone (PEEK) powder 64%, glass fiber 33%, graphene 3%.

[0075] (2) Liquid phase oxidation of fiber: Soak the glass fiber in 1000ml of a mixture of nitric acid and sulfuric acid, control the temperature at 60°C, stir for 60 minutes, cool and let stand, then centrifuge, wash the precipitate with distilled water, adjust the pH to 7, and then dry at 100°C.

[0076] ⑶ Fiber epoxidation: dissolve 350g of m-chloroperbenzoic acid (mCPBA) in 2000ml of chloroform solvent; then soak 1320g of surface-oxidized glass fiber in the chloroform solution for more than 4 hours, during which the material is intermittently stirred; after the reaction is completed, let it stand, centrifuge and dry.

[0077] (4) Dispersion of carbon nanoparticles: 120 g of graphene was added to 2400 ml of a 60% polyethyleneimine aqueous solution, and then ultrasonically dispersed for 1 hour to obtain a polyethyleneimine (PEI) solution containing graphene.

[0078] ⑸ Mechanical mixing: The glass fiber with surface epoxidation treatment is dispersed at high speed in a high-speed stirring disperser, and the polyethyleneimine (PEI) solution containing graphene is sprayed into the stirring disperser. The stirring and dispersion is continued until the fiber bundles are completely dispersed, and the material is taken out; the material is dried to remove moisture to obtain a dried material.

[0079] (6) Material kneading: Use a twin-rotor vacuum kneader at 150°C to knead 2560g of polyetheretherketone (PEEK) powder until a sticky mass appears on the surface, then add the dried material in three batches, increase the kneading speed, turn on the vacuum, raise the temperature to 240°C, continue mixing for 1 hour, take out the mixed material in a hot state, and crush it after the mixed material is completely cooled to obtain a crushed mixed material.

[0080] ⑺ Piston hot pressing molding: After the crushed mixed material is taken out, it is hot pressed in the mold at a temperature of 380°C and a pressing pressure of 15±2MPa. The pressure is maintained for 60 minutes and then the temperature is lowered. When the temperature is lower than 150°C, the pressure is released and the mixture is cooled to room temperature in the furnace. After demolding, the piston blank is taken out.

[0081] ⑻ Heat treatment of the piston blank is carried out as follows:

[0082] ① Dry the piston blank in an oven at 150℃ for 3 hours;

[0083] ② Gradually heat the piston blank to 200°C at a heating rate of 10°C / hour;

[0084] ③Keep warm at 200℃ for 8 hours;

[0085] ④ Gradually cool the piston blank to 140°C at a cooling rate of 10°C / hour;

[0086] ⑤ Close the oven and cool the piston blank to room temperature in the oven.

[0087] ⑼ The piston blank is obtained by machining.

[0088] Example 2 A method for preparing a corrosion-resistant lightweight piston for a fuel tank comprises the following steps:

[0089] ⑴ Weigh the following components: polyetheretherketone (PEEK) powder 50%, carbon fiber 45%, carbon nanotube 5%.

[0090] (2) Liquid phase oxidation of fiber: Soak the glass fiber in 1500 ml of a mixture of nitric acid and sulfuric acid, control the temperature at 60°C, stir for 60 minutes, cool and let stand, then centrifuge, wash the precipitate with distilled water, adjust the pH to 7, and then dry at 100°C.

[0091] ⑶ Fiber epoxidation: dissolve 350g of m-chloroperbenzoic acid (mCPBA) in 2800ml 2000ml chloroform solvent; then soak 1800g of surface-oxidized carbon fiber in chloroform solution for more than 4 hours, stirring the material intermittently during the process; after the reaction is completed, let it stand, centrifuge and dry it.

[0092] (4) Dispersion of carbon nanoparticles: 200 g of carbon nanotubes were added to 2400 ml of a 60% polyethyleneimine aqueous solution, and then ultrasonically dispersed for 1 hour to obtain a polyethyleneimine (PEI) solution containing carbon nanotubes.

[0093] ⑸ Mechanical mixing: The carbon fiber with surface epoxidation treatment is dispersed at high speed in a high-speed stirring disperser, and at the same time, the polyethyleneimine (PEI) solution containing carbon nanotubes is sprayed into the stirring disperser, and stirring and dispersing is continued until the fiber bundles are completely dispersed, and the material is taken out; the material is dried to remove moisture to obtain a dried material.

[0094] (6) Material kneading: Use a twin-rotor vacuum kneader at 150°C to knead 2000g of polyetheretherketone (PEEK) powder until a sticky mass appears on the surface, then add the dried material in three batches, increase the kneading speed, turn on the vacuum, raise the temperature to 240°C, continue mixing for 1 hour, take out the mixed material in a hot state, and crush the mixed material after it is completely cooled to obtain a crushed mixed material.

[0095] ⑺The piston hot pressing molding is the same as in Example 1.

[0096] ⑻ Heat treat the piston blank in the same process as in Example 1.

[0097] ⑼ The piston blank is obtained by machining.

[0098] Example 3 A method for preparing a corrosion-resistant lightweight piston for a fuel tank comprises the following steps:

[0099] ⑴ Weigh the following components: polyetheretherketone (PEEK) powder 84.8%, carbon fiber 15%, and graphene 0.2%.

[0100] (2) Liquid phase oxidation of fibers: Soak the carbon fibers in 1500 ml of a mixture of nitric acid and sulfuric acid, control the temperature at 60°C, stir for 60 minutes, cool and let stand, then centrifuge, wash the precipitate with distilled water, adjust the pH to 7, and then dry at 100°C.

[0101] ⑶ Fiber epoxidation: Dissolve 120g of meta-chloroperbenzoic acid (mCPBA) in 1000ml of chloroform solvent; then soak 600g of surface-oxidized carbon fiber in the chloroform solution for more than 4 hours, stirring the material intermittently during the process; after the reaction is completed, let it stand, centrifuge and dry it.

[0102] (4) Dispersion of carbon nanoparticles: 80 g of graphene was added to 200 ml of a 60% polyethyleneimine aqueous solution, and then ultrasonically dispersed for 1 hour to obtain a polyethyleneimine (PEI) solution containing carbon nanoparticles.

[0103] ⑸ Mechanical mixing: The carbon fiber with surface epoxidation treatment is dispersed at high speed in a high-speed stirring disperser, and at the same time, the polyethyleneimine (PEI) solution containing graphene is sprayed into the stirring disperser, and stirring and dispersing is continued until the fiber bundles are completely dispersed, and the material is taken out; the material is dried to remove moisture to obtain a dried material.

[0104] (6) Material kneading: Use a twin-rotor vacuum kneader at 150°C to knead 3392g of polyetheretherketone (PEEK) powder until a sticky mass appears on the surface, then add the dried material in three batches, increase the kneading speed, turn on the vacuum, raise the temperature to 240°C, continue mixing for 1 hour, take out the mixed material in a hot state, and crush it after the mixed material is completely cooled to obtain a crushed mixed material.

[0105] ⑺The piston hot pressing molding is the same as in Example 1.

[0106] ⑻ Heat treat the piston blank in the same process as in Example 1.

[0107] ⑼ The piston blank is obtained by machining.

[0108] The pistons obtained in Examples 1 to 3 were immersed in HAP fuel for 198 days. Figure 7As shown in the figure, the horizontal axis is the immersion time and the vertical axis is the volume change rate of the piston material.

[0109] During the initial soaking stage (until the 7th day), the piston material initially had slight liquid adsorption on its surface, causing the volume change rate to begin to increase. As time went on, the micro-swelling of the piston material became saturated, causing the volume change rate to gradually decrease. After 198 days of soaking, the volume change rate of the piston material obtained in Example 1 was 0.4%, the volume change rate of the piston material obtained in Example 2 was less than 0.1%, and the volume change rate of the piston material obtained in Example 3 was 0.55%.

[0110] The pistons obtained in Examples 1 to 3 were subjected to static sealing tests. Experimental conditions: room temperature, HAP fuel on the left side of the piston, and compressed air on the right side of the piston. The pressure difference and damping force on both sides of the piston change with the pressure level of the compressed air, showing a trend of increasing first and then stabilizing. The results are shown in Figure 8 As shown in the figure, it can be seen that between the pressure levels of 5 bar and 14 bar, as the compressed air pressure level increases, the pressure difference and damping force on both sides of the piston show a positive proportional increasing trend; between the pressure levels of 14 bar and 23 bar, as the compressed air pressure level increases, the pressure difference and damping force on both sides of the piston remain basically stable and no longer increase with the increase of the pressure level. At different pressure levels, the piston shows good low damping characteristics and sealing characteristics.

Claims

1. A method for preparing a corrosion-resistant lightweight piston for a fuel tank, comprising the following steps: (1) Weigh the following components by weight percentage: 40% to 90% of polyetheretherketone powder, 5% to 45% of inorganic short fibers and 0.1% to 5% of carbon nanoparticles; the inorganic short fibers are glass fibers or carbon fibers; the glass fibers are alkali-free fibers, which are short fibers with a length of more than 1 mm, a fiber size of 2000 to 4000 Denier, and a single fiber diameter of 10 to 15 μm; the carbon fibers are short fibers with a fiber length of 3.0 to 6.0 mm and a single fiber diameter of 5 to 10 μm; (2) Liquid phase oxidation of fibers: the inorganic short fibers are immersed in a mixed acid at a temperature of 50-80°C, stirred for reaction for more than 60 minutes, then cooled and allowed to stand for centrifugation, the precipitate is washed with distilled water, adjusted to a pH of 7, and then dried at 100°C; the mixed acid refers to an acid solution obtained by uniformly mixing nitric acid with a volume concentration of 68% and sulfuric acid with a volume concentration of 70% in a volume ratio of 1:3; ⑶ Fiber epoxidation: dissolve m-chloroperbenzoic acid in chloroform solvent to form a chloroform solution with a concentration of 15% to 30%; then immerse the inorganic short fibers that have undergone surface oxidation treatment in the chloroform solution for more than 4 hours, and stir the materials intermittently during this process; after the reaction is completed, let it stand, centrifuge and filter, and dry it; (4) Carbon nanoparticle dispersion: adding carbon nanoparticles to a polyethyleneimine (PEI) aqueous solution having a mass concentration of more than 60%, and obtaining a polyethyleneimine aqueous solution containing carbon nanoparticles having a mass concentration of 2-5% by ultrasonic dispersion; the polyethyleneimine having a molecular weight of less than 1000 and a viscosity of less than 3000 mPa·s; (5) Mechanical mixing: The short fibers subjected to surface epoxidation treatment are dispersed at high speed in a high-speed stirring and dispersing machine, and at the same time, the polyethyleneimine aqueous solution containing carbon nanoparticles is sprayed into the stirring and dispersing machine, and stirring and dispersing is continued until the fiber bundles are completely dispersed, and the material is taken out; the material is dried to obtain a dried material; (6) Material kneading: knead the polyetheretherketone powder at 150±10°C using a vacuum kneader until a sticky mass appears on the surface, add the dried material in batches according to proportion, increase the kneading speed to 200~500RPM, turn on the vacuum, increase the temperature to 200℃~240℃, continue mixing for 1 hour, take out the mixed material in a hot state, and crush the mixed material after it is completely cooled to obtain a crushed mixed material; (7) Piston hot pressing molding: the crushed mixed material is taken out and hot pressed in a mold, the temperature is lowered after molding, and the pressure is released after the temperature is lower than 150° C., and the mixture is cooled to room temperature in the furnace, and the piston blank is taken out after demolding; ⑻Heat treatment of the piston blank; ⑼ The piston blank is machined; the obtained piston has a tensile fracture strength greater than 250MPa, a tensile modulus greater than 27GPa, a compressive strength greater than 350MPa, and an impact strength greater than 9.0KJ / m 2 .

2. The method for preparing a corrosion-resistant lightweight piston for a fuel tank according to claim 1, characterized in that: The weight average molecular weight of the polyetheretherketone powder in step (1) is 65000~80000g / mol.

3. The method for preparing a corrosion-resistant lightweight piston for a fuel tank according to claim 1, characterized in that: In step (1), the carbon nanoparticles are graphene or carbon nanotubes; the graphene is mainly industrial-grade graphene oxide, with a sheet thickness of ≤5nm, an oxygen content of 20% to 30%, and a sheet diameter of 5 to 20μm; the carbon nanotubes are multi-walled carbon nanotubes with a tube diameter of 5 to 30nm and a length of 5 to 30μm, and the surface of the carbon nanotubes is carboxylated, wherein the carboxyl content is 2 to 5%.

4. The method for preparing a corrosion-resistant lightweight piston for a fuel tank according to claim 1, characterized in that: The conditions for hot pressing in step (7) are that the temperature is 380°C to 400°C, the pressing pressure is 5 to 20 MPa, and the holding time is 50 min to 90 min.

5. The method for preparing a corrosion-resistant lightweight piston for a fuel tank according to claim 1, characterized in that: The process of heat treatment in step (8) is as follows: ① Dry the piston blank in an oven at 150℃ for more than 3 hours; ② Gradually heat the piston blank to 200°C at a heating rate of 10°C / hour; ③Keep warm at 200℃ for 6~10 hours; ④ Gradually cool the piston blank to 140°C at a cooling rate of 10°C / hour; ⑤ Close the oven and cool the piston blank to room temperature in the oven.

Citation Information

Patent Citations

  • CF / PEEK composite materials with strong chemical bond interfaces and their preparation methods

    CN111440342B

  • Preparation method of carbon fiber composite material for piston

    CN112175346A

  • Polyether-ether-ketone composite material as well as preparation method and application thereof

    CN113024993A

  • Continuous carbon fiber surface modification method

    CN104018340A

  • Lightweight high-strength piston for fuel supply cabin and preparation method thereof

    CN112694712A