A method for chemically recycling waste PET products by utilizing the phase change properties of BHET crystals
By utilizing the phase change properties of BHET crystals, the separation of other additives in waste PET products is achieved, the recycling process is simplified, the purity and whiteness of BHET are improved, and the problems of low recycling efficiency and environmental pollution in the existing technology are solved. , providing an efficient and green PET recycling method.
Patent Information
- Application Number
- CN202211030736.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-26
AI Technical Summary
In the existing technology, in the chemical recycling of waste PET products, especially polyester textiles, other polymers and dyes have an impact on the purity of BHET, leading to problems of low recycling efficiency and environmental pollution.
Utilizing the unique phase change properties of BHET crystals, BHET is separated and purified through cooling crystallization, reduced pressure sublimation and condensation steps after alcoholysis reaction, simplifying the process and reducing energy consumption and costs.
It achieves high purity (>98%) and high whiteness (>97%) BHET recovery, solves the problem of polycondensation of amorphous BHET under heated vacuum conditions, and provides a new path for the recycling of waste PET products, and The process is simple, easy, green and environmentally friendly.
Smart Images

Figure CN115894223B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-quality recycling of waste polyester fabrics and environmental protection, and in particular to a method for chemically recycling waste PET products by utilizing the phase change properties of BHET crystals. Background Art
[0002] my country is a major producer and consumer of textiles, among which polyethylene terephthalate (PET, referred to as polyester) is the main textile raw material. In 2021, the production of PET reached 53.63 million tons. With the sharp increase in the annual output of PET, the amount of PET waste has also increased rapidly. Because PET is not biodegradable, it not only causes huge waste of resources, but also causes serious environmental pollution. Therefore, the development of clean and efficient recycling technology for waste PET products, especially waste polyester textiles, and the preparation of high-quality, high-value-added fiber raw materials are of great significance to improving resource utilization and reducing environmental pollution.
[0003] At present, there are mainly physical and chemical methods for recycling waste PET products. Among them, the physical method has become the mainstream regeneration method due to its simple process. However, the performance of the regenerated products of the physical method is poor, and it can only be downgraded for use, and it cannot achieve the real recycling of waste PET. The ethylene glycol alcoholysis method in the chemical method depolymerizes waste PET into oligomers or monomers ethylene glycol terephthalate (BHET), both of which are the main raw materials for synthesizing PET in industry. Therefore, the ethylene glycol alcoholysis method is an ideal method for achieving high-quality PET recycling. The depolymerization technology of preparing BHET by ethylene glycol alcoholysis of PET in industry is quite mature, but the technology of recycling waste PET products, especially polyester textiles, by ethylene glycol alcoholysis still has many problems in practical application. Waste PET products, especially waste polyester textiles, contain a large amount of other polymers or natural polymer materials (spandex, nylon, cotton). These added materials undergo depolymerization reactions or a series of complex chemical reactions under alcoholysis conditions, which will increase the difficulty of recycling the target product BHET, making the purity of the recovered BHET monomer low. In addition, a large amount of dyes contained in waste textiles will also undergo complex chemical reactions under alcoholysis conditions. Recovering colored BHET will greatly reduce the quality of recycled PET. Therefore, the decolorization and purification of PET depolymerization monomers are urgent issues to be solved in achieving the recycling of waste PET.
[0004] In order to solve the adverse effects of other polymers (spandex, nylon, cotton, etc.) in waste polyester textiles on the purity of the target product BHET during the alcoholysis process, the researchers mainly added a separation process before the alcoholysis reaction. Among them, the solvent method is an effective separation method. The invention patent with publication number US4345039 discloses a method of using hydrochloric acid to treat polyester / cotton blended waste and then separating cellulose materials from polyester fibers; the invention patent with publication number CN110790980A discloses a separation method of using an organic solvent with a boiling point of 20-230°C to fully contact and impregnate the waste PET products after opening at a temperature of 20-180°C to dissolve the easily soluble fibers other than PET; the invention patent with publication number CN110734578A discloses a separation method of using a solvent (dimethylacetamide, dimethyl sulfoxide, etc.) to separate easily soluble impurities such as spandex and nylon from waste PET pellets. However, most of these methods have problems such as long process flow, low efficiency and environmental pollution (using high-cost, toxic solvents and chemicals).
[0005] In order to solve the adverse effects of dyes in waste polyester textiles on the purity of the target product BHET during alcoholysis, researchers mainly add a decolorization process before / after alcoholysis. For example, the invention patent with publication number CN109574835A discloses a method for adsorbing and decolorizing PET alcoholysis products using ion-modified activated carbon; the invention patent with publication number US6642350B1 discloses a device for decolorizing and purifying BHET using a combination of activated carbon and ion exchange resin. The invention patent with publication number US5635584 discloses a method for decolorizing PET alcoholysis products using recrystallization. However, most of these methods have problems such as low decolorization rate, high cost, and serious environmental pollution.
[0006] Based on the above problems, an efficient, economical and green method for purifying PET alcoholysis product BHET is sought to achieve the recycling of waste polyester textiles. Summary of the invention
[0007] The purpose of the present invention is to provide a method for chemically recovering waste PET products by utilizing the phase change properties of BHET crystals. The method mainly utilizes the unique phase change properties of crystalline BHET relative to amorphous BHET to achieve the purification and decolorization of BHET. It is a universal method that can recover high-quality BHET from waste PET products with diverse components.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] The present invention provides a method for chemically recycling waste PET products by utilizing the phase change properties of BHET crystals, comprising the following steps:
[0010] The waste PET products and the catalyst are mixed in ethylene glycol to carry out alcoholysis reaction to obtain alcoholysis solution;
[0011] Cooling the alcoholysis solution to crystallize to obtain a BHET-containing crystal;
[0012] Subliming the crystals under reduced pressure;
[0013] Condensate and collect BHET.
[0014] Preferably, the reduced pressure sublimation is carried out at a temperature of 110 to 140° C. and a vacuum degree of 5 to 15 torr.
[0015] Preferably, the condensation temperature is 25°C to 30°C.
[0016] Preferably, the reaction temperature of the alcoholysis reaction is 230°C to 250°C.
[0017] Preferably, the reaction time of the alcoholysis reaction is 2 h to 4 h.
[0018] Preferably, the mass ratio of the waste PET product to the catalyst is 1:0.02-0.1.
[0019] Preferably, the molar ratio of the waste PET product to the ethylene glycol is 1:6-10.
[0020] Preferably, the temperature of the cooling crystallization is 8-10°C.
[0021] Preferably, the cooling crystallization time is 8 to 12 hours.
[0022] Preferably, the catalyst is any one of carbonates, acetates, hydroxides of alkaline earth metals, oxides of alkaline earth metals and transition metal coordination compounds having alkoxy groups, or a combination of several of them.
[0023] Preferably, the waste PET products are at least one of waste polyester textiles, plastic bottles, films, and industrial raw materials.
[0024] Preferably, the waste PET product further includes pretreatment steps of impurity removal, crushing and granulation before mixing with the catalyst.
[0025] Any range described in the present invention includes the end value and any numerical value between the end values and any sub-range formed by the end value or any numerical value between the end values.
[0026] Unless otherwise specified, all raw materials in the present invention can be purchased from the market, and the equipment used in the present invention can adopt conventional equipment in the relevant field or refer to the existing technology in the relevant field.
[0027] The beneficial effects of the present invention are as follows:
[0028] The present invention proposes for the first time to utilize the unique phase change properties of BHET crystals to achieve effective separation of BHET from other additives or reaction products in waste PET products, thereby recovering high-quality BHET.
[0029] The method provided by the present invention not only simplifies the recycling process of waste PET products, reduces the energy consumption and cost of recycling waste PET, but also breaks through the technical bottleneck of difficult decolorization and purification of BHET, effectively overcomes the key problem of easy polycondensation of non-crystalline BHET under heating and vacuum conditions, and provides a new path for high-quality recycling of waste PET products, especially waste polyester textiles.
[0030] When the chemical recovery method of the present invention is used to recover BHET in waste polyester textiles, a BHET monomer with a purity higher than 98% and a whiteness (L value) higher than 97 can be directly obtained. The BHET monomer can be directly used as a raw material for regenerated PET polyester without further ester exchange.
[0031] The method provided by the invention is simple and easy to implement, green and environmentally friendly, suitable for industrialization, and has good social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0033] Figure 1 A schematic diagram showing the process of preparing BHET crystals from waste polyester textiles in Example 1;
[0034] Figure 2 The nuclear magnetic resonance analysis spectrum of BHET prepared in Example 1 is shown;
[0035] Figure 3 The HPLC analysis spectrum of BHET prepared in Example 1 is shown;
[0036] Figure 4 The whiteness test L, a, and b values of the BHET prepared in Example 1 are shown;
[0037] Figure 5 A schematic diagram showing the process of preparing BHET crystals from waste polyester textiles in Example 2;
[0038] Figure 6 The nuclear magnetic resonance analysis spectrum of BHET prepared in Example 2 is shown;
[0039] Figure 7 The HPLC analysis spectrum of BHET prepared in Example 2 is shown;
[0040] Figure 8 The whiteness test L, a, and b values of the BHET prepared in Example 2 are shown;
[0041] Fig. 9 A schematic diagram showing the process of preparing BHET crystals from waste polyester textiles in Example 3;
[0042] Fig.10 The nuclear magnetic resonance analysis spectrum of BHET prepared in Example 3 is shown;
[0043] Fig.11 The HPLC analysis spectrum of BHET prepared in Example 3 is shown;
[0044] Fig.12 The whiteness test L, a, and b values of the BHET prepared in Example 3 are shown. DETAILED DESCRIPTION
[0045] The current recycling of waste PET products, especially the recycling of waste polyester textiles, usually includes at least three processes: separation of polymer additives, PET depolymerization and decolorization, which are not only inefficient, but also have high recycling costs and environmental pollution. Therefore, the present invention aims to provide an efficient, green and environmentally friendly method for high-quality chemical recycling of waste polyester textiles by utilizing the unique phase change properties of BHET crystals.
[0046] The recycling method of the present invention is to depolymerize PET products, especially waste polyester textiles, to obtain crude BHET (crude BHET refers to BHET containing various impurities, such as spandex, nylon, cotton, dyeing agents, colorants, etc. and their reaction by-products), and then purify the crude BHET to obtain BHET with higher purity and decolorization.
[0047] Specifically, in the step of obtaining an alcoholysis solution by alcoholysis reaction,
[0048] First, we need to prepare the raw materials: waste PET products.
[0049] The waste PET products may be at least one of waste polyester textiles, plastic bottles, films, industrial raw materials, and the like.
[0050] The main component of the waste PET products is PET, and more preferably the content of PET is at least 60% to 100%. These waste PET products often contain other additives, including but not limited to any one or a combination of heterogeneous polymers, colorants, moisture absorbents, delustering agents, flame retardants, moisture absorbents, and gas barrier agents.
[0051] The heterogeneous polymers include, but are not limited to, any one or more of spandex, nylon, cotton, polyethylene isophthalate, polyethylene naphthalate, polyethylene glycol acid, and the like.
[0052] The colorant includes natural colorants and / or synthetic colorants; the natural colorant includes but is not limited to any one or more of chrome yellow, ultramarine, manganese brown, cochineal red, indigo, madder, safflower, safflower, sophora japonica, turmeric, gardenia, phellodendron, lithospermum, perilla, etc.; the synthetic colorant includes but is not limited to any one or more of azo, anthracene and diphenylmethane, etc.
[0053] Next, a catalyst is selected. Those skilled in the art can select a catalyst suitable for PET alcoholysis according to needs, such as any one or a combination of carbonates, acetates, super solid acids, hydroxides of alkaline earth metals, oxides of alkaline earth metals, and transition metal coordination compounds having alkoxy groups, etc., wherein the carbonates may include alkali metal carbonates, alkaline earth metal carbonates, transition metal carbonates, etc.; the acetates may include alkaline earth metal acetates, transition metal acetates, etc.
[0054] Finally, an alcoholysis reaction is carried out. The alcoholysis reaction can be carried out in a device with heating, heat preservation, stirring and condensation reflux functions, or in a microwave radiation heating device (reference patent CN112940344A). Any existing technology that can depolymerize PET into BHET is applicable.
[0055] As a preferred embodiment, the molar ratio of the waste PET product to the ethylene glycol is 1:6-10.
[0056] As a more preferred embodiment, the reaction temperature of the alcoholysis reaction is 230° C. to 250° C.; wherein, by controlling the conditions of the alcoholysis reaction, side reactions can be reduced to a certain extent.
[0057] As a preferred embodiment, the alcoholysis reaction time is 2 hours to 4 hours, wherein the alcoholysis reaction time can be adjusted according to the activity of the catalyst and the amount of the reaction raw materials.
[0058] The step of cooling and crystallizing to obtain the BHET-containing crystal is to cool and crystallize the alcoholysis solution containing BHET obtained in the previous step, and then perform solid-liquid separation to remove some impurities soluble in ethylene glycol.
[0059] As a preferred embodiment, the temperature of the cooling crystallization is 8-10° C.; the time of the cooling crystallization can be adjusted according to the specific amount of the alcoholysis solution.
[0060] In the steps of reduced pressure sublimation and condensation collection,
[0061] First, it is necessary to prepare a device for decompression sublimation and condensation collection. According to the need, decompression sublimation can be performed first, and BHET can be condensed and collected after gas is collected. It can also be performed simultaneously, and it is preferably performed simultaneously to save time. Therefore, we preferably have a device with a vacuum heating unit and a condensation collection unit. Wherein, the crystals containing BHET obtained in the above steps are continuously heated in the vacuum heating unit of the device, and BHET undergoes a solid-to-gas phase transition during this process. When the gas phase BHET contacts the condensation unit in the device, it undergoes a gas-to-solid phase transition again. Due to the difference in the physicochemical properties of BHET and a small amount of other by-products, a relatively pure target product BHET is finally obtained.
[0062] Secondly, it is necessary to explore the conditions of reduced pressure sublimation. As a preferred embodiment, the reduced pressure sublimation is carried out at a temperature of 110-140°C and a vacuum degree of 5-15 torr. Under this condition, the crystalline BHET is converted into a gaseous state, but other dye molecules and impurities after alcoholysis catalysis reaction do not sublimate at this temperature.
[0063] As a more preferred embodiment, the sublimation under reduced pressure is carried out at a temperature of 130-140° C. and a vacuum degree of 8-12 torr.
[0064] To make the technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below with reference to the accompanying drawings.
[0065] Example 1
[0066] 1) 1.5 g of waste polyester textiles (PET content 100%, colorant disperse yellow 6GFS) that had been pretreated by washing, drying and slicing were put into a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, the textiles were cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET (such as Figure 1 shown).
[0067] 2) The above-mentioned BHET-containing crystals were placed in a vacuum environment of 10 torr and heated continuously to 138°C, BHET sublimated, and high-purity BHET was collected on a condenser at 25°C (the nuclear magnetic resonance analysis spectrum of the product BHET is shown in Figure 2 The yield was 84.5%. The purity of HPLC was 98.2% (the HPLC analysis spectrum of BHET is shown in Figure 3 The whiteness (L value) is 99.1 (the whiteness test L, a, b values of BHET are shown in Figure 4 shown).
[0068] Example 2
[0069] 1) 1.5 g of waste polyester textiles (PET content of 94%, cotton content of 6%, colorant of direct dark green SBL) after pretreatment such as washing, drying and slicing were put into a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, the textiles were cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET (such as Figure 5 shown).
[0070] 2) The obtained BHET-containing crystals were placed in a vacuum environment of 10 torr and heated continuously to 138°C, BHET sublimated, and high-purity BHET was collected on a condenser at 25°C (the nuclear magnetic resonance analysis spectrum of BHET is shown in Figure 6 The yield was 83.2%. The purity of HPLC was 99.2% (the HPLC analysis spectrum of BHET is shown in Figure 7 The whiteness (L value) is 98.1 (the whiteness test L, a, b values of BHET are shown in Figure 8 shown).
[0071] Example 3
[0072] 1) 1.5 g of waste polyester textiles (PET content of 93%, spandex content of 7%, colorant dispersed turquoise S-GL) that had been pretreated by washing, drying and slicing were put into a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, the textiles were cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET (such as Fig. 9 shown).
[0073] 2) The obtained BHET-containing crystals were placed in a vacuum environment of 10 torr and continuously heated to 138°C, BHET sublimated, and high-purity BHET was collected on a condenser at 25°C (the nuclear magnetic resonance analysis spectrum of BHET is shown in Fig.10 The yield was 83.8%. The purity of HPLC was 99.7% (the HPLC analysis spectrum of BHET is shown in Fig.11 The whiteness (L value) is 97.2 (the whiteness test L, a, b values of BHET are shown in Fig.12 shown).
[0074] Example 4
[0075] 1) 1.5 g of pre-treated waste polyester textiles (from the same source as in Example 1) after washing, drying and slicing were put into a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, the textiles were cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET;
[0076] 2) The obtained BHET-containing crystals were placed in an environment with a vacuum degree of 8 torr and continuously heated to 138°C, BHET sublimated, and high-purity BHET was collected on a condenser at 25°C. The yield was 82.1%. The HPLC purity was 99.4% after testing. The whiteness (L value) was 98.0.
[0077] Example 5
[0078] 1) 1.5 g of pre-treated waste polyester textiles (from the same source as in Example 1) after washing, drying and slicing were put into a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, the textiles were cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET;
[0079] 2) The obtained BHET-containing crystals were placed in an environment with a vacuum degree of 8 torr and continuously heated to 110° C., and BHET sublimated. High-purity BHET was collected on a condenser at 25° C. The yield was 80.2%. The HPLC purity was 99.6% after testing. The whiteness (L value) was 97.9.
[0080] Example 6
[0081] 1) 1.5 g of a PET plastic bottle that had been pre-treated by washing, drying and slicing was placed in a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, the bottle was cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET;
[0082] 2) The above-mentioned crystal containing BHET was placed in a vacuum environment of 10 torr and continuously heated to 138°C, BHET sublimated, and high-purity BHET was collected on a condenser at 25°C. The yield was 84.6%. The HPLC purity was 99.8% after testing. The whiteness (L value) was 98.4.
[0083] Example 7
[0084] 1) 1.5 g of PET film that had been pre-treated by washing, drying and slicing was placed in a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, it was cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET;
[0085] 2) The above-mentioned crystal containing BHET was placed in an environment with a vacuum degree of 10 torr and continuously heated to 138°C, BHET sublimated, and high-purity BHET was collected on a condenser at 25°C. The yield was 84.0%. The HPLC purity was 99.3% after testing. The whiteness (L value) was 98.0.
[0086] Comparative Example 1
[0087] 1) 1.5 g of pre-treated waste polyester textiles (from the same source as in Example 1) after washing, drying and slicing were put into a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, the textiles were cooled and crystallized at a temperature of 8 to 10° C. for 12 h to obtain a crystal containing BHET;
[0088] 2) The obtained BHET-containing crystals were placed in a vacuum sublimator with a vacuum degree of 10 torr and the temperature was continuously raised to 195° C., and BHET was collected on a condenser at 25° C. The BHET crystals were polycondensed, and the yield was <5%.
[0089] Comparative Example 2
[0090] 1) 1.5 g of pre-treated waste polyester textiles (from the same source as in Example 1) after washing, drying and slicing were placed in a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, ethylene glycol was removed by vacuum distillation to obtain a solid powder containing BHET.
[0091] 2) The obtained solid powder was placed in a vacuum sublimator with a vacuum degree of 10 torr and the temperature was continuously raised to 138° C., and BHET was collected on a condenser at 25° C. The yield was <5%.
[0092] Comparative Example 3
[0093] 1) 1.5 g of pre-treated waste polyester textiles (from the same source as in Example 1) after washing, drying and slicing were placed in a reaction vessel containing 9 mL of ethylene glycol and 0.03 g of potassium carbonate, and alcoholyzed at 250° C. for 2.5 h under normal pressure and nitrogen protection. After the depolymerization reaction was complete, ethylene glycol was removed by vacuum distillation to obtain a solid powder containing BHET.
[0094] 2) The obtained solid powder was placed in a vacuum sublimator with a vacuum degree of 10 torr and the temperature was continuously raised to 138° C., and BHET was collected on a condenser at 25° C. The yield was <5%.
[0095] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for chemically recovering waste PET products by utilizing the phase change properties of BHET crystals, characterized in that: The following steps are involved: The waste PET products and the catalyst are mixed in ethylene glycol to carry out alcoholysis reaction to obtain alcoholysis solution; Cooling the alcoholysis solution to crystallize to obtain a BHET-containing crystal; Subliming the crystals under reduced pressure; Condensing and collecting BHET; Wherein, the reduced pressure sublimation is carried out at a temperature of 110 to 140° C. and a vacuum degree of 5 to 15 torr; The condensation temperature is 25°C to 30°C; The reaction temperature of the alcoholysis reaction is 230°C to 250°C; The molar ratio of the waste PET product to the ethylene glycol is 1:6-10; The cooling crystallization temperature is 8 to 10°C; The catalyst is an alkali metal carbonate.
2. The chemical recovery method according to claim 1, characterized in that: The reaction time of the alcoholysis reaction is 2h to 4h.
3. The chemical recovery method according to claim 1, characterized in that: The mass ratio of the waste PET product to the catalyst is 1:0.02-0.
1.
4. The chemical recovery method according to claim 1, characterized in that: The cooling crystallization time is 8 to 12 hours.
5. The chemical recovery method according to claim 1, characterized in that: The waste PET products are at least one of waste polyester textiles, PET plastic bottles and PET films.
6. The chemical recovery method according to claim 1, characterized in that: Before the waste PET product is mixed with the catalyst, the pretreatment steps of impurity removal, crushing and granulation are also included.
Citation Information
Cited By
Polyol gradient synergistic depolymerization-esterification coupling reaction device for chemical recovery of PETG (Polyethylene Terephthalate Glycol)
CN121972124A