A method for magnetron sputtering assisted copper deposition
The magnetron sputtering-assisted copper deposition method solves the problem of no copper in the hole and missing plating caused by chemical copper deposition, achieves an increase in the thickness of the copper layer and improves the quality, ensuring the smooth progress of the electroplating process and simple operation. Copper plating works well.
Patent Information
- Application Number
- CN202210719474.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-23
AI Technical Summary
The existing electroless copper deposition technology is difficult to avoid the problems of no copper in the holes and missing plating, especially on IC carrier boards, which leads to insufficient copper layer thickness and large hole pattern differences.
The magnetron sputtering-assisted copper deposition method is used, including drilling, ultrasonic cleaning, dry ice cleaning, nitrogen oxygenation and magnetron sputtering coating steps to increase the thickness of the copper layer and prevent oxidation, ensuring that the copper seeds are not easily oxidized.
It effectively avoids the problem of no copper in the hole and missing plating, improves the thickness and quality of the copper layer, ensures the smooth progress of the electroplating process, and is simple to operate and has good copper plating effect.
Abstract
Description
Technical Field
[0001] The invention relates to the field of circuit boards, and in particular to a method for magnetron sputtering assisted copper deposition. Background Art
[0002] Chemical copper deposition is required before electroplating. However, chemical copper deposition can only obtain a copper layer thickness of about 0.5 microns. In this case, once sulfuric acid residues in the hole due to improper treatment, it is very likely to cause the problem of no copper in the hole. This problem is particularly prominent in IC substrates.
[0003] The conventional production process of PCB includes cutting, lamination, drilling, copper plating, board electricity, pattern making, etching and post-processing. The seed copper layer formed by chemical copper plating is relatively thin and easily oxidized and corroded, which can easily cause the problem of no copper in the hole. If drilling causes a lot of burrs in the hole, even if it is removed by potassium permanganate, it will cause a poor hole shape and copper plating will leak. Summary of the invention
[0004] In order to solve the problem of no copper in the hole and missed plating after copper deposition, the present invention provides a method for copper deposition assisted by magnetron sputtering.
[0005] A method for magnetron sputtering assisted copper deposition comprises the following steps in sequence:
[0006] Drilling and copper deposition: Drill holes and deposit copper on the substrate in sequence;
[0007] Ultrasonic cleaning: Ultrasonic cleaning removes copper particles that are not stably adsorbed on the substrate surface and in the holes;
[0008] Dry ice cleaning: Dry ice particles are sprayed on the substrate surface to remove residual chemicals and oxides on the substrate surface;
[0009] Nitrogen flushing: Nitrogen is sprayed on the surface of the substrate to expel the oxygen in the holes;
[0010] Magnetron sputtering coating: Use magnetron sputtering coating machine to plate copper film. Increase the thickness of copper on the board surface and holes, avoid the problem of no copper in the hole and missed plating. The copper plating effect is good and easy to operate.
[0011] Optionally, during dry ice cleaning and nitrogen flushing, the spray direction is perpendicular to the substrate to ensure the cleaning effect.
[0012] Optionally, the ultrasonic cleaning adopts a frequency of 12 to 16 kHz, a time of 5 to 8 minutes, and a temperature of 40 to 60°C.
[0013] Optionally, the ultrasonic cleaning is performed with pure water to remove copper particles that are not stably adsorbed, so as to improve the effect of subsequent copper plating.
[0014] Optionally, the dry ice cleaning has a spray pressure of 1.0 to 2.0 kg / cm 2 . Removes oxides and residual chemicals.
[0015] Optionally, in the dry ice cleaning, the dry ice particles are transported from the dry ice storage box through a negative pressure machine and then to the spray tank by a conduit. A plurality of rows of small holes are vertically arranged on both sides of the spray tank, and the dry ice particles are sprayed onto the substrate through the small holes to remove oxides and residual chemicals.
[0016] Optionally, the nitrogen gas flushing oxygen has a spray pressure of 1.8 to 2.5 kg / cm 2 . Expel oxygen from the hole to prevent oxidation of the copper surface.
[0017] Optionally, in the nitrogen oxygen flushing, nitrogen is vertically sprayed to the substrate from above and below the substrate at the same time under negative pressure, and the sprayed nitrogen is recovered to the negative pressure box through a conduit. The nitrogen oxygen flushing effect is good.
[0018] Optionally, the magnetron sputtering coating has an acceleration voltage of 250-900 V, a magnetic field of 60-200 G, a pressure of 1-10 mTorr, and a current density of 15-60 mA / cm 2 , power density is 2~60W / cm 2 . The copper plating film has good effect.
[0019] Optionally, the magnetron sputtering coating has a deposition rate ranging from 150 nm / min to 500 nm / min. The copper coating has a good effect.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention provides a method for copper deposition assisted by magnetron sputtering, which performs film coating by magnetron sputtering to increase the thickness of copper and can avoid the problems of no copper in the hole and missed plating; nitrogen flushing discharges oxygen in the hole to prevent oxidation of the copper surface, so as to ensure that the newly applied copper seeds are not easily oxidized during magnetron sputtering copper plating; the method is easy to operate and has a good copper plating effect. DETAILED DESCRIPTION
[0021] In order to explain the technical solution of the present invention in detail, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Embodiment 1:
[0023] A method for magnetron sputtering assisted copper deposition comprises the following steps in sequence:
[0024] Drilling and copper deposition: The substrate is processed with drilling and copper deposition in sequence.
[0025] Ultrasonic cleaning: Ultrasonic cleaning removes copper particles that are not stably adsorbed on the substrate surface and in the holes; the ultrasonic cleaning adopts a frequency of 12kHz, a time of 5 minutes, and a temperature of 40°C. This embodiment uses pure water for washing. Too high a frequency will damage the copper layer formed by copper deposition.
[0026] Dry ice cleaning: Dry ice particles are sprayed on the substrate surface to remove residual chemicals and oxides on the substrate surface. The spray direction is perpendicular to the substrate.
[0027] The dry ice cleaning spray pressure is 1.0kg / cm 2 . Dry ice cleaning, dry ice particles pass through the negative pressure machine from the dry ice storage box, and then are transmitted to the spray tank by the conduit. Several rows of small holes are vertically set on both sides of the spray tank, and the dry ice particles are sprayed onto the substrate through the small holes. The diameter of the small hole is 0.5mm, and the spraying method is to spray vertically from both sides to the two surfaces of the substrate. Dry ice cleaning can slightly remove oxides without causing copper to be absent in the holes, and remove chemical residues on the surface of the substrate under pressure.
[0028] Nitrogen flushing: Nitrogen is sprayed on the substrate surface to expel oxygen in the holes. The spraying direction is perpendicular to the substrate.
[0029] The nitrogen flushing oxygen has a spray pressure of 1.8 kg / cm 2 Under negative pressure, nitrogen is sprayed vertically to the substrate from above and below the substrate at the same time, and the sprayed nitrogen is recovered to the negative pressure box through the conduit. Specifically, nitrogen is sprayed vertically from the bottom and top of the oxygen exhaust tank to the substrate located in the middle of the oxygen exhaust tank, and the nitrogen can be recovered to the negative pressure box for recycling.
[0030] The purpose of nitrogen flushing is to expel oxygen in the hole and prevent oxidation of the copper surface, so as to ensure that the newly applied copper seeds are not easily oxidized during sputtering copper plating. Because sputtering has a certain temperature, about 100-200℃, if there is oxygen in the hole, oxides are easily formed.
[0031] Magnetron sputtering coating: Use magnetron sputtering coating machine to coat copper film.
[0032] The magnetron sputtering coating has an acceleration voltage of 250V, a magnetic field of 60G, a pressure of 1mTorr, and a current density of 15mA / cm 2 , power density is 2W / cm 2 , the deposition rate range is 150nm / min~500nm / min.
[0033] After copper deposition, the substrate is placed in a vacuum sputtering machine after a series of treatments such as ultrasonic cleaning, dry ice cleaning, and nitrogen flushing. The specific principle is: in magnetron sputtering, due to the Lorentz force of moving electrons in the magnetic field, their motion trajectories will bend or even produce spiral motion, and their motion paths will become longer, thereby increasing the number of collisions with working gas molecules, increasing the plasma density, and thus greatly improving the magnetron sputtering rate. It can also work at a lower sputtering voltage and pressure, reducing the tendency of film contamination; on the other hand, it also increases the energy of atoms incident on the substrate surface, thereby greatly improving the quality of the film. At the same time, electrons that have lost energy after multiple collisions have become low-energy electrons when they reach the anode, so that the substrate will not overheat.
[0034] General chemical copper deposition utilizes palladium activation and adsorption to promote chemical copper deposition. If the pore shape is poor, the specific surface area will increase rapidly, and the possibility of palladium achieving full adsorption in the same time will decrease, resulting in leakage. Magnetron sputtering has a certain temperature, and the position where copper has not yet been deposited, that is, the point where copper is leaked, will be partially softened. The single-point atomic coordination ability of organic molecular materials will be further released, promoting the growth of the crystal nucleus of the sputtered copper seed, that is, magnetron sputtering after copper deposition can avoid leakage.
[0035] The present invention performs film coating by magnetron sputtering after chemical copper deposition to increase the thickness of copper and ensure smooth electroplating. Magnetron sputtering is a type of physical vapor deposition, which has the advantages of simple equipment, easy control, large coating area and strong adhesion. The magnetron sputtering method realizes high-speed, low-temperature and low-damage copper film coating.
[0036] The present embodiment provides a method for magnetron sputtering assisted copper deposition, which performs film coating by magnetron sputtering to increase the thickness of copper, thereby avoiding the problem of no copper in the hole and missed plating; nitrogen flushing is used to discharge oxygen in the hole to prevent oxidation of the copper surface, thereby ensuring that the newly applied copper seeds are not easily oxidized during magnetron sputtering copper plating; the method is easy to operate and has a good copper plating effect.
[0037] Example 2
[0038] A method for magnetron sputtering assisted copper deposition comprises the following steps in sequence:
[0039] Drilling and copper deposition: The substrate is processed with drilling and copper deposition in sequence.
[0040] Ultrasonic cleaning: Ultrasonic cleaning removes copper particles that are not stably adsorbed on the surface of the substrate and in the holes; the ultrasonic cleaning adopts a frequency of 16kHz, a time of 8 minutes, and a temperature of 60°C. This embodiment uses pure water for washing. Too high a frequency will damage the copper layer formed by copper deposition.
[0041] Dry ice cleaning: Dry ice particles are sprayed on the substrate surface to remove residual chemicals and oxides on the substrate surface. The spray direction is perpendicular to the substrate.
[0042] The dry ice cleaning spray pressure is 2.0kg / cm 2 . Dry ice cleaning, dry ice particles pass through the negative pressure machine from the dry ice storage box, and then are transmitted to the spray tank by the conduit. Several rows of small holes are vertically set on both sides of the spray tank, and the dry ice particles are sprayed onto the substrate through the small holes. The diameter of the small hole is 0.5mm, and the spraying method is to spray vertically from both sides to the two surfaces of the substrate. Dry ice cleaning can slightly remove oxides without causing copper to be absent in the holes, and remove chemical residues on the surface of the substrate under pressure.
[0043] Nitrogen flushing: Nitrogen is sprayed on the substrate surface to expel oxygen in the holes. The spraying direction is perpendicular to the substrate.
[0044] The nitrogen flushing oxygen is injected at a pressure of 2.5 kg / cm 2 Under negative pressure, nitrogen is sprayed vertically to the substrate from above and below the substrate at the same time, and the sprayed nitrogen is recovered to the negative pressure box through the conduit. Specifically, nitrogen is sprayed vertically from the bottom and top of the oxygen exhaust tank to the substrate located in the middle of the oxygen exhaust tank, and the nitrogen can be recovered to the negative pressure box for recycling.
[0045] The purpose of nitrogen flushing is to expel oxygen in the hole and prevent oxidation of the copper surface, so as to ensure that the newly applied copper seeds are not easily oxidized during sputtering copper plating. Because sputtering has a certain temperature, about 100-200℃, if there is oxygen in the hole, oxides are easily formed.
[0046] Magnetron sputtering coating: Use magnetron sputtering coating machine to coat copper film.
[0047] The magnetron sputtering coating has an acceleration voltage of 900 V, a magnetic field of 200 G, a pressure of 10 mTorr, and a current density of 60 mA / cm 2 , power density is 60W / cm 2 , the deposition rate range is 150nm / min~500nm / min.
[0048] After copper deposition, the substrate is placed in a vacuum sputtering machine after a series of treatments such as ultrasonic cleaning, dry ice cleaning, and nitrogen flushing. The specific principle is: in magnetron sputtering, due to the Lorentz force of moving electrons in the magnetic field, their motion trajectories will bend or even produce spiral motion, and their motion paths will become longer, thereby increasing the number of collisions with working gas molecules, increasing the plasma density, and thus greatly improving the magnetron sputtering rate. It can also work at a lower sputtering voltage and pressure, reducing the tendency of film contamination; on the other hand, it also increases the energy of atoms incident on the substrate surface, thereby greatly improving the quality of the film. At the same time, electrons that have lost energy after multiple collisions have become low-energy electrons when they reach the anode, so that the substrate will not overheat.
[0049] General chemical copper deposition utilizes palladium activation and adsorption to promote chemical copper deposition. If the pore shape is poor, the specific surface area will increase rapidly, and the possibility of palladium achieving full adsorption in the same time will decrease, resulting in leakage. Magnetron sputtering has a certain temperature, and the position where copper has not yet been deposited, that is, the point where copper is leaked, will be partially softened. The single-point atomic coordination ability of organic molecular materials will be further released, promoting the growth of the crystal nucleus of the sputtered copper seed, that is, magnetron sputtering after copper deposition can avoid leakage.
[0050] The present invention performs film coating by magnetron sputtering after chemical copper deposition to increase the thickness of copper and ensure smooth electroplating. Magnetron sputtering is a type of physical vapor deposition, which has the advantages of simple equipment, easy control, large coating area and strong adhesion. The magnetron sputtering method realizes high-speed, low-temperature and low-damage copper film coating.
[0051] The present embodiment provides a method for magnetron sputtering assisted copper deposition, which performs film coating by magnetron sputtering to increase the thickness of copper, thereby avoiding the problem of no copper in the hole and missed plating; nitrogen flushing is used to discharge oxygen in the hole to prevent oxidation of the copper surface, thereby ensuring that the newly applied copper seeds are not easily oxidized during magnetron sputtering copper plating; the method is easy to operate and has a good copper plating effect.
[0052] Example 3
[0053] A method for magnetron sputtering assisted copper deposition comprises the following steps in sequence:
[0054] Drilling and copper deposition: The substrate is processed with drilling and copper deposition in sequence.
[0055] Ultrasonic cleaning: Ultrasonic cleaning removes copper particles that are not stably adsorbed on the substrate surface and in the holes; the ultrasonic cleaning adopts a frequency of 14kHz, a time of 6 minutes, and a temperature of 50°C. This embodiment uses pure water for washing. Too high a frequency will damage the copper layer formed by copper deposition.
[0056] Dry ice cleaning: Dry ice particles are sprayed on the substrate surface to remove residual chemicals and oxides on the substrate surface. The spray direction is perpendicular to the substrate.
[0057] The dry ice cleaning spray pressure is 1.5kg / cm 2 . Dry ice cleaning, dry ice particles pass through the negative pressure machine from the dry ice storage box, and then are transmitted to the spray tank by the conduit. Several rows of small holes are vertically set on both sides of the spray tank, and the dry ice particles are sprayed onto the substrate through the small holes. The diameter of the small hole is 0.5mm, and the spraying method is to spray vertically from both sides to the two surfaces of the substrate. Dry ice cleaning can slightly remove oxides without causing copper to be absent in the holes, and remove chemical residues on the surface of the substrate under pressure.
[0058] Nitrogen flushing: Nitrogen is sprayed on the substrate surface to expel oxygen in the holes. The spraying direction is perpendicular to the substrate.
[0059] The nitrogen flushing oxygen has a spray pressure of 2.1 kg / cm 2 Under negative pressure, nitrogen is sprayed vertically to the substrate from above and below the substrate at the same time, and the sprayed nitrogen is recovered to the negative pressure box through the conduit. Specifically, nitrogen is sprayed vertically from the bottom and top of the oxygen exhaust tank to the substrate located in the middle of the oxygen exhaust tank, and the nitrogen can be recovered to the negative pressure box for recycling.
[0060] The purpose of nitrogen flushing is to expel oxygen in the hole and prevent oxidation of the copper surface, so as to ensure that the newly applied copper seeds are not easily oxidized during sputtering copper plating. Because sputtering has a certain temperature, about 100-200℃, if there is oxygen in the hole, oxides are easily formed.
[0061] Magnetron sputtering coating: Use magnetron sputtering coating machine to coat copper film.
[0062] The magnetron sputtering coating has an acceleration voltage of 570V, a magnetic field of 130G, a pressure of 5mTorr, and a current density of 40mA / cm 2 , power density is 30W / cm 2 , the deposition rate range is 150nm / min~500nm / min.
[0063] After copper deposition, the substrate is placed in a vacuum sputtering machine after a series of treatments such as ultrasonic cleaning, dry ice cleaning, and nitrogen flushing. The specific principle is: in magnetron sputtering, due to the Lorentz force of moving electrons in the magnetic field, their motion trajectories will bend or even produce spiral motion, and their motion paths will become longer, thereby increasing the number of collisions with working gas molecules, increasing the plasma density, and thus greatly improving the magnetron sputtering rate. It can also work at a lower sputtering voltage and pressure, reducing the tendency of film contamination; on the other hand, it also increases the energy of atoms incident on the substrate surface, thereby greatly improving the quality of the film. At the same time, electrons that have lost energy after multiple collisions have become low-energy electrons when they reach the anode, so that the substrate will not overheat.
[0064] General chemical copper deposition utilizes palladium activation and adsorption to promote chemical copper deposition. If the pore shape is poor, the specific surface area will increase rapidly, and the possibility of palladium achieving full adsorption in the same time will decrease, resulting in leakage. Magnetron sputtering has a certain temperature, and the position where copper has not yet been deposited, that is, the point where copper is leaked, will be partially softened. The single-point atomic coordination ability of organic molecular materials will be further released, promoting the growth of the crystal nucleus of the sputtered copper seed, that is, magnetron sputtering after copper deposition can avoid leakage.
[0065] The present invention performs film coating by magnetron sputtering after chemical copper deposition to increase the thickness of copper and ensure smooth electroplating. Magnetron sputtering is a type of physical vapor deposition, which has the advantages of simple equipment, easy control, large coating area and strong adhesion. The magnetron sputtering method realizes high-speed, low-temperature and low-damage copper film coating.
[0066] The present embodiment provides a method for magnetron sputtering assisted copper deposition, which performs film coating by magnetron sputtering to increase the thickness of copper, thereby avoiding the problem of no copper in the hole and missed plating; nitrogen flushing is used to discharge oxygen in the hole to prevent oxidation of the copper surface, thereby ensuring that the newly applied copper seeds are not easily oxidized during magnetron sputtering copper plating; the method is easy to operate and has a good copper plating effect.
[0067] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of this implementation shall be included in the protection scope of the present invention.
Claims
1. A method for magnetron sputtering assisted copper deposition, characterized in that: The following steps are included in sequence: Drilling and copper deposition: Drill holes and deposit copper on the substrate in sequence; Ultrasonic cleaning: Ultrasonic cleaning removes copper particles that are not stably adsorbed on the substrate surface and in the holes. The ultrasonic cleaning adopts a frequency of 12-16 kHz, a time of 5-8 min, and a temperature of 40-60°C; Dry ice cleaning: Dry ice particles are sprayed on the substrate surface to remove residual chemicals and oxides on the substrate surface. The spray pressure of dry ice cleaning is 1.0~2.0kg / cm 2 The dry ice particles are transported from the dry ice storage box through the negative pressure machine and then to the spray tank through the conduit. A number of rows of small holes are vertically arranged on both sides of the spray tank, and the dry ice particles are sprayed onto the substrate through the small holes. Nitrogen flushing: Nitrogen is sprayed on the substrate surface to discharge the oxygen in the hole. The pressure of the nitrogen flushing is 1.8~2.5kg / cm 2 , under negative pressure, nitrogen is sprayed vertically to the substrate from above and below the substrate at the same time, and the sprayed nitrogen is recovered to the negative pressure box through the conduit; Magnetron sputtering coating: Use magnetron sputtering coating machine to coat copper film; The magnetron sputtering coating has an acceleration voltage of 250-900 V, a magnetic field of 60-200 G, a pressure of 1-10 mTorr, and a current density of 15-60 mA / cm 2 , power density is 2~60W / cm 2 The magnetron sputtering coating has a deposition rate ranging from 150 nm / min to 500 nm / min.
2. The method for magnetron sputtering assisted copper deposition according to claim 1, characterized in that: During dry ice cleaning and nitrogen flushing, the spray direction is perpendicular to the substrate.
3. The method for magnetron sputtering assisted copper deposition according to claim 1, characterized in that: The ultrasonic cleaning adopts pure water washing.