A high-density, amphiphilic macroporous adsorption resin and a preparation method thereof, and a method for treating high-salt phenol-containing wastewater

By copolymerizing hydroxy-modified styrene monomers with methacrylate monomers, high-density, amphiphilic macroporous adsorption resins are prepared, which solves the problem of removing phenol substances in high-salt phenol-containing wastewater and achieves high efficiency The highly selective adsorption performance and simple preparation process improve the environmental protection and economic benefits of wastewater treatment.

CN116135894BActive Publication Date: 2024-12-03WANHUA CHEM GRP CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202111365466.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-18
Publication Date
2024-12-03
Estimated Expiration
2041-11-18

AI Technical Summary

Technical Problem

When treating high-saltitude phenol-containing chemical wastewater, existing polymer macroporous adsorption resins have problems such as insufficient density, poor anti-pollution ability, small pore size, low adsorption efficiency and complex preparation process, which is difficult to meet the efficient removal of various phenol substances. and selective requirements.

Method used

By copolymerizing hydroxy-modified styrene monomers with methacrylate monomers, polar functional groups such as hydroxyl groups, ester groups and amino groups are introduced to prepare high-density, amphipathic macroporous adsorption resins, which are simplified by suspension copolymerization method Process to adjust the pore size and functional group content of resin to improve its stability and adsorption properties in high-salt environments.

Benefits of technology

It realizes efficient adsorption and selective removal of various phenolic substances in a high-salt environment. The resin has good wetting, anti-pollution ability and long life. The preparation process is simple and environmentally friendly, which significantly improves the treatment of high-salt phenol-containing treatment. Environmental protection and economic benefits of wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003360573890000041
    Figure BDA0003360573890000041
  • Figure FDA0005082886330000011
    Figure FDA0005082886330000011
  • Figure FDA0005082886330000012
    Figure FDA0005082886330000012
Patent Text Reader

Abstract

The present invention discloses a high-density, amphiphilic macroporous adsorption resin and a preparation method thereof, as well as a method for treating high-salt phenol-containing wastewater. The preparation process of the adsorption resin comprises: first, modifying a styrene-based monomer with a functional small molecule under a catalyst condition, and introducing a hydroxyl-containing functional group on its benzene ring; then, suspending and copolymerizing the modified styrene-based monomer with a methacrylate monomer to obtain a high-density, amphiphilic macroporous adsorption resin. The adsorption resin obtained has multiple polar functional groups such as hydroxyl groups, ester groups, and amino groups bonded on its surface and inside. The introduction of multiple polar groups increases the density of the adsorption resin on the one hand, and the resin can also be stably deposited in the bed in a high-salt environment; on the other hand, the resin is endowed with amphiphilicity and provides multiple hydrogen bonding sites, which have a synergistic effect on the adsorption of phenolic substances in wastewater, showing more efficient adsorption efficiency and selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of porous polymer materials, in particular to a macroporous adsorption resin for treating phenol-containing wastewater. Background Art

[0002] A large amount of phenol-containing wastewater is often produced in the production process of coal chemical industry, new materials, pharmaceuticals, etc., in which the phenol concentration is high and there are many types. At the same time, it may also contain organic matter such as acids and amines. The wastewater has the characteristics of high COD, high salt content, and difficult biodegradation. Due to the wide variety of pollutants in this type of chemical wastewater, dephenolization treatment is often required. Compared with extraction dephenolization, adsorption dephenolization is more economical and efficient. However, high salt and complex composition have always been the difficulties that limit the application of polymer macroporous adsorption resins in the treatment of such chemical wastewater. First, the salt content is high and the wastewater density is high. Most polymer macroporous adsorption resins cannot form a stable column bed in the wastewater; second, the impurity composition in the wastewater is complex, which makes the polymer macroporous adsorption resin easy to be contaminated, greatly reducing its service life, and the properties of different impurities are different. Most adsorbents cannot meet the selective removal of phenolic substances. Therefore, this type of phenol-containing chemical wastewater has higher requirements for polymer macroporous adsorption resins, requiring macroporous adsorption resins to have high density, strong anti-pollution ability, hydrophilicity and lipophilicity, high adsorption efficiency and high selectivity for a variety of different phenols.

[0003] CN102229710B reports a method for preparing phenolic adsorption resin by chloromethylation of polymerized white balls, which has improved density through secondary crosslinking process and can be applied to high-salt organic wastewater treatment. CN103087246B has been improved on this basis, by adding ester monomers to obtain polymerized white balls containing ester groups, and then obtaining high specific surface area adsorption resin through chloromethylation. Although the density of the above-mentioned high crosslinked adsorbent is up to standard, the technical route adopted is relatively cumbersome, and needs to go through a three-step process of low crosslinked primary suspension polymerization-chloromethylation secondary crosslinking-amination modification. In addition, in order to improve the crosslinking density, it is necessary to use carcinogens such as chloromethyl ether, which are extremely harmful to the environment and human health. On the other hand, the adsorption effect of this type of macroporous adsorption resin on phenols in wastewater is not good enough, and the selectivity is worse.

[0004] CN104910313A discloses a method for preparing a polar modified ultra-high cross-linked resin. Although the chloromethyl group on the active monomer 4-vinylbenzyl chloride is used for secondary cross-linking and then amination is performed, although the use of carcinogens such as chloromethyl ether is avoided, the internal pore size is small (2.1-5.5nm) due to the limitation of its structure, and there is a disadvantage of poor adsorption and desorption cyclicity (not resistant to pollution). CN102974324A discloses a method for preparing a polar macroporous resin. A polar resin containing an ester group and a cyano group is prepared by copolymerizing a styrene monomer with a monomer such as an acrylate / acrylonitrile, but the materials are complex, and the specific surface area of ​​the resulting adsorption resin is small, and there is a problem of poor adsorption effect on substances such as phenol.

[0005] "Synthesis and Application of High Specific Surface Area Adsorption Resin" (Changchun University of Technology, Wang Haizhi, 2011 master's degree thesis) uses active monomer 4-vinylbenzyl chloride and divinylbenzene to copolymerize, and adds phenol to introduce phenolic hydroxyl groups on the resin skeleton during secondary crosslinking. Although the polarity of the resin can be adjusted by adjusting the amount of phenol added, it also has the problem of small resin pore size (2.55nm) and poor adsorption and desorption cycle (not resistant to pollution). "Research Progress of Adsorption Resin Modification" (Liaoning Chemical Industry, Vol.48, No.8, p796) discloses macroporous resins modified with functional groups such as phenolic hydroxyl groups and amino groups, but its preparation process is generally complicated, often requiring more than two steps, and the phenolic hydroxyl groups and amino groups grafted on the resin are difficult to accurately control, so there is a problem of poor adsorption of target substances.

[0006] Therefore, in order to solve the above problems, it is still urgent to develop a macroporous adsorption resin suitable for high-salt environment, with good wettability, strong anti-pollution ability, good adsorption performance and selectivity for a variety of phenolic substances, so as to achieve environmentally friendly treatment of phenol-containing chemical wastewater. At the same time, the preparation process of this macroporous adsorption resin should be simple, economical and environmentally friendly. Summary of the invention

[0007] In order to overcome the above-mentioned deficiencies and application limitations of the prior art, the present invention provides a high-density, amphiphilic macroporous adsorption resin and a preparation method thereof, as well as a method for treating high-salt phenolic wastewater. The resin is used for the removal and recycling of phenolic substances in high-salt phenolic chemical wastewater, and has the advantages of good wettability, strong anti-pollution ability, long life, good adsorption effect on different phenols, etc., and the preparation process of the adsorption resin is simple and environmentally friendly, providing a solution for the industrialization of treating phenolic chemical wastewater by adsorption.

[0008] The present invention can obtain a macroporous adsorption resin with polar functional groups such as hydroxyl, ester, and amino groups modified on the skeleton by copolymerizing hydroxyl-modified styrene monomers and methacrylate monomers. On the one hand, the introduction of multiple polar groups increases the density of the adsorption resin, and the resin can also be stably accumulated in the bed in a high-salt environment, thereby ensuring the dynamic adsorption efficiency; on the other hand, multiple hydrogen bonding sites are provided, especially the ion exchange between the amino group and the phenolic hydroxyl group, so that it exhibits a more efficient adsorption efficiency for substances such as phenols in wastewater.

[0009] More importantly, the traditional method for preparing multifunctional macroporous resins is to introduce functional groups such as hydroxyl and amino groups after Friedel-Crafts secondary crosslinking. This process will reduce the pore size of the final target resin, and the substances adsorbed into the resin pores cannot be completely desorbed, thereby deteriorating the anti-pollution property of the resin, and the adsorption amount of the resin will gradually decrease during use. The present invention can obtain the final target resin modified with polar groups through polymerization, and its pore size can be adjusted according to the amount of porogen used in the oil phase during the polymerization process. The principle of phase separation pore formation ensures that the internal pore size of the resin is a mesopore of moderate size; on the other hand, the resin skeleton is modified with hydroxyl groups, and the hydrophilic group has better anti-pollution properties, so the combination of these two will give the resin a better adsorption and desorption cycle.

[0010] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0011] A high-density, amphiphilic macroporous adsorption resin comprising the following structural units:

[0012]

[0013] Among them, the substituent R 1 express One or more of; Substituent R 2 express One or more of .

[0014] A method for preparing a high-density, amphiphilic macroporous adsorption resin comprises the following steps:

[0015] (1) Monomer modification: Under the action of a catalyst, the styrene monomer reacts with a functional small molecule to introduce a hydroxyl-containing functional group on the benzene ring to obtain a modified styrene monomer modified with an alcohol hydroxyl group;

[0016] (2) Suspension copolymerization: The modified styrene monomer, methacrylate monomer, porogen and initiator are mixed and dissolved to form a uniform oil phase; the oil phase is dispersed in an aqueous medium containing a stabilizer and a dispersant; and a high-density, amphiphilic macroporous adsorption resin is obtained by free radical polymerization.

[0017] As a preferred solution, in a specific synthesis step, the step (1) is to add the styrene monomer and the functional small molecule to the reactor in sequence, stir and mix them evenly, then add the catalyst, heat to a certain temperature and react for 5-20 hours. After the reaction is completed, cool to room temperature, filter to remove the solid, remove the unreacted functional small molecule by vacuum distillation of the filtrate, wash with water and dry to obtain the modified styrene monomer modified with alcohol hydroxyl group.

[0018] In the method of the present invention, the styrene monomer in step (1) comprises divinylbenzene and monovinylbenzene, wherein monovinylbenzene is selected from one or more of styrene, methylstyrene, ethylstyrene, fluorostyrene, chlorostyrene and bromostyrene, preferably one or more of styrene, methylstyrene and ethylstyrene.

[0019] In the method of the present invention, the functional small molecule is selected from one or more of propylene oxide, epichlorohydrin, methyl epichlorohydrin, epibromohydrin, 1,2-butylene oxide, chloropropanol, bromopropanol, chlorobutanol, bromobutanol, etc., preferably one or more of epichlorohydrin, methyl epichlorohydrin, epibromohydrin, and chloropropanol, and the mass ratio of the styrene monomer to the functional small molecule is 1:1.2-1:3.

[0020] As a preferred embodiment, step (1) of the present invention is carried out in the presence of a catalyst, wherein the catalyst is selected from one or more of anhydrous ferric chloride, anhydrous aluminum chloride, anhydrous zinc chloride, boron fluoride or sulfuric acid, preferably one or more of anhydrous ferric chloride, anhydrous aluminum chloride and anhydrous zinc chloride. The mass ratio of the styrene monomer to the catalyst is 1:0.1-1:1.

[0021] As a preferred scheme, in a specific synthesis step, the suspension copolymerization in step (2) is to add the uniformly stirred oil phase comprising modified styrene monomers, methacrylate monomers, porogens and initiators to the aqueous phase comprising stabilizers and dispersants, and to carry out suspension polymerization reaction by stirring and heating to generate macroporous resin, and then to obtain macroporous adsorption resin after filtering, hot water washing, acetone Soxhlet extraction, and water washing to remove residual porogens, stabilizers, etc.

[0022] In the method of the present invention, the methacrylate monomers in step (2) include methacrylate monomers containing two or more C=C double bonds and methacrylate monomers containing amino groups. The use of methacrylate monomers can make the resulting resin have higher structural stability and better resistance to acid hydrolysis.

[0023] The methacrylate monomer containing two or more C=C double bonds described in the present invention is selected from one or more of allyl methacrylate, vinyl methacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, butanediol dimethacrylate, and trimethylolpropane trimethacrylate, preferably one or more of ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, butanediol dimethacrylate, and trimethylolpropane trimethacrylate.

[0024] The amino-containing methacrylate monomer of the present invention is selected from one or more of 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl methacrylate, 2-(diisopropylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl methacrylate, and ethylene urea ethoxy methacrylate.

[0025] In the present invention, based on the total mass of the modified styrene monomers and the methacrylate monomers as 100%, the modified divinylbenzene accounts for 40-80%, the modified monovinylbenzene accounts for 0-20%, the methacrylate monomers containing two or more C=C double bonds account for 10-40%, and the methacrylate monomers containing amino groups account for 5-20%; preferably, the modified divinylbenzene accounts for 55-80%, the modified monovinylbenzene accounts for 0-10%, the methacrylate monomers containing two or more C=C double bonds account for 10-30%, and the methacrylate monomers containing amino groups account for 10-20%.

[0026] In the method of the present invention, the porogen can be selected from one or more of the following substances: aromatic hydrocarbons such as toluene, ethylbenzene, and xylene; alkanes such as normal or isomeric carbon atoms of C6-C20, cycloalkanes, including but not limited to n-heptane, n-octane, isooctane, cyclohexane, liquid paraffin, solvent oil, white oil; esters such as ethyl acetate, butyl acetate, isobutyl acetate, etc.; ketones such as cyclohexanone, methyl isobutyl ketone, etc.; ethers such as petroleum ether, anisole, etc.

[0027] The ratio of the total mass of the monomers to the mass of the porogen is 1:0.6-1:2.

[0028] In the method of the present invention, the initiator is selected from one or more of azo compounds such as azobisisobutyronitrile and azobisisoheptanonitrile, and peroxide compounds such as lauroyl peroxide, benzoyl peroxide, dioctanoyl peroxide, and the like.

[0029] The initiator of the present invention is 0.5-2% of the total mass of the monomers.

[0030] As a preferred embodiment, in the method of the present invention, the aqueous phase comprises deionized water, an inorganic salt, a dispersant and a stabilizer.

[0031] The mass ratio of the oil phase to the water phase of the present invention is 1:2-1:5.

[0032] In the method of the present invention, the inorganic salt is one or more of sodium chloride, potassium chloride, sodium sulfate, potassium sulfate, etc., and the inorganic salt accounts for 0-10wt% of the mass of the aqueous phase, preferably 3-10wt%.

[0033] In the method of the present invention, the dispersant is one or more of gelatin, polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, methyl hydroxyethyl cellulose, and hydroxypropyl cellulose.

[0034] The dispersant of the present invention is 0.05-0.5wt% of the mass of the water phase.

[0035] In the method of the present invention, the stabilizer is one or more of methylene blue and sodium nitrite, and the stabilizer is 0.0001-0.001wt% of the mass of the water phase.

[0036] The macroporous adsorption resin skeleton is bonded with functional groups such as hydroxyl, ester and amino groups. The wet true density is 1.04-1.20cm 3 / g, specific surface area of ​​500-950m 2 / g, pore volume is 0.7-2.2cm 3 / g, and the BJH desorption pore size is 4.0-18.0nm.

[0037] A method for treating high-salt phenol-containing wastewater comprises the following steps:

[0038] a) The high-salt phenol-containing wastewater passes through the macroporous adsorption resin bed at a certain flow rate, and the adsorption stops when the phenol content in the effluent exceeds 0.1ppm;

[0039] b) Wash the bed layer 2BV with deionized water, then use NaOH solution to desorb in the column. After desorption, wash the resin with deionized water until the effluent is neutral. Repeat the process of column adsorption and desorption.

[0040] In step a) of the present invention, the aspect ratio of the macroporous adsorption resin bed is (2-8):1.

[0041] In step a) of the present invention, the flow rate is 2-10 BV / h.

[0042] In step b) of the present invention, the water washing flow rate is 2-10 BV / h.

[0043] In step b) of the present invention, the concentration of the NaOH solution is 2-8%, the desorption flow rate is 0.5-4 BV / h, and the desorption time is 3-10h.

[0044] The high-salt phenol-containing wastewater of the present invention is composed of water-soluble inorganic salts and phenolic compounds, wherein the inorganic salts are one or more of sodium chloride, potassium chloride, sodium sulfate, potassium sulfate, sodium nitrate and potassium nitrate, with a concentration of 4-20%; the phenolic compounds are one or more of phenol, cresol, aminophenol, nitrophenol, chlorophenol, hydroquinone, bisphenol A, bisphenol F and naphthol.

[0045] Compared with the macroporous adsorption resin prepared by the prior art, the macroporous adsorption resin prepared by the technical solution of the present invention has the following beneficial effects:

[0046] (1) The macroporous adsorption resin of the present invention has a more stable chemical composition, higher density, better hydrophilicity, better adsorption selectivity and anti-pollution properties for phenolic molecules, and has a simple preparation process, low cost, and is environmentally friendly. It can generate significant environmental and economic benefits in treating high-salt, high-concentration phenol-containing wastewater.

[0047] (2) The macroporous adsorption resin of the present invention can be bonded with functional groups such as hydroxyl groups, ester groups and amino groups on its skeleton without post-modification introduction, and the content of such functional groups can be accurately controlled according to the input amount of the corresponding monomers.

[0048] (2) The present invention can modify polar functional groups such as hydroxyl, ester, and amino groups on the resin skeleton through two-step reactions. On the one hand, the pore size of the obtained resin can be adjusted according to the amount of porogen used in the oil phase. The principle of phase separation pore formation ensures that the internal pore size of the resin is a mesopore of moderate size; on the other hand, the resin skeleton is modified with hydroxyl groups. These two factors give the resin better adsorption and desorption cyclicity. The traditional method for preparing multifunctional macroporous resins is to introduce functional groups such as hydroxyl and amino groups after Friedel-Crafts secondary crosslinking to reduce the pore size, thereby making the resin less resistant to pollution.

[0049] (3) The macroporous adsorption resin of the present invention is amphiphilic, and the benzene ring and alkyl group on the skeleton provide hydrophobicity for the non-polar group, and the hydroxyl group, ester group and amino group provide hydrophilicity for the polar group, and the hydroxyl group, ester group and amino group can provide multiple hydrogen bonding sites. Through the synergistic effect of hydrophilicity and hydrogen bonding, it exhibits a more excellent adsorption effect and selectivity for the target molecule.

[0050] (4) The macroporous adsorption resin of the present invention is amphiphilic. The introduction of multiple polar groups increases the density of the adsorption resin on the one hand, and the resin can also be stably deposited in the bed in a high-salt environment, thereby ensuring the dynamic adsorption efficiency; on the other hand, it provides multiple hydrogen bonding sites, especially the ion exchange effect between the amino group and the phenolic hydroxyl group, so that it exhibits a more efficient adsorption efficiency for substances such as phenols in wastewater. DETAILED DESCRIPTION

[0051] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0052] In the method of the present invention, the density of the polymer macroporous adsorption resin refers to the wet true density of the resin, which is obtained by the method of national standard GB / T 8330-2008. The BET specific surface area, BJH desorption pore size and BET pore volume are all obtained by Micromeritics ASAP2460M.

[0053] Example 1

[0054] 80g of divinylbenzene monomer and 96g of epichlorohydrin were added to a 250mL three-necked flask in sequence, and 8g of anhydrous ferric chloride powder was added after stirring at room temperature. The stirring was adjusted to 150rpm, and the water bath was heated to 40°C for 10 hours. After the reaction was completed, the mixture was cooled to room temperature, the solid powder was removed by suction filtration, and the unreacted epichlorohydrin was removed by vacuum distillation of the filtrate. The filtrate was washed with water, separated, and dried to obtain a modified styrene monomer.

[0055] In a 500mL four-necked flask, add 240g of deionized water, 2g of 10% polyvinyl alcohol solution, 10g of sodium chloride and 0.5g of 0.1% methylene blue solution in sequence, and mix them evenly to form an aqueous phase. Then add the premixed oil phase, the oil phase composition: 35g of the above-mentioned modified styrene monomer, 10g of ethylene glycol dimethacrylate, 5g of 2-(dimethylamino)ethyl methacrylate, 40g of toluene, 20g of n-decane, 0.15g of azobisisobutyronitrile, 0.1g of dibenzoyl peroxide. Turn on stirring, the stirring speed is 130rpm, and the temperature is raised to 60℃ for reaction for 3h, and then raised to 90℃ for aging for 5h to obtain a macroporous adsorption resin. After the reaction is completed, filter and wash with hot water 3 times to remove polyvinyl alcohol, then use acetone to extract to remove the porogen, and then wash with water to remove acetone, and finally obtain a macroporous adsorption resin.

[0056] Example 2

[0057] 80g of divinylbenzene monomer, 20g of styrene and 200g of epibromopropane were added to a 500mL three-necked flask in sequence, and 20g of anhydrous aluminum chloride powder was added after stirring at room temperature. The stirring was adjusted to 150rpm, and the water bath was heated to 40°C for 5 hours. After the reaction was completed, the mixture was cooled to room temperature, the solid powder was removed by suction filtration, and the unreacted epibromopropane was removed by vacuum distillation of the filtrate. The filtrate was washed with water, separated and dried to obtain a modified styrene monomer.

[0058] In a 1L four-necked flask, add 382g of deionized water, 2g of 10% polyvinyl alcohol solution, 16g of potassium chloride and 0.4g of 0.1% methylene blue solution in sequence, and mix them evenly to form an aqueous phase. Then add the premixed oil phase, the oil phase composition: 50g of the above-mentioned modified styrene monomer, 40g of ethylene glycol dimethacrylate, 10g of 2-(diethylamino) ethyl methacrylate, 50g of toluene, 50g of 3# white oil, 0.5g of azobisisoheptonitrile, and 0.5g of dibenzoyl peroxide. Turn on stirring, the stirring speed is 120rpm, and the temperature is raised to 70℃ for reaction for 3h, and then raised to 90℃ for aging for 6h to obtain a macroporous adsorption resin. After the reaction is completed, filter and wash with hot water 3 times to remove the dispersant, then use acetone to extract to remove the porogen, and then wash with water to remove acetone to finally obtain a macroporous adsorption resin.

[0059] Example 3

[0060] 130g of divinylbenzene monomer, 40g of ethylstyrene and 300g of chloropropanol were added to a 500mL three-necked flask in sequence, and 80g of anhydrous zinc chloride powder was added after stirring at room temperature. The stirring was adjusted to 150rpm, and the water bath was heated to 42°C for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, the solid powder was removed by suction filtration, and the unreacted chloropropanol was removed by vacuum distillation of the filtrate. The filtrate was washed with water, separated and dried to obtain a modified styrene monomer.

[0061] In a 1L four-necked flask, add 407g of deionized water, 24g of 10% hydroxyethyl cellulose solution, 48g of sodium sulfate and 0.96g of 0.1% methylene blue solution in sequence, and mix them evenly to form an aqueous phase. Then add the premixed oil phase, the oil phase composition: 85g of the above-mentioned modified styrene monomer, 10g of trimethylolpropane trimethacrylate, 5g of 2-(diisopropylamino)ethyl methacrylate, 60g of toluene, 0.5g of azobisisobutyronitrile, 0.5g of lauroyl peroxide. Turn on stirring, the stirring speed is 110pm, and the temperature is raised to 70℃ for reaction for 6h, and then raised to 90℃ for aging for 3h to obtain a macroporous adsorption resin. After the reaction is completed, filter and wash with hot water 3 times to remove the dispersant, then use acetone to extract to remove the porogen, and then wash with water to remove acetone to finally obtain a macroporous adsorption resin.

[0062] Example 4

[0063] 100g of divinylbenzene monomer and 300g of methyl epichlorohydrin are added to a 500mL three-necked flask in sequence, stirred and mixed at room temperature, and then 100g of anhydrous zinc chloride powder is added. The stirring is adjusted to 140rpm, and the water bath is heated to 42°C for 8 hours. After the reaction is completed, it is cooled to room temperature, and the solid powder is removed by suction filtration. The filtrate is decompressed and distilled to remove the unreacted methyl epichlorohydrin. The filtrate is washed with water, separated, and dried to obtain a modified styrene monomer.

[0064] In a 1L four-necked flask, add 593g of deionized water, 6g of 10% gelatin solution and 1.2g of 0.1% methylene blue solution in sequence, and mix them evenly to form an aqueous phase. Then add the premixed oil phase, the oil phase composition: 80g of the above-mentioned modified styrene monomer, 10g of trimethylolpropane trimethacrylate, 10g of 2-(tert-butylamino)ethyl methacrylate, 100g of ethylbenzene, 50g of 200# solvent oil, 0.6g of azobisisobutyronitrile, and 0.6g of benzoyl peroxide. Turn on stirring, the stirring speed is 130rpm, and the temperature is raised to 70℃ for reaction for 5h, and then raised to 90℃ for aging for 5h to obtain a macroporous adsorption resin. After the reaction is completed, filter and wash with hot water 3 times to remove the dispersant, then use acetone to extract to remove the porogen, and then wash with water to remove acetone to finally obtain a macroporous adsorption resin.

[0065] Example 5

[0066] 120g of divinylbenzene monomer, 20g of methylstyrene and 200g of epichlorohydrin were added to a 500mL three-necked flask in sequence, and 40g of anhydrous ferric chloride powder was added after stirring at room temperature. The stirring was adjusted to 130rpm, and the water bath was heated to 30°C for 20 hours. After the reaction was completed, the mixture was cooled to room temperature, the solid powder was removed by suction filtration, and the unreacted epichlorohydrin was removed by vacuum distillation of the filtrate. The filtrate was washed with water, separated and dried to obtain a modified styrene monomer.

[0067] In a 2L four-necked flask, add 846g of deionized water, 9g of 10% polyvinyl alcohol solution, 36g of sodium chloride and 9g of 0.1% methylene blue solution in sequence, and mix them evenly to form an aqueous phase. Then add the premixed oil phase, the oil phase composition: 70g of the above-mentioned modified styrene monomer, 10g of butanediol dimethacrylate, 20g of methacrylate ethylene urea ethoxy ester, 120g of toluene, 80g of ethyl acetate, 1.0g of azobisisobutyronitrile, 1.0g of benzoyl peroxide. Turn on the stirring, the stirring speed is 130pm, and the temperature is raised to 70℃ for reaction for 6h, and then raised to 90℃ for aging for 5h to obtain a macroporous adsorption resin. After the reaction is completed, filter and wash with hot water 3 times to remove the dispersant, then use acetone to extract to remove the porogen, and then wash with water to remove the acetone, and finally obtain a macroporous adsorption resin.

[0068] Comparative Example 1 (unmodified styrene monomer)

[0069] In a 500mL four-necked flask, add 240g of deionized water, 2g of 10% polyvinyl alcohol solution, 10g of sodium chloride and 0.5g of 0.1% methylene blue solution in sequence, and mix them evenly to form an aqueous phase. Then add the premixed oil phase, the oil phase composition: 35g of divinylbenzene, 10g of ethylene glycol dimethacrylate, 5g of 2-(dimethylamino)ethyl methacrylate, 40g of toluene, 20g of n-decane, 0.15g of azobisisobutyronitrile, 0.1g of dibenzoyl peroxide. Turn on stirring, the stirring speed is 130rpm, and the temperature is raised to 60℃ for reaction for 3h, and then raised to 90℃ for aging for 5h to obtain a macroporous adsorption resin. After the reaction is completed, filter and wash with hot water 3 times to remove polyvinyl alcohol, then use acetone to extract to remove the porogen, and then wash with water to remove acetone to finally obtain a macroporous adsorption resin.

[0070] Comparative Example 2 (without amino methacrylate)

[0071] 80g of divinylbenzene monomer and 96g of epichlorohydrin were added to a 250mL three-necked flask in sequence, and 8g of anhydrous ferric chloride powder was added after stirring at room temperature. The stirring was adjusted to 150rpm, and the water bath was heated to 40°C for 10 hours. After the reaction was completed, the mixture was cooled to room temperature, the solid powder was removed by suction filtration, and the unreacted epichlorohydrin was removed by vacuum distillation of the filtrate. The filtrate was washed with water, separated, and dried to obtain a modified styrene monomer.

[0072] In a 500mL four-necked flask, add 240g of deionized water, 2g of 10% polyvinyl alcohol solution, 10g of sodium chloride and 0.5g of 0.1% methylene blue solution in sequence, and mix them evenly to form an aqueous phase. Then add the premixed oil phase, the oil phase composition: 35g of the above-mentioned modified styrene monomer, 10g of ethylene glycol dimethacrylate, 5g of ethyl methacrylate, 40g of toluene, 20g of n-decane, 0.15g of azobisisobutyronitrile, 0.1g of dibenzoyl peroxide. Turn on the stirring, the stirring speed is 130rpm, and the temperature is raised to 60℃ for reaction for 3h, and then the temperature is raised to 90℃ for aging for 5h to obtain a macroporous adsorption resin. After the reaction is completed, filter and wash with hot water 3 times to remove polyvinyl alcohol, then use acetone to extract to remove the porogen, and then wash with water to remove acetone, and finally obtain a macroporous adsorption resin.

[0073] Comparative Example 3 (phenol post-modification)

[0074] Phenol-modified macroporous adsorption resin was prepared with reference to "Synthesis and Application of High Specific Surface Area Adsorption Resin".

[0075] Take 20.0g of chloromethylstyrene and 0.514g of divinylbenzene and add them in turn into a three-necked flask containing 360g of 0.9% polyvinyl alcohol solution, then add 0.136g of benzoyl peroxide, stir to dissolve, and react at 80℃ under nitrogen protection for 6 hours; wash three times with 70℃ deionized water, filter while hot, extract with acetone for 8 hours, and dry to obtain the precursor polychloromethylstyrene-divinylbenzene.

[0076] Take 15.0g of chloromethylstyrene-divinylbenzene and place it in a 500mL three-necked flask containing 200mL of 1,2-dichloroethane, add 5.0g of FeCl 3 , stir and swell at room temperature for 12 hours, react at 80°C for 6 hours, then add 0.075g phenol (0.5% of the polymer mass), react at 80°C for 6 hours, cool and filter, add the product to a 1% hydrochloric acid / acetone solution, stir and wash until the washing liquid is colorless, extract with acetone for 8 hours, wash with water to remove acetone to obtain a hydroxyl-modified macroporous resin.

[0077] The sample parameters of the embodiments and comparative examples are shown in Table 1.

[0078] Table 1 Parameters of Examples and Comparative Examples

[0079] Sample name <![CDATA[Specific surface area m 2 / g]]> <![CDATA[Pore volume cm 3 / g]]> BJH desorption pore size nm Wet true density g / mL Example 1 750 1.10 7.6 1.08 Example 2 680 1.00 7.8 1.05 Example 3 580 0.70 4.0 1.07 Example 4 900 1.60 9.0 1.20 Example 5 760 2.20 15.0 1.12 Comparative Example 1 760 1.03 7.6 1.04 Comparative Example 2 740 1.08 7.7 1.06 Comparative Example 3 980 0.64 2.9 1.05

[0080] Prepare phenolic wastewater with a NaCl content of 10% for standby use, wherein the organic matter composition is: 100ppm phenol, 150ppm cresol, and 100ppm bisphenol A. Take 25mL of the wet resin of the above embodiment and comparative example and load it into a chromatography column with an inner diameter of 20mm, so that the height-to-diameter ratio of the bed is 4:1. The above phenolic wastewater is introduced into the column for adsorption at a flow rate of 5BV / h, and the adsorption is stopped when the phenol content of the effluent exceeds 0.1ppm; then the bed is rinsed with deionized water at a flow rate of 5BV / h for 2BV, and then 4% NaOH is introduced into the column for desorption at a flow rate of 1.5BV / h for 6h. After desorption, the resin is rinsed with deionized water at a flow rate of 2BV / h until the effluent is neutral, and then it is introduced into the column for adsorption again. This cycle is repeated for 20 cycles, and the average adsorption amount and average desorption rate of 20 cycles are calculated. As shown in Table 2 below.

[0081] Table 2 Performance of Examples and Comparative Examples

[0082] Sample name Average adsorption capacity mg / mL Average desorption rate% Example 1 88 96 Example 2 85 97 Example 3 83 95 Example 4 92 97 Example 5 86 98 Comparative Example 1 65 83 Comparative Example 2 64 94 Comparative Example 3 59 82

[0083] From the experimental data of 20 cycles of dynamic operation, it can be obtained that the average adsorption amount of Examples 1-5 in 20 cycles is 83-92 mg / mL, and the desorption rate is between 95-98%. Among them, since Example 3 has a slightly lower specific surface area, its adsorption amount is slightly lower than that of other examples, but despite its small pore size, its average desorption rate is still as high as 95%. In contrast, since the resin skeletons of Comparative Examples 1 and 2 lack hydroxyl groups and amino groups respectively, the synergistic effect of hydrogen bonds is lacking or weakened during adsorption, so its adsorption amount is lower than that of the examples, and since there are no hydroxyl groups on the skeleton of Comparative Example 1, the resin has poor anti-pollution properties, so its desorption rate is also low; Comparative Example 3 has a higher specific surface area and the resin skeleton is modified with hydroxyl groups, so its average adsorption amount in the initial stage of adsorption reaches or even exceeds that of the examples, and its average adsorption amount in the first five cycles is as high as 83 mg / mL. However, due to its small pore size (2.9 nm), as the operating cycle increases, the adsorbed substances cannot be completely desorbed, and the desorption rate gradually decreases, resulting in a decrease in the adsorption amount. Therefore, the average adsorption amount within 20 cycles is lower than that in the embodiment.

[0084] From the above results, it can be found that the macroporous adsorption resin prepared by the technical solution of the present invention has a more stable chemical composition, higher density, better adsorption selectivity and anti-pollution properties for phenolic molecules, and the preparation process is simple, the cost is low, and it is environmentally friendly. It can produce significant environmental and economic benefits in the treatment of high-salt phenol-containing wastewater.

[0085] Although the content of the present invention has been described in detail through the above embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. It can be understood by those skilled in the art that some modifications or adjustments may be made to the present invention under the guidance of this specification. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A high-density, amphiphilic macroporous adsorption resin comprising the following structural units: The R1 is independent of each other. One or more of; the substituent R2 represents One or more of .

2. A method for preparing the resin according to claim 1, comprising the following steps: (1) Monomer modification: Under the action of a catalyst, the styrene monomer reacts with a functional small molecule to introduce a hydroxyl-containing functional group on the benzene ring to obtain a modified styrene monomer modified with an alcohol hydroxyl group; (2) Suspension copolymerization: The modified styrene monomer, methacrylate monomer, porogen and initiator are mixed and dissolved to form a uniform oil phase; the oil phase is dispersed in an aqueous medium containing a stabilizer and a dispersant; and a high-density, amphiphilic macroporous adsorption resin is obtained by free radical polymerization.

3. The method according to claim 2, characterized in that The styrene monomers in step (1) include divinylbenzene and monovinylbenzene, wherein monovinylbenzene is selected from one or more of styrene, methylstyrene, ethylstyrene, fluorostyrene, chlorostyrene and bromostyrene.

4. The method according to claim 3, characterized in that The functional small molecules are selected from one or more of propylene oxide, epichlorohydrin, methyl epichlorohydrin, epibromohydrin, 1,2-butylene oxide, chloropropanol, bromopropanol, chlorobutanol, and bromobutanol, and the mass ratio of the styrene monomer to the functional small molecules is 1:1.2-1:

3.

5. The method according to claim 4, characterized in that The methacrylate monomers in step (2) include methacrylate monomers containing two or more C=C double bonds and methacrylate monomers containing amino groups.

6. The method according to claim 5, characterized in that The methacrylate monomer containing two or more C=C double bonds is selected from one or more of allyl methacrylate, vinyl methacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, butanediol dimethacrylate and trimethylolpropane trimethacrylate.

7. The method according to claim 5, characterized in that The amino-containing methacrylate monomer is selected from one or more of 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl methacrylate, 2-(diisopropylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl methacrylate, and ethylene urea ethoxy methacrylate.

8. The method according to claim 5, characterized in that Taking the total mass of modified styrene monomers and methacrylate monomers as 100%, modified divinylbenzene accounts for 40-80%, modified monovinylbenzene accounts for 0-20%, methacrylate monomers containing two or more C=C double bonds account for 10-40%, and methacrylate monomers containing amino groups account for 5-20%.

9. The method according to claim 8, characterized in that Modified divinylbenzene accounts for 55-80%, modified monovinylbenzene accounts for 0-10%, methacrylate monomers containing more than two C=C double bonds account for 10-30%, and methacrylate monomers containing amino groups account for 10-20%.

10. The resin according to claim 1 or the resin prepared by the method according to any one of claims 2 to 8, characterized in that: The wet true density of the resin is 1.04-1.20cm 3 / g, specific surface area of ​​500-950m 2 / g, pore volume is 0.7-2.2cm 3 / g, and the BJH desorption pore size is 4.0-18.0nm.

11. A method for treating high-salt phenolic wastewater, comprising the following steps: a) high-salt phenol-containing wastewater passes through the macroporous adsorption resin bed of claim 1 at a certain flow rate, and adsorption is stopped when the phenol content in the effluent exceeds 0.1 ppm; b) Wash the bed with deionized water for 2 BV, then use NaOH solution to desorb, and after desorption, wash the resin with deionized water until the effluent is neutral.

Citation Information

Patent Citations

  • Method for producing phenol adsorbent resin

    CN102229710B

  • Strong-polarity macroporous adsorption resin

    CN102974324A

  • A high specific surface area adsorption resin containing ester groups and its preparation method

    CN103087246B

  • Method for preparing polar modified ultrahighly-crosslinked resin and application of resin

    CN104910313A

  • Pretreatment and recycling method of phenolic wastewater in production of basic purple dye

    CN101628768A