A carbon-free and solid-waste-free electrolytic cell for co-production of oxygen and aluminum
By employing an oxygen-aluminum co-production electrolysis process with carbon-free anodes and cathodes, combined with a specially designed electrode structure and a carbon-free tank bottom substrate, the greenhouse gas emissions and solid waste pollution problems in the Hall-Herrou process electrolysis have been solved, achieving green and environmentally friendly electrolytic aluminum production.
Patent Information
- Application Number
- CN202110602251.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-05-31
AI Technical Summary
The existing Hall-Erou process for producing primary aluminum involves significant greenhouse gas emissions, solid waste pollution, production instability, and high labor intensity. In particular, the consumption of carbon materials and solid waste treatment cause serious environmental damage.
The oxygen-aluminum co-production electrolysis process employs carbon-free anodes and carbon-free cathodes, combined with a specially designed vertical inert electrode and carbon-free tank bottom substrate structure, including a vertical carbon-free anode, a metal-ceramic conductive cathode, and a carbon-free tank bottom substrate. Through the combination of inert conductive ceramic materials and special structural layers, the stability of the electrode and the recycling of materials are achieved.
This process achieves zero solid waste emissions during electrolysis, reduces production costs, improves production efficiency, reduces land occupation, lowers labor intensity and occupational risks, and uses oxygen as a byproduct, thus reducing environmental pollution.
Smart Images

Figure CN115478303B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aluminum smelting and renewable energy utilization, and relates to an oxygen-aluminum co-production electrolysis method, which is characterized by being carbon-free and solid waste-free. Background Art
[0002] In 1886, Heroult of France and Hall of the United States independently applied for and registered patents for the electrolytic production of aluminum by alumina in cryolite melt, ushering in the large-scale electrolytic production of primary aluminum by the Hall-Heroult process (HH electrolysis process).
[0003] The current Hall-Heroult process for electrolytic production of primary aluminum uses consumable carbon anodes and carbon cathodes. The anode not only consumes a large amount of carbon materials, mainly high-quality petroleum coke, but also emits a large amount of greenhouse gas CO. 2 , strong greenhouse gases fluorocarbons (CF 4 , C 2 F 6 ), SO 2 In addition, in the current aluminum electrolysis process, the prebaked anode carbon blocks need to be replaced frequently, which leads to unstable electrolysis production, increased labor intensity, personal risks faced by workers in high-temperature melts, and unorganized emissions of fluorides. The production process of prebaked carbon anodes also emits carcinogenic aromatic compounds (PAH), SO 2 , dust, which are one of the main sources of PM2.5; the use of carbon electrodes as cathodes is also one of the main sources of solid waste in current aluminum electrolysis, and the environmental harm it brings cannot be underestimated.
[0004] Entering the 21st century, the production of electrolytic aluminum in my country and the world has developed rapidly. According to statistics, the current production of electrolytic aluminum in my country is about 40 million tons. With the increase in the production of electrolytic aluminum, the production of solid waste generated in the electrolytic process, such as waste cathode carbon blocks, waste anode carbon slag, waste refractory bricks, waste insulation bricks, and waste insulation slag, has also increased rapidly. Under normal circumstances, every 10,000 tons of electrolytic aluminum produced will produce 100 tons of waste carbon materials, 80 tons of waste refractory materials and a certain amount of insulation materials. Under existing technical conditions, most electrolytic aluminum plants use the construction of plant buildings to pile up solid waste from electrolytic aluminum, which not only occupies a large amount of land, but also contains soluble fluorides and cyanides that may seep into the ground to pollute the soil, groundwater, and surface water, causing great harm to the surrounding ecological environment, human health, and the growth of plants and animals. Summary of the invention
[0005] The use of non-carbon anodes or inert anodes to realize the new process of oxygen and aluminum co-production electrolysis can solve the above-mentioned emission and pollution problems, and can improve production efficiency, reduce floor space, and reduce production costs. It has become the focus of attention and research hotspot in the international aluminum industry and materials industry. The use of carbon-free anodes in the oxygen-aluminum co-production electrolysis process has the following advantages:
[0006] (1) The electrodes are hardly consumed during the electrolysis process, and no additional carbon processing plant or carbon anode assembly plant is required, which reduces production costs and eliminates the environmental impact and pollution caused by the production and use of carbon anodes;
[0007] (2) No carbon residue solid waste is generated;
[0008] (3) The electrodes are not consumed, the inter-electrode distance is stable and easy to control, the frequency of anode replacement is reduced by more than ten times, and the labor intensity and occupational risks are greatly reduced;
[0009] (4) A higher current per unit volume can be used to increase the capacity of the electrolytic cell;
[0010] (5) The anode product is oxygen, which avoids environmental pollution. Oxygen can also be used as a by-product.
[0011] Furthermore, the present invention not only adopts carbon-free anode, but also carbon-free cathode and carbon-free cell bottom, mainly through specially designed cathode structure, aluminum water pool and aluminum electrolytic cell lining structure, which can solve the solid waste pollution of aluminum electrolysis. It is specifically achieved through the following technical solutions:
[0012] An oxygen-aluminum co-production carbon-free and solid waste-free electrolytic cell, using a vertical inert electrode and a carbon-free cell bottom substrate, wherein the vertical inert electrode includes a vertical carbon-free anode and a vertical metal ceramic conductive cathode structure, wherein the cathode structure includes: a cathode plate, a conductive ceramic pile, a small cathode conductive rod, a small cathode conductive rod protective sleeve, and a large cathode conductive rod; the cathode plate is connected to the small cathode conductive rod and the large cathode conductive rod through the conductive ceramic pile; the large cathode conductive rod outputs electricity from the bottom or side of the electrolytic cell;
[0013] The carbon-free tank bottom matrix structure includes, from bottom to top, a thermal insulation structure layer, an anti-seepage structure layer, an aluminum pool main construction layer, and an aluminum liquid scouring prevention layer.
[0014] The cathode plate is made of an inert conductive ceramic material that can be wetted by aluminum water and is resistant to aluminum water corrosion. It is formed by powder metallurgy and has a flat plate structure as a whole, or a flat plate at the top and a trapezoidal structure at the bottom, or a flat plate at the top and an inverted T-shaped structure at the bottom, or a flat plate with an open hole at the bottom. The four structures are all convenient for assembling the cathode plate and the conductive ceramic pile. When assembling, the joint surface of the two is made of TiB 2 The paste is fixed to prevent the cathode plate from falling off during operation.
[0015] The conductive ceramic pile material is an inert conductive ceramic material that can be wetted by aluminum water and is resistant to aluminum water corrosion, and is formed by powder metallurgy. A flat groove, a trapezoidal groove, an inverted T-shaped groove, or a wedge pin structure with a hole is opened on the upper part of the conductive ceramic pile to correspond to and be fixed to the lower part of the cathode plate; two large and small step holes are opened on the lower part of the conductive ceramic pile, the large hole is glued to the protective cover of the cathode small conductive rod through an anti-oxidation sealing filler for the small conductive rod, and the small hole is pressurized and connected to the cathode small conductive rod through high-temperature conductive slurry and foam metal.
[0016] There are two step holes, one large and one small, on the cathode large conductive rod. The small hole is used to position the cathode small conductive rod and the cathode large conductive rod. Pure molten iron is poured around the large hole to fix the two, or they are fixed by crimping with foam metal and conductive sealant.
[0017] The cathode small conductive rod protection sleeve is mainly used to prevent the small conductive rod from oxidation and protect it from high temperature electrolyte and aluminum water corrosion. 2 O 3 、SiC、TiB 2 , mullite or basalt.
[0018] The cathode small conductive rod and the cathode large conductive rod are made of conductive metal or alloy material. Further, the cathode small conductive rod and the cathode large conductive rod are made of carbon steel, stainless steel, copper, nickel, pure iron or pure iron with anti-oxidation coating.
[0019] The thermal insulation structure layer uses calcium silicate board, thermal insulation bricks, and anti-seepage thermal insulation bricks in order from bottom to top; the bottom two layers (calcium silicate board and thermal insulation bricks) in the thermal insulation structure layer mainly play the role of thermal insulation and heat insulation;
[0020] The anti-seepage structural layer is mainly composed of dry anti-seepage materials; the dry anti-seepage powder in the anti-seepage structural layer for anti-seepage and heat insulation completely covers the cathode large conductive rod, combines with the electrolyte to form a glassy state in the early stage, and forms a whole to prevent further penetration of aluminum water and electrolyte, and plays a role in protecting the cathode large conductive rod and the cathode small conductive rod;
[0021] The main construction layer of the aluminum pool plays the role of forming an aluminum water pool, protecting the cathode steel rod, and heat insulation, and is mainly composed of a high-aluminum prefabricated layer I, an alumina powder layer, and a high-aluminum prefabricated layer II; further, the high-aluminum prefabricated layer I in the main construction layer of the aluminum pool is assembled from multiple blocks, with a yin-yang L-shaped or yin-yang T-shaped fit, and the gaps between the blocks are filled with alumina powder; the alumina powder layer between the upper and lower high-aluminum prefabricated layers is 1-3 cm, and is initially combined with the electrolyte to form a solid state; the high-aluminum prefabricated layer II is also assembled from multiple blocks, with a yin-yang L-shaped or yin-yang T-shaped fit, and the gaps between the blocks are filled with alumina powder; the top high-aluminum prefabricated layer forms a "leg-extending" structure with the high-aluminum prefabricated layers around the groove; considering the convenience of structural assembly, the high-aluminum prefabricated layer is designed to be 2 or more layers, and the layers are separated by an alumina powder layer.
[0022] The anti-aluminum liquid erosion layer plays a role of corrosion resistance and wear resistance. It is mainly composed of sintered high-aluminum prefabricated layer, corundum, SiC, MgO, MgO-C, TiB 2 , BN materials or one or more of them are made into thin plates and laid out.
[0023] Cathode material recycling:
[0024] ① The cathode plate and conductive ceramic pile are made of conductive ceramic (such as TiB 2 , ZrB 2 ② Cathode small conductive rod protective cover (mainly made of Al 2 O 3 ) can be recycled and added to the electrolyte or used as the tank lining or anti-seepage layer; ③ the cathode small conductive rod and the large conductive rod are made of metal or alloy materials and can be smelted into new conductive rods;
[0025] Liner recycling:
[0026] ① The three layers at the bottom (calcium silicate board, thermal insulation bricks, anti-seepage insulation bricks) are the most stable. The structure can be retained and continued to be used when the electrolytic cell is overhauled; ② The dry anti-seepage material layer will be divided into two layers: the upper glassy thin layer and the bottom powder layer, the glassy thin layer; the powder layer can be recycled; ③ The upper high-aluminum prefabricated parts and alumina powder can be recycled after being corroded by the electrolyte and aluminum liquid, and used as the electrolyte raw material when starting the cell; ④ The aluminum liquid erosion-resistant layer uses high-aluminum sintered plates, corundum, SiC, MgO, MgO-C, TiB2, and BN, which can be recycled or used for cell lining. High-aluminum sintered plates and corundum can also be directly added to the electrolyte.
[0027] The beneficial effects of the present invention are:
[0028] The electrolytic cell of the present invention can realize the recovery and recycling of all materials in the cell, truly realizing zero solid waste, i.e. eliminating dangerous solid wastes such as carbon slag and waste cathode carbon blocks inherent in traditional carbon-containing aluminum electrolytic cells, making the aluminum industry cleaner, greener and more environmentally friendly, and aluminum a greener metal. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of a solid waste-free electrolytic cell; a-front view, b-left view;
[0030] Figure 2 Cathode plate and installation form with conductive ceramic pile 1-flat plate, a-front view, b-left view, c-assembly drawing;
[0031] Figure 3 Cathode plate and installation form with conductive ceramic pile 2-trapezoidal plate, a-front view, b-left view, c-assembly drawing;
[0032] Figure 4 Cathode plate and installation form with conductive ceramic pile 3-"T" shaped plate, a-front view, b-left view, c-assembly drawing;
[0033] Figure 5 Cathode plate and installation form with conductive ceramic pile 4-hole plate, a-front view, b-left view, c-assembly drawing;
[0034] Figure 6 Schematic diagram of the "yin-yang fit" "L"-shaped structure of high-aluminum prefabricated parts;
[0035] Figure 7 Schematic diagram of the "yin-yang fit" "T" structure of high-aluminum prefabricated parts;
[0036] Figure 8 Schematic diagram of the assembly of ceramic conductive pile, cathode small conductive rod and cathode small conductive rod protection set, the cathode small conductive rod is partially sealed;
[0037] Fig. 9 Schematic diagram of the assembly of ceramic conductive pile, cathode small conductive rod and cathode small conductive rod protection set, the cathode small conductive rod is fully sealed;
[0038] Fig.10 Schematic diagram of the assembly of the cathode large conductive rod, the cathode small conductive rod, and the cathode small conductive rod protection set;
[0039] Description of reference numerals:
[0040] 1 anode, 2 cathode plate, 3 high aluminum prefabricated layer II, 4 alumina powder layer, 5 high aluminum prefabricated layer I, 6 dry anti-seepage material, 7 aluminum liquid erosion prevention layer, 8 cathode small conductive rod protective cover, 9 cathode small conductive rod, 10 cathode large conductive rod, 11 conductive ceramic pile. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with the specification and examples, but is not intended to limit the scope of protection thereof.
[0042] Example 1
[0043] like Figure 1 As shown, it is a schematic diagram of the oxygen-aluminum co-production carbon-free and solid waste-free electrolytic cell of the present invention, which adopts a vertical carbon-free anode, a vertical metal ceramic conductive cathode structure, and a carbon-free cell bottom substrate, wherein the cathode structure comprises: a cathode plate 2, a conductive ceramic pile 11, a cathode small conductive rod 9, a cathode small conductive rod protection sleeve 8, and a cathode large conductive rod 10; the cathode plate 2 is connected to the cathode small conductive rod 9 and the cathode large conductive rod 10 through the conductive ceramic pile 11; the cathode large conductive rod 10 outputs electricity from the bottom or side of the electrolytic cell; specifically: the cathode plate 2 is assembled with the conductive ceramic pile 11, and the bonding surface of the two is made of TiB during assembly. 2The paste is fixed; the upper structure of the conductive ceramic pile 11 corresponds to and is fixed to the lower part of the cathode plate 2; two step holes of different sizes are opened at the lower part of the conductive ceramic pile 11, the large hole is glued to the cathode small conductive rod protection sleeve 8 through the anti-oxidation sealing filler of the small conductive rod, and the small hole is pressurized and connected to the cathode small conductive rod 9 through high-temperature conductive paste and foam metal; there are two step holes of different sizes on the cathode large conductive rod 10, the small hole is used to position the cathode small conductive rod 9 and the cathode large conductive rod 10, and pure iron water is poured around the large hole to fix the two or they are crimped and fixed by foam metal and conductive sealant;
[0044] The cathode plate 2 is made of an inert conductive ceramic material that is wettable by aluminum water and resistant to aluminum water corrosion, and is formed by powder metallurgy;
[0045] The conductive ceramic pile 11 is made of an inert conductive ceramic material that can be wetted by aluminum water and is resistant to aluminum water corrosion, and is formed by powder metallurgy.
[0046] The cathode small conductive rod protection sleeve 8 is made of Al 2 O 3 、SiC、TiB 2 , mullite or basalt;
[0047] The cathode small conductive rod 9 and the cathode large conductive rod 10 are made of carbon steel, stainless steel, copper, nickel, pure iron or pure iron with an anti-oxidation coating.
[0048] The carbon-free tank bottom matrix structure is: from bottom to top, it mainly includes a thermal insulation structure layer, an anti-seepage structure layer, an aluminum pool main construction layer, and an aluminum liquid scouring prevention layer.
[0049] The thermal insulation structure layer uses calcium silicate board, thermal insulation bricks, and anti-seepage insulation bricks in order from bottom to top;
[0050] The anti-seepage structural layer is composed of a dry anti-seepage material 6, which completely covers the cathode large conductive rod 10, and combines with the electrolyte to form a glass state in the initial stage, forming a whole to protect the cathode large and small conductive rods 9;
[0051] The main construction layer of the aluminum pool is composed of a high-aluminum prefabricated layer I, an alumina powder layer, and a high-aluminum prefabricated layer II; the high-aluminum prefabricated layer is designed to have 2 or more layers, and the layers are separated by an alumina powder layer;
[0052] The anti-aluminum liquid erosion layer is composed of a sintered high-aluminum prefabricated layer, corundum, SiC, MgO, MgO-C, TiB 2 , BN materials or one or more of them are made into thin plates and laid out.
[0053] Example 2
[0054] like Figure 2 , Figure 2 As shown in (a) and (b), the cathode plate is a flat plate structure. Figure 2(c) The cathode plate and the conductive ceramic pile are installed. The flat cathode plate is assembled with the conductive ceramic pile 11 with a flat groove on the top. The joint surface of the two is made of TiB 2 The paste is fixed, and other structures are the same as those in Example 1.
[0055] Example 3
[0056] like Figure 3 , Figure 3 As shown in (a) and (b), the cathode plate is a flat plate on the top and a trapezoidal structure on the bottom. Figure 3 (c) The cathode plate and the conductive ceramic pile installation form, the upper flat plate, the lower trapezoidal cathode plate and the upper trapezoidal groove conductive ceramic pile 11 are assembled, and the joint surface of the two is made of TiB 2 The paste is fixed, and other structures are the same as those in Example 1.
[0057] Example 4
[0058] like Figure 4 , Figure 4 As shown in (a) and (b), the cathode plate is a flat plate on the top and an inverted T-shaped structure on the bottom. Figure 4 (c) The cathode plate and the conductive ceramic pile installation form, the upper flat plate, the lower inverted T-shaped cathode plate and the upper inverted T-shaped groove conductive ceramic pile 11 are assembled, and the joint surface of the two is made of TiB 2 The paste is fixed, and other structures are the same as those in Example 1.
[0059] Example 5
[0060] like Figure 5 , Figure 5 As shown in (a) and (b), the cathode plate is a flat plate with holes at the bottom. Figure 5 (c) The cathode plate and the conductive ceramic pile are installed in the form of a cathode plate with a hole structure at the bottom of the flat plate and a conductive ceramic pile 11 with a wedge pin structure with a hole at the top. When assembling, the joint surface of the two is made of TiB 2 The paste is fixed, and other structures are the same as those in Example 1.
[0061] Example 6
[0062] like Figure 6 As shown, in this embodiment, the high-aluminum prefabricated layer I and the high-aluminum prefabricated layer II in the main construction layer of the aluminum pool are assembled in multiple pieces, and the high-aluminum prefabricated parts are matched in a yin-yang "L" shape. Other structures are the same as in Example 1.
[0063] Example 7
[0064] like Figure 7As shown, in this embodiment, the high-aluminum prefabricated layer I and the high-aluminum prefabricated layer II in the main construction layer of the aluminum pool are assembled in multiple pieces, and the high-aluminum prefabricated parts are connected in a yin-yang "T" shape. Other structures are the same as Example 1.
[0065] Example 8
[0066] In this design, the ceramic conductive pile, the cathode small conductive rod, and the cathode small conductive rod protection set are arranged as follows: Figure 8 The structure is not limited to round rods, rectangular rods and polygonal rods are also possible.
[0067] like Figure 8 As shown, a schematic diagram of the assembly of a ceramic conductive pile 11, a cathode small conductive rod 9, and a cathode small conductive rod protection sleeve 8 is shown. Two step holes of different sizes are opened at the lower part of the conductive ceramic pile 11. The large hole is glued to the cathode small conductive rod protection sleeve 8 through an anti-oxidation sealing filler for the small conductive rod, and the small hole is pressurized and connected to the cathode small conductive rod 9 through high-temperature conductive paste and foam metal. Among them, the cathode small conductive rod is partially sealed, and other structures are the same as those in Example 1.
[0068] Example 9
[0069] In this design, the ceramic conductive pile, the cathode small conductive rod, and the cathode small conductive rod protection set are arranged as follows: Fig. 9 The structure is not limited to round rods, rectangular rods and polygonal rods are also possible.
[0070] like Fig. 9 As shown, a schematic diagram of the assembly of a ceramic conductive pile 11, a cathode small conductive rod 9, and a cathode small conductive rod protection cover 8 is shown. Two step holes of different sizes are opened at the lower part of the conductive ceramic pile 11. The large hole is glued to the cathode small conductive rod protection cover 8 through an anti-oxidation sealing filler for the small conductive rod, and the small hole is pressurized and connected to the cathode small conductive rod 9 through high-temperature conductive paste and foam metal. Among them, the cathode small conductive rod is fully sealed, and other structures are the same as those in Example 1.
[0071] Example 10
[0072] In this design, the cathode large conductive rod 10, the cathode small conductive rod 9, and the cathode small conductive rod protective cover 8 are assembled as follows: Fig.10 The cathode large conductive rod 10 shown has two stepped holes, one large and one small. The small hole is used to position the cathode small conductive rod 9 and the cathode large conductive rod 10. Pure molten iron is poured around the large hole to fix the two or they are crimped and fixed by foam metal plus conductive sealant.
[0073] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An oxygen-aluminum co-production carbon-free and solid waste-free electrolytic cell, characterized in that: A vertical inert electrode and a carbon-free tank bottom substrate are used, wherein the vertical inert electrode comprises a vertical carbon-free anode and a vertical carbon-free metal ceramic conductive cathode structure, wherein the cathode structure comprises: a cathode plate (2), a conductive ceramic pile (11), a small cathode conductive rod (9), a small cathode conductive rod protective sleeve (8), and a large cathode conductive rod (10); the cathode plate (2) is connected to the small cathode conductive rod (9) and the large cathode conductive rod (10) through the conductive ceramic pile (11); the large cathode conductive rod (10) outputs electricity from the bottom or side of the electrolytic tank; The cathode plate (2) is made of an inert conductive ceramic material that can be wetted by aluminum water and is resistant to aluminum water corrosion, and is formed by powder metallurgy. The overall structure is a flat plate; or an upper flat plate and a lower trapezoidal structure; or an upper flat plate and a lower inverted T-shaped structure; or a flat plate with an open hole at the bottom. The cathode plate (2) is assembled with a conductive ceramic pile (11), and the joint surface of the two is fixed with TiB2 paste during assembly. The carbon-free tank bottom matrix structure includes, from bottom to top, a thermal insulation structure layer, an anti-seepage structure layer, an aluminum pool main construction layer, and an aluminum liquid scouring prevention layer.
2. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The conductive ceramic pile (11) is made of an inert conductive ceramic material that can be wetted by aluminum water and is resistant to aluminum water corrosion, and is formed by powder metallurgy. The upper part of the conductive ceramic pile (11) is provided with a flat groove, a trapezoidal groove, an inverted T-shaped groove, or a wedge pin structure with a hole, which corresponds to and is fixed to the lower part of the cathode plate (2); the lower part of the conductive ceramic pile (11) is provided with two stepped holes, one large and one small, the large hole is glued to the cathode small conductive rod protective sleeve (8) through a sealing filler to prevent the small conductive rod from oxidation, and the small hole is pressurized and connected to the cathode small conductive rod (9) through high-temperature conductive paste and foam metal.
3. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The cathode large conductive rod (10) has two stepped holes, one large and one small. The small hole is used to position the cathode small conductive rod (9) and the cathode large conductive rod (10). Pure molten iron is poured around the large hole to fix the two, or they are fixed by crimping with foam metal and conductive sealant.
4. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The cathode small conductive rod protective sleeve (8) is made of Al2O3, TiB2, mullite or basalt; the cathode small conductive rod (9) and the cathode large conductive rod (10) are made of conductive metal or alloy material.
5. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The small cathode conductive rod (9) and the large cathode conductive rod (10) are made of stainless steel, copper, nickel, pure iron or pure iron with an anti-oxidation coating.
6. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The thermal insulation structure layer uses calcium silicate board, thermal insulation bricks and anti-seepage thermal insulation bricks in sequence from bottom to top.
7. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The anti-seepage structural layer is composed of a dry anti-seepage material (6). The dry anti-seepage material completely covers the cathode large conductive rod (10) and combines with the electrolyte to form a glassy state in the initial stage to form a whole, thereby protecting the cathode large conductive rod (10) and the cathode small conductive rod (9).
8. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The main structure of the aluminum pool is composed of a high-aluminum prefabricated layer I (5), an aluminum oxide powder layer (4), and a high-aluminum prefabricated layer II (3); The high-aluminum prefabricated layer I (5) in the main structure of the aluminum pool is assembled in multiple blocks, with positive and negative L-shaped or positive and negative T-shaped fits, and the gaps between the blocks are filled with alumina powder; the alumina powder layer between the upper and lower high-aluminum prefabricated layers is 1-3 cm, and is combined with the electrolyte to form a solid state in the early stage; The high-aluminum prefabricated layer II (3) is also assembled with multiple blocks, which are matched in a positive and negative L-shape or a positive and negative T-shape, and the gaps between the blocks are filled with alumina powder; the top high-aluminum prefabricated layer forms a "stretched leg" structure with the high-aluminum prefabricated layers around the groove; the high-aluminum prefabricated layer is designed to have 2 or more layers, and the layers are separated by alumina powder layers (4).
9. The carbon-free and solid-waste-free electrolytic cell for oxygen-aluminum co-production according to claim 1, characterized in that: The anti-aluminum liquid erosion layer is composed of a sintered high-aluminum prefabricated layer, a thin plate made of one or more materials selected from corundum, MgO, TiB2, and BN.