A process for improving the recovery rate of B and Nb in boron-containing heat-resistant steel
By optimizing the electroslag remelting process and smelting conditions in heat-resistant steel metallurgy, the B and Nb burn loss problems are solved, their yield and yield are improved, and the high-temperature performance and stability of the material are improved.
Patent Information
- Application Number
- CN202310007517.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-01-04
AI Technical Summary
In steel metallurgy, the burn loss problem of B and Nb in heat-resistant steel causes large fluctuations in its yield rate, which is difficult to stabilize and control, affecting the material yield and high-temperature service performance.
By measuring the acid-soluble boron content, the electroslag remelting process is optimized, and the electroslag remelting is used to use CaF2, Al2O3, B2O3 ternary slag systems and protective atmosphere to control the boron oxide and toner content, and the smelting conditions are adjusted to suppress B and Nb Oxidation and nitriding burn, and the composition uniformity is improved through high-temperature homogenization and annealing treatment.
It effectively suppresses the burn loss of B and Nb, improves its yield rate, achieves the stability of yield rate and the improvement of high-temperature performance, and enhances the market competitiveness of the materials.
Smart Images

Figure CN116121624B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a process for improving the yield of B and Nb in boron-containing heat-resistant steel. Background Art
[0002] Boron (B) is an important strengthening element in steel. Depending on the amount added, the material exhibits different performance characteristics. Adding a small amount of B (≤10ppm) to alloy structural steel can significantly improve the hardenability of the steel; adding 0.01-0.03% B to heat-resistant steel can improve the long-term service performance of the material at high temperatures (improve high-temperature durability and creep performance); and when the B content is ≥1%, the B-containing compounds at the grain boundary will form a network structure, deteriorating the processing performance of the material. This type of material can shield high-energy neutrons and is mostly used in the nuclear power field. Patent CN111270125A proposes a smelting method for heat-resistant steel for steam turbines, which is used to achieve stable control of the B element, including vacuum carbon deoxidation refining, adding B-Fe before long steel, controlling the mold filling rate (d = (0.55 ~ 0.85) D, D is the diameter of the crystallizer), electroslag remelting under a protective atmosphere, using CaF2 40 ~ 55 / Al2O 15 ~ 30 / MgO 2 ~ 5 / CaO 20 ~ 30 / ZrO 0.5 ~ 3 five-element slag system, controlling the final oxygen content of the steel billet and other methods to achieve stable control of the B element. It emphasizes the preservation of boron by controlling oxygen, and adding additional B during the ESR process to inhibit burning (the added B-Fe replaces the B in the steel billet, which is oxidized and burned during the ESR process). The problem of nitriding burning is not fully considered.
[0003] Patent CN111057827A relates to a method for regulating the distribution of B element in heat-resistant steel 9Cr3W3CoB by heat treatment + hot deformation process, the steps include: heating the workpiece to 1150-1200℃, keeping warm for 1.5-2h; rolling for 5-7 times, controlling the deformation of each time to less than 20%, and the total deformation to 60-90%, and then air cooling; air cooling at 750-780℃ for 1-2h. The purpose is to dissolve all the borides and make the B element appear in the matrix. Patent CN108004486A relates to a composition optimization scheme for high-strength heat-resistant steel, which improves the creep strength and high-temperature durability of the material by improving the composition ratio (especially increasing the B content in the steel) and smelting process conditions (such as melting and refining temperature, etc.). The main discussion is the influence of composition control (B%) on the high-temperature service performance of heat-resistant steel.
[0004] B in steel can be roughly divided into acid-soluble boron and non-acid-soluble boron. Acid-soluble boron includes B in the form of solid solution, free state, carboride and oxide; non-acid-soluble boron is mainly BN. Except for a small amount of B in the form of solid solution, most of the B in steel enters the grain boundary in the form of free state or compound. Some B combines with the grain boundary carbide M23C6 to form a more stable structure M23(C,B)6, which can inhibit the growth of carbides (Ostwald ripening). B2O3 exists in the form of brittle oxide inclusions. A small amount of small size can play a pinning role and inhibit grain growth. Large-sized inclusions may form crack sources under the action of external loads, seriously affecting the plasticity and toughness of the material. BN acts similarly to MnS and can improve the cutting performance of the material.
[0005] 2. Key process links prone to B and Nb burning
[0006] As the B content in steel increases, the problem of B element burning during smelting becomes increasingly prominent. In production practice, it is found that B burning in heat-resistant steel mainly occurs during the electroslag remelting process. When B burning is serious, other easily oxidized elements in the heat-resistant steel, such as Nb, will also be lost in large quantities. How to suppress B burning is a common problem faced in the smelting of such high-alloy steels.
[0007] To address this problem, the conventional approach is to increase the proportion of B in molten steel during smelting, leaving a burn-off margin so that after ESR (electroslag remelting) treatment, the final composition of B falls within the required range. However, in practice, it is found that the B yield is not a fixed value, but is directly and indirectly affected by multiple factors such as the front-end smelting process conditions, electrode rod composition and organizational uniformity, and the state of electroslag equipment. The B yield will fluctuate violently between 40% and 90%, and it is difficult to achieve stable control simply by reserving a burn-off margin during batching. How to stabilize and improve the B yield is the key to achieving stable control of the heat-resistant steel composition and improving the yield.
[0008] 3. Electroslag burning mechanism of B and Nb
[0009] First of all, it is necessary to clarify the burning mechanism of B and why a large amount of B element is lost during the electroslag process.
[0010] By combing through the burning mechanism of B element, it is found that B has high chemical activity at high temperature, and B element in steel is mainly burned through two ways: oxidation and nitridation. B can react with O in steel to form oxides (boron oxides in molten steel are variable valence oxides, which exist in various forms such as B2O2, B2O3, etc.), and can also react with N to form BN with stable structure. In smelting, the oxidation activity of B is higher than that of Mn and Si, but lower than that of Ti and Al. In the smelting process, B reacts preferentially with O to produce oxides, and if the boron oxides cannot be reduced in time, they are easily adsorbed by the slag, resulting in the loss of boron element. In the solidification process, B reacts with N to form a stable compound BN. According to the Gibbs free energy of the chemical reaction, the binding ability of B and N in the smelting process is greater than that of Al, but lower than that of Ti and Zr.
[0011] Combination Figure 1a and Figure 1b In the temperature range of 700-1700℃, Al, Ti, Si react with oxygen before B; Ti reacts with nitrogen before B; in the range of 1500-1700℃, B reacts with nitrogen before Al, and in the range of >1700℃, the opposite is true. (It can be seen that during the smelting process, elements such as Al, Si, and Ti can inhibit the oxidation and burning of B, while Ti (or Zr) can inhibit the nitridation and burning of B. By optimizing the alloy composition and adjusting the denitrification system during smelting, the formation of B oxides and nitrides can be effectively inhibited.
[0012] B oxide is mainly formed during the smelting process. At a higher temperature, B directly reacts with O in the molten steel to form oxide. The size, distribution and morphology of B oxide are directly affected by the oxygen content in the steel. The higher the oxygen content, the more B oxide inclusions are formed and the larger the size. BN is generally formed during the non-equilibrium solidification process during casting, and segregates at the grain boundary, and is easy to form a composite structure with other types of inclusions. The morphology and size of the BN precipitate phase are affected by the solidification rate. When the solidification rate of the steel billet is high, BN is a dispersed distribution of small-sized particles; when the solidification rate is low, the size of the BN particles increases, and it is easy to agglomerate to form a large-sized cluster structure (ISIJ International, Vol. 46 (2006), No. 11, pp. 1712–1719). The electroslag remelting process has a good removal effect on large-sized inclusions. When the size of BN and B2O3 inclusions in the electrode rod is too large, they are easily filtered out by the slag during the ESR process.
[0013] During the ESR process, the easily burnable elements in steel (such as B, Al, Ti, etc.) are easily oxidized and burned, that is, the oxygen in the electroslag atmosphere diffuses into the metal molten pool through the slag layer, reacts with such elements to form oxidized inclusions, and enters the slag layer through agglomeration and floating. Even if a protective atmosphere (Ar atmosphere) is used, it is difficult to completely isolate the impurity gas from mixing into the atmosphere. The gas close to the slag in the crystallizer expands due to heat, and forms convection with the gas with a lower temperature at the exhaust port, which may bring external impurity gas into the crystallizer. In addition, the equipment status such as the airtightness of the crystallizer is also an important influencing factor.
[0014] Experimental studies have found that the burning of Nb is directly related to the oxygen content in the atmosphere during the electroslag remelting process. When oxygen is mixed into the protective atmosphere, the burning of Nb in the heat-resistant steel will be aggravated. In particular, when the protective gas mixed with oxygen continues to enter the crystallizer, the burning of Nb is more serious. Summary of the invention
[0015] The present invention aims to provide a process for improving the recovery rate of B and Nb in boron-containing heat-resistant steel. To achieve the above object, the present invention provides the following technical solutions:
[0016] A process for improving the recovery rate of B and Nb in boron-containing heat-resistant steel, the method comprising:
[0017] By measuring the acid-soluble boron content in the boron-containing and nitrogen-containing heat-resistant steel electrode base material, it is determined whether the acid-soluble boron content in the heat-resistant steel ingot meets the predetermined range;
[0018] When the content of acid-soluble boron in the heat-resistant steel ingot meets a predetermined range, the heat-resistant steel ingot is subjected to an electroslag remelting treatment, and mixed slag is used as an electroslag slag material, wherein the electroslag slag material comprises a ternary slag system of CaF2, Al2O3, B2O3 and carbon powder;
[0019] The electroslag remelting is carried out in a protective atmosphere, with a filling ratio of d=(0.6-0.8)D, where D is the diameter of the crystallizer; the electroslag melting rate is controlled at 7-11 kg / min.
[0020] Furthermore, in the electroslag slag material, the content of boron oxide is 1.0-1.2%, and the content of carbon powder is 0.1-0.15%.
[0021] The electroslag slag material is fully baked at 850±20° C. for 12 to 16 hours before use.
[0022] Further, the measurement of the acid-soluble boron content in the boron-containing and nitrogen-containing heat-resistant steel electrode base material includes:
[0023] Take multiple sets of drill cuttings samples from the head and tail of the boron-containing heat-resistant steel electrode base material;
[0024] Weigh 1-2g of drill cuttings sample for each group and dissolve the sample with 1% strong acid solution;
[0025] When the sample is fully dissolved, filter it through filter paper; let it stand for a while, take the supernatant after the solution is separated, and dilute it to a concentration of 10%; take 20 ml of the diluted solution and inject it into the separatory funnel;
[0026] preparing a boron ion extractant, wherein the boron ion extractant is a solution of 2-ethyl-1,3-hexanediol and chloroform in a volume ratio of 1:120;
[0027] Pour the extractant into the separatory funnel, seal it, and shake it for 3-5 min; after standing, take the supernatant and dilute it to 10% concentration;
[0028] The B content in the diluted supernatant, i.e., the acid-soluble boron content in the boron- and nitrogen-containing heat-resistant steel electrode base material, is obtained by ICP detection.
[0029] Furthermore, the total boron content in the electrode base material was obtained by spark direct reading;
[0030] The content of non-acid-soluble boron in the heat-resistant steel ingot is obtained by subtracting the acid-soluble boron content in the boron-containing and nitrogen-containing heat-resistant steel electrode base material from the total boron content.
[0031] Furthermore, the method further comprises:
[0032] When the content of acid-soluble boron in the heat-resistant steel ingot is lower than the predetermined range, the electrode rod is subjected to high-temperature homogenization treatment: the homogenization heat treatment temperature is 1050-1080°C, and the insulation time is 10-15h; after the homogenization treatment, it is cooled to 300°C in the furnace and then air-cooled.
[0033] Further, electroslag remelting is performed using a protective atmosphere, including
[0034] During electroslag remelting using protective atmosphere, the O2 content is ≤0.04%;
[0035] For heat-resistant steel ingots with a total weight of ≤3t, the electroslag melting rate is controlled at 7-9kg / min; for heat-resistant steel ingots with a total weight of ≥3t, the electroslag melting rate is controlled at 9-11kg / min.
[0036] Furthermore, the method further comprises:
[0037] After electroslag remelting, the electroslag ingot is left to stand in the crystallizer for 1 to 2 hours before being tapped, hood-cooled for 24 to 36 hours, and then annealed at 750 to 800°C for 24 to 30 hours.
[0038] Furthermore, obtaining the heat-resistant steel ingot includes:
[0039] Raw material pretreatment: Shot blast the alloy raw materials to completely remove the oxide scale, and weigh them for later use;
[0040] Loading and melting: Load the alloy raw materials into the crucible in a loose upper and tight lower manner, close the furnace and evacuate, wait until the vacuum degree of the melting chamber is lower than 20Pa, then turn on the power to start melting, take samples for analysis after the alloy is completely melted, and fine-tune the composition in the furnace;
[0041] Vacuum carbon deoxidation refining: heat up to the refining temperature, refining for 50 to 80 minutes in a vacuum environment, add deoxidizer, take samples for analysis after melting, then add Nb-Fe and V-Fe respectively and stir;
[0042] Add ferroboron and pour steel: Add N-Cr and sponge Ti and stir, add B-Fe, Mn and Al after they are melted, fill in inert gas to increase the pressure in the furnace and control the steel tapping temperature range at 1550-1600℃, and pour at a predetermined speed to obtain heat-resistant steel ingots.
[0043] Furthermore, the raw material components of the heat-resistant steel ingot include, by mass percentage (%): C: 0.09-0.11, Mn: 0.4-0.5, Si: ≤0.1, P: ≤0.015, S: ≤0.01, Cr: 11-11.5, Ni: 0.3-0.7, Mo: 0.1-0.4, Co: 2.5-3.5, W: 2.4-3, V: 0.2-0.24, Nb: 0.08-0.14, N: 0.013-0.02, B: 0.012-0.16, Al: 0.01-0.015, Ti: 0.01-0.02, and the rest is Fe except for a small amount of impurity elements.
[0044] Furthermore, during the vacuum carbon deoxidation refining process, the oxygen content in the electrode base material is controlled to be ≤30ppm.
[0045] Technical effects and advantages of the present invention:
[0046] To inhibit B burning loss, we mainly reduce the precipitation of B2O3 and BN in steel, adjust the morphology of the precipitated phase to avoid the appearance of large-sized B oxides or nitrides, and reduce the loss of B in the form of compounds during the ESR process from three aspects:
[0047] (1) Ingredient optimization:
[0048] Effect of oxygen and nitrogen content:
[0049] The simulation of boron-nitrogen-containing heat-resistant steel found that the boron oxide (such as B2O3) in the steel is affected by the oxygen content. When the oxygen content is ≤40ppm, B2O3 will not appear, but when the oxygen content is greater than 50ppm, it will begin to appear (such as Figure 2a shown).
[0050] When heat-resistant steel contains both B and N, BN is easily formed. As the N content increases, the number of BN inclusions increases and the size gradually increases. According to reports in the literature, the B and N content in 9-12% Cr heat-resistant steel and the formation of BN follow the following rules (such as Figure 2b ):
[0051] lg[B]=-2.45lg[N]-6.81
[0052] When the B and N contents in the steel satisfy (or are close to) this relationship, that is, the B and N contents in the heat-resistant steel composition are distributed in Figure 3 When it is near the middle oblique line, the precipitated BN is mainly dispersed small-sized particles; when the components are distributed in the upper right area of the oblique line, BN mostly appears in the form of large-sized agglomerates; when distributed in the lower left area, no BN precipitates.
[0053] When optimizing the composition of boron-containing heat-resistant steel, the B and N contents should be kept as low as possible. Figure 3 For heat-resistant steel containing both boron and nitrogen, the composition should be kept close to the oblique line in the figure to avoid the formation of BN cluster structure.
[0054] (2) Optimization of billet casting process
[0055] The solidification rate of the steel billet is another factor affecting the BN morphology. In order to suppress the BN cluster structure, the solidification rate of the steel billet should be increased as much as possible to reduce the component segregation. In actual production, it is possible to consider appropriately lowering the casting temperature and using auxiliary cooling methods, such as using a high-power fan to blow air into the ingot mold to assist in heat dissipation, etc.
[0056] (3) Characterization of non-acid-melted boron content in electrode rods
[0057] B oxide inclusions can be suppressed by strict oxygen control, while BN inclusions have high requirements for composition and process control. Generally, in boron- and nitrogen-containing steels, the B and N contents are limited by the control range of the steel grade composition; and the actual controllable range of the solidification rate is also limited, especially for large ingots, which are difficult to cool quickly. Therefore, it is necessary to understand the relative BN content of the electrode rod before electroslag remelting for subsequent process formulation and optimization.
[0058] Based on the stable structure of BN, the electrode rod scraps are treated with acid and the filtered solution (or insoluble precipitate) is quantitatively analyzed for composition. The proportion of B in the form of BN in the total B content can be obtained. When the remaining B content is in the upper limit of the composition control range after deducting the BN proportion, electroslag remelting can be carried out directly according to the general process flow. When the remaining B content is lower than the lower limit, the process needs to be adjusted.
[0059] (4) ESR process inhibits the loss of B and Nb
[0060] In view of the high proportion of BN in the electrode rod, three measures are taken to inhibit the burning of B and Nb and the loss of B. The first is to improve the purity of the Ar protective atmosphere and reduce the proportion of impurity gas O2, so as to avoid the oxidation and burning of B and Nb during the electroslag remelting process. Then the slag system is adjusted to increase the B content in the slag by changing the slag system composition. 3+ The relative content of B in the steel can be used to delay or inhibit the diffusion of B oxides and nitrides into the slag (i.e., reduce the B content gradient between the slag and the molten metal). The third is to optimize the process conditions: through the aforementioned process, the B oxides or nitrides in the electrode rods are usually small in size and more dispersed, while the diffusion, agglomeration and floating of inclusions in the ESR process require a certain amount of time. By appropriately accelerating the solidification rate of the electroslag molten pool, the diffusion trend of B compounds into the slag pool can be inhibited, and the component segregation in the electroslag ingot can be reduced.
[0061] The present invention starts from two aspects: inhibiting the precipitation of B compounds in steel and reducing the loss of B through ESR slag during smelting. By optimizing the composition, appropriately reducing the pouring temperature to increase the solidification rate of the steel billet, using Ar atmosphere and low O2 environment for electroslag remelting, especially using CaF2 / Al2O3 / B2O3 ternary slag system for electroslag remelting treatment. It has a significant effect on improving the boron element recovery rate in the electroslag remelting process of boron-containing and nitrogen-containing steel (especially steel with relatively high boron content), which is conducive to improving the finished product rate of such steel.
[0062] This invention can improve the recovery rate of B element in boron- and nitrogen-containing heat-resistant steel, realize stable control of B and Nb elements, and effectively avoid product composition incompatibility caused by excessive burning of B and Nb. By improving the yield rate and quality stability of such high-value steel production, it helps to improve the reputation of the product among users and increase the market share of such products.
[0063] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1a is the ΔGθ-T relationship of the element oxidation reaction;
[0065] Figure 1b is the ΔGθ-T relationship of the element nitridation reaction;
[0066] Figure 2a The effect of the change of O content in boron-nitrogen-containing heat-resistant steel on the precipitation of B2O3;
[0067] Figure 2bThe effect of the change of N content in boron-nitrogen-containing heat-resistant steel on BN precipitation;
[0068] Figure 3 is the relationship between B, N content and BN precipitation;
[0069] Figure 4 The present invention is a flow chart of the process for improving the recovery rate of B and Nb in boron-containing heat-resistant steel. DETAILED DESCRIPTION
[0070] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0071] In order to solve the shortcomings of the prior art, the present invention discloses a process method for improving the recovery rate of B and Nb in boron-containing heat-resistant steel. The method comprises: by measuring the acid-soluble boron content in the boron-containing and nitrogen-containing heat-resistant steel electrode base material, judging whether the acid-soluble boron content in the heat-resistant steel ingot meets a predetermined range; when the acid-soluble boron content in the heat-resistant steel ingot meets the predetermined range, performing electroslag remelting treatment on the heat-resistant steel ingot, and using mixed slag as electroslag slag material, the electroslag slag material comprises boron oxide and carbon powder; using protective atmosphere for electroslag remelting, the filling ratio d=(0.6-0.8)D, D is the diameter of the crystallizer; and controlling the electroslag melting rate at 7-11kg / min.
[0072] In a specific embodiment of the present invention, when the content of acid-soluble boron in the heat-resistant steel ingot is in the range of 0.01 to 0.25%, the heat-resistant steel ingot is directly subjected to electroslag remelting treatment; when the content of acid-soluble boron in the heat-resistant steel ingot is lower than 0.01%, the electrode rod is subjected to high-temperature homogenization treatment: the homogenization heat treatment temperature is 1050 to 1080°C, and the insulation time is 10 to 15 hours; after the homogenization treatment, the heat-resistant steel ingot is cooled to 300°C in the furnace and then air-cooled, and then the heat-resistant steel ingot is subjected to electroslag remelting treatment.
[0073] In a specific embodiment of the present invention, Figure 4 As shown, the method of the present invention comprises the following steps:
[0074] Raw material pretreatment: Shot blast the alloy raw materials to completely remove the oxide scale, and weigh them for later use;
[0075] Loading and melting: Load the alloy raw materials into the crucible in a loose upper and tight lower manner, close the furnace and evacuate, wait until the vacuum degree of the melting chamber is lower than 20Pa, then turn on the power to start melting, take samples for analysis after the alloy is completely melted, and fine-tune the composition in the furnace;
[0076] Vacuum carbon deoxidation refining: heat up to the refining temperature, refining for 50 to 80 minutes in a vacuum environment, add deoxidizer, take samples for analysis after melting, then add Nb-Fe and V-Fe respectively and stir;
[0077] Add ferroboron, steel pouring: Add N-Cr and sponge Ti and stir, add B-Fe, Mn and Al after they are melted, fill with inert gas to increase the pressure in the furnace and control the steel tapping temperature range
[0078] 1550~1600℃, low speed pouring to obtain heat-resistant steel ingots.
[0079] Detection of non-acid molten boron content in heat-resistant steel ingots
[0080] The acid-soluble boron content in the boron- and nitrogen-containing heat-resistant steel electrode base material is obtained by combining dissolution, filtration, B ion extraction and ICP plasma spectroscopy; the total boron content in the electrode rod is obtained by spark direct reading; the non-acid-soluble boron content (BN) in the billet is obtained by subtracting the acid-soluble boron content from the total boron content. The non-acid-soluble boron content can be used to evaluate the amount of B burned during the ESR process of the billet, providing a reference for adjusting subsequent processes.
[0081] Electroslag remelting: high-purity Ar is used as the protective atmosphere, Ar 6-12min is introduced into the bottom of the crystallizer in advance, and it is ensured that the O2 content in the crystallizer is always ≤0.04% during the ESR process; the filling ratio d=(0.5-0.8)D, D is the diameter of the crystallizer (mm); the CaF2 69 / Al2O3 30 / B2O3 1 ternary slag system is used (the total slag amount is in the middle limit or lower limit of the equipment allowable range); the carbon powder content is 0.1-0.15%, and the present invention preferably adds 0.1% carbon powder to form a mixed slag; the slag material is fully baked at 850±20℃ for 12-16h before use, and is briefly stored in a 100℃ oven before use; for electrode rods ≤3t, the electroslag melting rate is controlled at 7-9kg / min, and for ingots ≥3t, at 9-11kg / mi n; After electroslag remelting treatment, the electroslag ingot is left to stand in the crystallizer for 1 to 2 hours before being tapped, hood cooled for 24 to 36 hours, and then annealed at 750 to 800°C for 24 to 30 hours.
[0082] In a specific embodiment of the present invention, the raw material components of the boron-containing nitrogen-containing heat-resistant steel are as follows in mass percentage (%): C: 0.08-0.13, Mn: 0.4-0.65, Si: ≤0.1, P: ≤0.01, S: ≤0.01, Cr: 10-12, Ni: 0.4-0.7, Mo: 0.15-0.4, Co: 2.5-3.3, W: 2.4-3, V: 0.1-0.25, Nb: 0.05-0.11, N: 0.01-0.3, B: 0.01-0.025, Al: ≤0.015, Ti: ≤0.05, and the rest is Fe except for a small amount of impurity elements.
[0083] The composition optimization scheme for suppressing B burning includes: N takes the middle limit of the composition (0.013-0.02%), and the target composition is 0.017%; B takes the upper limit of the composition (0.012-0.020%), and the target composition is 0.017%;
[0084] In a specific embodiment of the present invention, Al deoxidation is used to ensure that the residual Al in the molten steel before steel casting is within the range of 0.01-0.015%; and the oxygen content in the electrode base material is controlled to be ≤30ppm.
[0085] In a specific embodiment of the present invention, B is added in the form of Fe-B alloy before steelmaking, and Fe-B is remelted before use to make B in the alloy uniform and remove impurity elements and inclusions as much as possible; N is added in the form of nitrogen-containing alloy, and alloy raw materials with fewer impurities and more uniform composition are selected as much as possible; B and N are added separately, and it must be ensured that the added alloys are completely dissolved.
[0086] In a specific embodiment of the present invention, the acid-soluble boron content in the boron-containing and nitrogen-containing heat-resistant steel electrode base material is measured. The present invention adopts the following technical solution:
[0087] (1) Take drill cuttings samples (multiple groups of samples) from the head and tail of the boron-containing heat-resistant steel electrode base material, and try to avoid mixing iron oxide scale into the drill cuttings;
[0088] (2) Weigh 1-2 g of drill cuttings sample; prepare 1% (v / v) H2SO4 solution (or HNO3 solution) to dissolve the sample (for high-chromium refractory alloys, add an appropriate amount of H2O2 (20-30%) to aid dissolution);
[0089] (3) When the sample is fully dissolved, filter it through filter paper; let it stand for a while until the solution separates into layers, take the supernatant, and dilute it to a concentration of 10%; take 20 ml of the diluted solution and inject it into a polypropylene separatory funnel;
[0090] (4) Prepare B ion extractant: 2-ethyl-1,3-hexanediol + chloroform in a volume ratio of 1:120; inject the extractant into a separatory funnel, seal it, and shake it well (3 to 5 min); let it stand for a while until the solution is mixed and separated into layers, and the supernatant is diluted to a concentration of 10% (corrosion residues can also be separated by centrifuge);
[0091] (5) Using ICP to detect the boron content in the diluted supernatant and infer the acid-soluble boron content in the electrode matrix; obtaining the total boron content in the electrode matrix by spark direct reading; and obtaining the non-acid-soluble boron content (BN with large particles or cluster structures) by subtracting the acid-soluble boron from the total boron content;
[0092] (6) The non-acid-soluble boron content obtained is the B burned after the heat-resistant steel is treated with electroslag remelting. Compare the acid-soluble boron content with the control range of the B content in the steel. If the two coincide, the steel is treated according to the conventional ESR process; if they do not coincide, make targeted process adjustments to make the B content meet the requirements;
[0093] (7) If the test finds that the proportion of non-acid soluble boron in the steel billet is too high and the non-acid soluble boron content is lower than the composition control range, the electrode rod needs to be subjected to high-temperature homogenization treatment. The heat treatment temperature is affected by the material composition and phase change temperature. The lower limit temperature of the austenite and delta ferrite two-phase interval (temperature range) of 1050-1080°C is selected as the homogenization heat treatment temperature. The holding time is affected by the size of the steel billet and is controlled at 10-15h. After homogenization treatment, it is cooled to 300°C in the furnace and then air-cooled.
[0094] The scheme of the present invention is further described below in conjunction with examples, but the present invention is not limited thereto.
[0095] Example 1
[0096] A process for inhibiting the burning loss of boron element in boron-containing and nitrogen-containing heat-resistant steel, the steps of which include:
[0097] 1) Raw material pretreatment: The alloy raw materials are shot blasted to remove the surface oxide scale, weighed according to the composition range and then loaded into the vacuum induction furnace respectively. The composition is shown in Table 1 (V-Fe and B-Fe are remelted in the vacuum induction furnace before use):
[0098] Table 1 Composition control range (wt%) of boron- and nitrogen-containing heat-resistant steel 10Cr11Co3W3NiMoVNbNB
[0099]
[0100] 2) First, Fe, Fe-Ni, Fe-Cr, Co, Mo-Fe, and W-Fe alloy materials are loaded into the crucible; the furnace is evacuated to below 20Pa and power is supplied;
[0101] 3) After the alloy is melted, take samples for analysis and make fine adjustments to the composition in the furnace to ensure that the main components are within the control range;
[0102] 4) Refining is performed for 50 to 60 minutes in a vacuum environment, and a deoxidizer is added after the refining is completed. Samples are taken for analysis after melting, and then Nb-Fe and V-Fe are added respectively and stirred;
[0103] 5) Add N-Cr and stir it. After it is completely melted, add B-Fe and Mn. Fill with Ar gas to increase the pressure in the furnace and measure the temperature.
[0104] 6) The tapping temperature range is controlled at 1550-1590°C, and the cast billet (heat-resistant steel ingot) is about 150kg;
[0105] 7) After the billet solidifies, remove the riser end and the nozzle end and treat the surface, and take drill cuttings samples from the head and tail of the billet;
[0106] 8) Weigh and acid dissolve the drill cuttings; filter after the drill cuttings are completely dissolved, and perform ICP component analysis on the solution; compare the B content (acid-soluble boron) in the solution and the total boron content in the steel billet (detected by spark direct reading), and indirectly obtain the proportion of non-acid-soluble boron (BN);
[0107] 9) When the proportion of non-acid soluble boron is too high, that is, the proportion of acid soluble boron is lower than the composition control range, the steel billet is subjected to high temperature homogenization treatment at 1080°C for 10 hours; after the treatment, the steel billet is cooled to room temperature with the furnace;
[0108] 10) Welding dummy electrodes to make electrode rods and charging the electroslag furnace;
[0109] 11) Before electroslag remelting, check the air tightness of the equipment, introduce 5-10min Ar into the crystallizer in advance, and ensure that the O2 content in the crystallizer is less than 0.4% under Ar protective atmosphere;
[0110] 12) Using CaF2 69 / Al2O3 30 / B2O3 1 ternary slag system, the total slag amount is 15kg, and 0.1% carbon powder is added to the slag to form a mixed slag, wherein the mixed slag is baked at 850±20℃ for 6-8h before use;
[0111] 13) Use Benxi Steel materials as arc starter to carry out electroslag remelting treatment, and control the electroslag melting rate at 7-9 kg / min;
[0112] 14) The steel billet is cooled in the furnace for 1 hour before being tapped out, hood cooled for 24 to 36 hours, and then annealed at 750 to 800°C for 24 to 30 hours.
[0113] The steel billet before and after ESR treatment was fully inspected and the B yield was calculated:
[0114] Table 2. Composition of 10Cr11Co3W3N iMoVNbNB before and after electroslag remelting (%)
[0115]
[0116] According to Table 2, the B yields in the heat-resistant steel ingots before ESR treatment are 82.7%, 71.8% and 77.4% respectively, and the B yields fluctuate greatly. By adopting the process method of the present invention, the B yield can be stably controlled within the range of 70-80% after ESR treatment, and the B yield is stable.
[0117] Embodiment 2:
[0118] Drill cuttings samples (drill cuttings below a certain depth on the surface of the steel billet) were taken from the 10Cr11Co3W3NiMoVNbNB electrode rod, and chemical dissolution and filtration were performed. As shown in Table 3, the acid-soluble boron content in the steel was measured by ICP; a block sample was taken from the same steel billet, and the surface was polished and the total B content in the spectrum was measured by spark direct reading (direct reading spectrum); the difference between the two values was the content of non-acid-soluble boron (BN). The average content of non-acid-soluble boron was about 0.01%.
[0119] For the same electrode rod, the B% before and after electroslag remelting was tested (total B content was measured), and the difference ΔB between the B content before and after electroslag treatment was calculated. The average value of ΔB was also 0.01%. Therefore, it is inferred that the B lost during electroslag remelting is mainly non-acid soluble boron. By measuring the non-acid soluble boron content before electroslag treatment, the amount of B burned in the billet can be roughly predicted, providing a reference for formulating electroslag process plans.
[0120] Table 3.10Cr11Co3W3NiMoVNbNB electrode rod acid-soluble boron (BN) content and B burnout (ΔB) before and after electroslag remelting
[0121]
[0122] Embodiment 3:
[0123] The electroslag remelting test of 150kg 10Cr11Co3W3NiMoVNbNB electrode rod was carried out in the laboratory to compare the changes of easily burned elements in the billet before and after treatment, and calculate the element recovery rate. The diameter of the electrode rod is Φ150mm, and the inner diameter of the crystallizer is Φ220mm; the electroslag slag system is CaF2:Al2O3:B2O3 ternary slag system (using two ratios of 69.5:30:0.5 and 69:30:1 respectively), the total slag amount is 15kg; the electroslag melting rate is 6-7kg / min.
[0124] The composition comparison and element recovery rate of the easily burned elements before and after electroslag treatment of the steel billet are shown in Table 4. Among them, the B recovery rate reaches 66.67% and the Nb recovery rate reaches 79.65% by adding CaF2:Al2O3:B2O3=69.5:30:0.5; the B recovery rate is 84.21% and the Nb recovery rate is 98.96% by using the CaF2:Al2O3:B2O3=69:30:1 scheme, and the Al% decreases. In terms of the recovery rates of B and Nb, the CaF2:Al2O3:B2O3=69:30:1 slag system scheme has the best effect.
[0125] Table 4.10Cr11Co3W3NiMoVNbNB
[0126]
[0127] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A process for improving the recovery rate of B and Nb in boron-containing heat-resistant steel, It is characterized in that The method comprises, The raw materials are sequentially subjected to pretreatment, charging, melting, vacuum carbon deoxidation refining, adding ferroboron, and steel pouring to obtain heat-resistant steel ingots, wherein: The raw material components of the heat-resistant steel ingot include, by mass percentage (%): C: 0.09-0.11, Mn: 0.4-0.5, Si: ≤0.1, P: ≤0.015, S: ≤0.01, Cr: 11-11.5, Ni: 0.3-0.7, Mo: 0.1-0.4, Co: 2.5-3.5, W: 2.4-3, V: 0.2-0.24, Nb: 0.08-0.14, N: 0.013-0.02, B: 0.012-0.16, Al: 0.01-0.015, Ti: 0.01-0.02, and the rest is Fe except for a small amount of impurity elements; Vacuum carbon deoxidation refining: heat up to the refining temperature, refining for 50 to 80 minutes in a vacuum environment, add deoxidizer, take samples for analysis after melting, then add Nb-Fe and V-Fe respectively and stir; Add ferroboron and cast steel: Add N-Cr and sponge Ti and stir, add B-Fe, Mn and Al after they are melted, fill in inert gas to increase the pressure in the furnace and control the steel tapping temperature range at 1550-1600℃, and cast at a predetermined speed to obtain heat-resistant steel ingots; By measuring the acid-soluble boron content in the boron-containing and nitrogen-containing heat-resistant steel electrode base material, it is determined whether the acid-soluble boron content in the heat-resistant steel ingot meets the predetermined range; When the content of acid-soluble boron in the heat-resistant steel ingot meets a predetermined range, the heat-resistant steel ingot is subjected to electroslag remelting treatment, and mixed slag is used as the electroslag slag material, wherein the electroslag slag material includes a ternary slag system CaF 2 、Al 2 O 3 , B 2 O 3 and carbon powder; in the electroslag slag material, the content of boron oxide is 1.0-1.2%, and the content of carbon powder is 0.1-0.15%; The electroslag remelting is carried out in a protective atmosphere, and the filling ratio d = (0.6-0.8)D, where D is the diameter of the crystallizer; the electroslag melting rate is controlled at 7-11 kg / min. During the electroslag remelting process in a protective atmosphere, O 2 Content ≤ 0.04%; When the content of acid-soluble boron in the heat-resistant steel ingot is lower than the predetermined range, the electrode rod is subjected to high-temperature homogenization treatment: the homogenization heat treatment temperature is 1050-1080°C, and the insulation time is 10-15h; after the homogenization treatment, it is cooled to 300°C in the furnace and then air-cooled.
2. A process for improving the yield of B and Nb in boron-containing heat-resistant steel according to claim 1, It is characterized in that The electroslag slag material is fully baked at 850±20° C. for 12 to 16 hours before use.
3. A process for improving the yield of B and Nb in boron-containing heat-resistant steel according to claim 1, It is characterized in that Measuring the acid-soluble boron content in the boron- and nitrogen-containing heat-resistant steel electrode base material includes: Take multiple sets of drill cuttings samples from the head and tail of the boron-containing heat-resistant steel electrode base material; Weigh 1-2g of drill cuttings sample for each group and dissolve the sample with 1% strong acid solution; When the sample is fully dissolved, filter it through filter paper; let it stand for a while, take the supernatant after the solution is separated, and dilute it to a concentration of 10%; take 20 ml of the diluted solution and inject it into the separatory funnel; preparing a boron ion extractant, wherein the boron ion extractant is a solution of 2-ethyl-1,3-hexanediol and chloroform in a volume ratio of 1:120; Pour the extractant into the separatory funnel, seal it, and shake it for 3-5 minutes; after standing, take the supernatant and dilute it to 10% concentration; The B content in the diluted supernatant, i.e., the acid-soluble boron content in the boron- and nitrogen-containing heat-resistant steel electrode base material, is obtained by ICP detection.
4. A process for improving the yield of B and Nb in boron-containing heat-resistant steel according to claim 3, It is characterized in that Also includes, The total boron content in the electrode base material is obtained by spark direct reading; The content of non-acid-soluble boron in the heat-resistant steel ingot is obtained by subtracting the acid-soluble boron content in the boron-containing and nitrogen-containing heat-resistant steel electrode base material from the total boron content.
5. A process for improving the yield of B and Nb in boron-containing heat-resistant steel according to claim 1, It is characterized in that Electroslag remelting in a protective atmosphere includes For heat-resistant steel ingots with a total weight of ≤3t, the electroslag melting rate is controlled at 7-9kg / min; for heat-resistant steel ingots with a total weight of ≥3t, the electroslag melting rate is controlled at 9-11kg / min.
6. A process for improving the yield of B and Nb in boron-containing heat-resistant steel according to claim 1, It is characterized in that The method further comprises, After electroslag remelting, the electroslag ingot is left to stand in the crystallizer for 1 to 2 hours before being tapped, hood-cooled for 24 to 36 hours, and then annealed at 750 to 800°C for 24 to 30 hours.
7. A process for improving the yield of B and Nb in boron-containing heat-resistant steel according to claim 1, It is characterized in that The acquisition of the heat-resistant steel ingot comprises: Raw material pretreatment: Shot blast the alloy raw materials to completely remove the oxide scale, and weigh them for later use; Charging and melting: Load the alloy raw materials into the crucible in a loose-up and tight-down manner, close the furnace and evacuate the chamber. When the vacuum degree in the smelting chamber is lower than 20Pa, power on and start smelting. After the alloy is completely melted, take samples for analysis and make fine adjustments to the composition in the furnace.
8. A process for improving the yield of B and Nb in boron-containing heat-resistant steel according to claim 1 or 7, It is characterized in that During the vacuum carbon deoxidation refining process, the oxygen content in the electrode base material is controlled at ≤30ppm.
Citation Information
Patent Citations
High-strength heat-resistant steel novel material
CN108004486A
Method for regulating and controlling boron element distribution state in 9Cr3W3CoB heat-resistant steel for ultra-supercritical unit
CN111057827A
Boron element content smelting control method for heat-resistant steel ingot for steam turbine
CN111270125A
Boron-containing stainless steel and boron alloyage smelting method thereof
CN103469105A
Production method of VCD B-containing stainless steel
CN114045427A