Inorganic composite polyphenyl A-grade insulation board and production method thereof

A technology of composite polyphenylene and production methods, applied in thermal insulation, chemical instruments and methods, ceramic molding machines, etc., can solve problems such as difficult completion of thermal insulation boards, falling off of thermal insulation layers, and insufficient ash-sticking ability, so as to eliminate fire hazards and keep thermal insulation The effect is improved and the heat preservation effect is good

CN114856010APending Publication Date: 2022-08-05山东刚磊建材科技有限公司
0 Cites 1 Cited by

Patent Information

Authority / Receiving Office
CN · China
Current Assignee / Owner
Publication Date
2022-08-05

Smart Images

  • Figure 1
    Figure 1
Patent Text Reader

Abstract

The invention relates to the technical field of insulation board production, in particular to an inorganic composite polyphenyl A-grade insulation board and a production method thereof. Which comprises an insulation board body, and is characterized in that the insulation board body comprises 7kg / m < 3 > seven mature polystyrene board blank; the polystyrene board blank is internally provided with a net-shaped supporting framework structure which is formed by uniformly permeating cement-based inorganic slurry into the polystyrene board blank through high-pressure adsorption and curing, and the net-shaped supporting framework structure wraps polystyrene board blank particles. The inorganic composite polyphenyl A-grade insulation board produced by adopting the formula and the production method has the following remarkable characteristics of excellent fireproof performance, good insulation effect, better waterproofness, strong adhesive property, high tensile and compressive strength, stable performance, long service life, mature and stable system, cost saving and good flatness.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to the technical field of thermal insulation board production, in particular to an inorganic composite polyphenylene A-level thermal insulation board and a production method thereof. Background technique

[0002] Inorganic composite polystyrene grade A insulation board industry standard "JG / T536-2017", the main index requirements for inorganic composite polystyrene grade A insulation board: ①The combustion performance grade is A2 grade calorific value≦3MJ; ②The thermal conductivity is divided into 050 Class (≦0.050W / (m*k)) and Class 060 (>0.050W / (m*k) and ≦0.060W / (m*k)); ③Tensile strength perpendicular to the board direction: Class 050 ≧0.10MPa, 060 grade is ≧0.12; ④Compressive strength: 050 grade is ≧0.15MPa, 060 grade is ≧0.2MPa; ⑤Volume water absorption ≦10%.

[0003] In recent years, fires of external thermal insulation materials have occurred successively in Nanjing Central International Plaza, Harbin Jingwei 360 Degree G...

Examples

Embodiment 1

[0046] The production method of the inorganic composite polyphenylene grade A thermal insulation board described in this embodiment includes the following steps:

[0047] 1. Put the water and modifier into the mixing tank according to the proportion and stir for 10 minutes, then put the fireproof material 15#P.O425 cement into the mixing tank and stir for 5-10 minutes according to the proportion to obtain the cement-based inorganic slurry material;

[0048] The modifier adopts the following raw material formula: in parts by weight, it contains 100kg of 0# internal waterproofing agent, 64kg of 8# skeleton proppant, 140kg of 14# linking agent, 4kg of 16# suspension modifier, and 19# high-end reducing thermal conductivity. Coefficient material 1640kg, 20# reinforced internal health agent 50kg, 22# early strength stabilizer 2kg; the added amounts of the water, modifier and 15#P.O425 cement are respectively in weight fractions: water 470kg, modifier 200kg, 15#P.O425 cement 700kg. ...

Embodiment 2

[0057] The production method of the inorganic composite polyphenylene grade A thermal insulation board described in this embodiment includes the following steps:

[0058] 1. Put the water and modifier into the mixing tank according to the proportion and stir for 10 minutes, then put the fireproof material 15#P.O425 cement into the mixing tank and stir for 5-10 minutes according to the proportion to obtain the cement-based inorganic slurry material;

[0059] The modifier adopts the following raw material formula: in parts by weight, it contains 64kg of 8# skeleton proppant, 140kg of 14# linking agent, 4kg of 16# suspension modifier, 1740kg of 19# high-end thermal conductivity reducing material, 20# reinforcement Internal health agent 50kg, 22# early-strength stabilizer 2kg; the addition amounts of the water, modifier and 15#P.O425 cement in terms of weight fractions are: water 490kg, modifier 200kg, 15#P.O425 Cement 750kg.

[0060] 2. Make the width and thickness conform to t...

Embodiment 3

[0068] 1. Put the water and modifier into the mixing tank according to the proportion and stir for 10 minutes, then put the fireproof material 15#P.O425 cement into the mixing tank and stir for 5-10 minutes according to the proportion to obtain the cement-based inorganic slurry material;

[0069] The modifier adopts the following raw material formula: in parts by weight, it contains 65kg of 8# skeleton proppant, 130kg of 14# linking agent, 4kg of 16# suspension modifier, 7# low-end thermal conductivity reducing material 750kg, 20# Enhanced internal health agent 50kg, 22# early strength stabilizer 1kg; the addition amounts of the water, modifier and 15#P.O425 cement in terms of weight fractions are: water 410kg, modifier 100kg, 15#P. O425 cement 800kg.

[0070] 2. Make the width and thickness conform to the product specification (1200×600mm) of 7kg / m 3 The seven mature polystyrene sheet blanks are input into the high-pressure adsorption line, and the inorganic composite polys...