A catalyst for synthesizing alicyclic amines, and its preparation method and application
By using carbon nitride support to support the ruthenium palladium catalyst in nitro aromatic compounds, a two-dimensional nanosheet structure is formed, which solves the problems of low catalyst selectivity and many by-products in the prior art, and achieves a high-efficiency step of nitro aromatic compounds Hydrogenation of alicyclic amines improves reaction efficiency and safety.
Patent Information
- Application Number
- CN202111521782.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-12-13
AI Technical Summary
The catalysts used in the prior art for the preparation of alicyclic amines have problems such as low selectivity, high by-product production, insufficient conditions and low safety, especially in the hydrogenation reaction of nitro aromatic compounds.
Carbon nitride is used as a support and the metals ruthenium and palladium are supported to form a two-dimensional nanosheet structure through thermal peeling. The synergistic action of ruthenium palladium is used to achieve a green hydrogenation process without alkaline liquid addition, which improves the activity and selectivity of the catalyst.
The nitro aromatic compound is synthesized in one-step tandem hydrogenation under mild conditions, which improves the selectivity and reaction efficiency of the alicyclic amine, reduces the generation of by-products, and avoids the use of alkaline additives.
Smart Images

Figure CN116262240B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalytic synthesis, and in particular to a catalyst for synthesizing alicyclic amines, a preparation method and application thereof, and in particular to a catalyst for synthesizing alicyclic amines from nitroaromatic compounds, a preparation method and application thereof. Background Art
[0002] At present, alicyclic amines, as an important raw material and intermediate for organic chemical and fine chemical industry, have been widely used in food, pharmaceutical, textile, coating, papermaking and plastic processing industries. Compared with aromatic amines, alicyclic amines do not contain benzene ring structure, thus overcoming the disadvantage of aromatic amines being easily oxidized. In addition, due to their excellent high temperature resistance, corrosion resistance, sun exposure resistance, yellowing resistance, insulation and flexibility, the application scope of alicyclic amines is gradually developing towards high-performance functional fields such as high-performance coatings, special polyurethanes, high-precision equipment, and aerospace. In particular, alicyclic amines are important raw materials for synthesizing alicyclic isocyanates (ADI), and the isocyanates prepared from them have become the key basic materials for the production of high-grade polyurethanes, and are also known as the "pearl" on the crown of polyurethanes. At present, the industrial process routes for preparing alicyclic amines from nitroaromatic compounds are mainly divided into "two-step method" and "one-step method". The existing production route is mainly based on the "two-step method", that is, the nitro group in the nitro aromatic compound is first selectively hydrogenated to synthesize the corresponding aromatic amine (Ar-NO2+H2→Ar-NH2), and then the synthesized aromatic amine is selectively hydrogenated to generate the corresponding alicyclic amine (aromatic ring+H2→cycloalkyl). However, the two-step reaction involves different reaction devices, catalysts, process conditions, separation processes, etc., resulting in high costs, high energy consumption, complex operations, and low safety factors. The "one-step method" is rarely used in actual production due to harsh reaction conditions, expensive catalysts, low selectivity and other factors. Therefore, it is of great significance to develop a process for preparing alicyclic amines by one-step hydrogenation of nitro aromatic compounds under mild conditions.
[0003] CN103450028A discloses a carbon nanotube-supported Pd catalyst. By controlling the temperature and pressure, nitrobenzene can generate cyclohexylamine and dicyclohexylamine in one step, but the reaction process requires the addition of an alkaline auxiliary agent and an inhibitor, wherein the alkaline auxiliary agent is at least one of Na2CO3, Ni(NO3)2, CH3COONH4, and ZnSO4·7H2O, and the inhibitor is at least one of FeCl3, CuCl2, and Na2SO4. The alkaline auxiliary agent can effectively inhibit the condensation reaction of cyclohexylamine to generate dicyclohexylamine, but even with the addition of the alkaline auxiliary agent, the selectivity of cyclohexylamine is still only 18-37%.
[0004] CN103772207A discloses a Rh-Ni bimetallic catalyst for one-step hydrogenation of nitrobenzene to synthesize cyclohexylamine. Rh and Ni are successfully loaded on a carbon-based carrier by an impregnation method, and alkaline additives such as LiOH, KOH, etc. are added to inhibit the generation of by-products, so that the selectivity of cyclohexylamine reaches 59.8%-91.6%. However, the added alkaline additive requires an additional separation process, which increases the production cost, and the generated alkaline waste liquid seriously pollutes the environment.
[0005] In summary, the catalysts disclosed in the prior art for preparing alicyclic amines have problems such as the addition of alkali solution, the conditions are not mild enough, the safety is low, and the selectivity of the target product is low. More importantly, in the hydrogenation reaction, different functional groups often have a competitive adsorption relationship on the surface of the active component. The catalysts supported by a single metal can often only achieve the selective hydrogenation of a single functional group. For the reaction system of simultaneous hydrogenation of multiple groups, such as the hydrogenation reaction system of nitroaromatic compounds to synthesize alicyclic amines, the reaction conditions are not mild enough and the selectivity of the target product is low. Therefore, the development of a new type of efficient and green catalyst for synthesizing alicyclic amines has important guiding significance and practical value for the production of alicyclic amines. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a catalyst for synthesizing alicyclic amines from nitroaromatic compounds, and a preparation method and application thereof, so as to solve the problems of low selectivity and high by-product generation of the current catalysts for synthesizing alicyclic amines.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a catalyst for synthesizing alicyclic amines from nitroaromatic compounds, the catalyst comprising a carrier and an active component supported on the carrier;
[0009] The carrier is carbon nitride, and the active components are metal ruthenium and metal palladium, with 0.01-7% ruthenium and 0.01-7% palladium in terms of mass percentage, and the rest being the carrier.
[0010] Carbon nitride is used as a carrier and treated by thermal stripping to form a two-dimensional nanosheet structure. While increasing the specific surface area of carbon nitride, the distance between carbon nitride layers is increased, which is conducive to the high dispersion of the active component ruthenium palladium and provides a channel for the mass transfer process in the hydrogenation reaction. The Lewis basic sites provided by the thermally stripped carbon nitride realize a green hydrogenation process without the addition of alkali solution. Utilizing the synergistic effect of ruthenium palladium hydrogenation catalysis, when the palladium loading ratio is (0.9-1.1):1, the catalyst characteristic activity (mol alicyclic amine / molRu·Pd / h) is significantly higher than that of catalysts loaded at other ratios and single metal loaded catalysts at the same ratio, but it does not mean that the catalysts under other ratios have no catalytic effect. The one-step tandem hydrogenation of nitroaromatic compounds to synthesize alicyclic amines under mild conditions is realized.
[0011] In the present invention, the metal ruthenium in the catalyst is present in an amount of 0.01-7% by mass, such as 0.01%, 1%, 2%, 3%, 4%, 5%, 6% or 7%, etc., but is not limited to the listed values, and other combinations not listed within this range are also applicable.
[0012] In the present invention, the metal palladium in the catalyst is 0.01-7% by mass, such as 0.01%, 1%, 2%, 3%, 4%, 5%, 6% or 7%, but is not limited to the listed values, and other combinations not listed within this range are also applicable.
[0013] The above-mentioned mass percentages of metal ruthenium and palladium in the catalyst refer to theoretical mass percentages, that is, it is assumed that all metal ruthenium and palladium raw materials are successfully loaded in the catalyst.
[0014] In the present invention, the graphite phase carbon nitride with a two-dimensional nanosheet structure is obtained by subjecting bulk graphite phase carbon nitride to thermal exfoliation treatment; the thermal exfoliation temperature is 400-600°C, the time is 0.5-3h, and the atmosphere is air and / or inert gas.
[0015] In the present invention, the thermal stripping temperature is 400-600°C, such as 400°C, 450°C, 500°C, 550°C or 600°C, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0016] In the present invention, the thermal stripping time is 0.5-3h, such as 0.5h, 1h, 1.5h, 2h, 2.5h or 3h, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0017] The bulk graphite carbon nitride is prepared by calcining any one of cyanamide, dicyandiamide, melamine, thiourea, urea or guanidine hydrochloride or a combination of at least two thereof. The calcination atmosphere is air or an inert gas, preferably nitrogen.
[0018] The combination of at least two, for example, a combination of cyanamide and dicyandiamide, a combination of dicyandiamide and melamine, a combination of thiourea and urea, etc., but is not limited to the listed combinations, and other combinations not listed within the scope are also applicable.
[0019] In the present invention, the calcination temperature in the preparation of the bulk graphite phase carbon nitride is 450-650°C, such as 450°C, 500°C, 550°C, 600°C or 650°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0020] In the present invention, the calcination time in the preparation of the bulk graphite phase carbon nitride is 0.5-5h, such as 0.5h, 1h, 2h, 3h, 4h or 5h, but is not limited to the listed values, and other unlisted combinations within the range are also applicable.
[0021] That is, any one of cyanamide, dicyandiamide, melamine, thiourea, urea or guanidine hydrochloride or a combination of at least two thereof is calcined in air or inert gas at 450-650° C. for 0.5-5 h to obtain bulk graphite phase carbon nitride; and the bulk graphite phase carbon nitride is thermally stripped in air at a temperature of 400-600° C. for 0.5-3 h to obtain graphite phase carbon nitride with a two-dimensional nanosheet structure.
[0022] In a second aspect, the present invention provides a method for preparing the catalyst according to the first aspect, the preparation method comprising the following steps:
[0023] (1) mixing a metal ruthenium precursor solution and a carbon nitride suspension according to a formula, and then adding a first reducing agent to obtain a ruthenium-containing carbon nitride suspension;
[0024] (2) The ruthenium-containing carbon nitride suspension obtained in step (1) and the metal palladium precursor solution are mixed for a second time, and then a second reducing agent is added to obtain a ruthenium-palladium carbon nitride suspension, and the catalyst is obtained by solid-liquid separation and drying.
[0025] In the present invention, when the carbon nitride suspension, the metal ruthenium precursor solution and the metal palladium precursor solution are mixed, the volume ratio of the solutions when mixed is determined according to the above formula, such as 50-80 mL of the carbon nitride suspension is mixed with 10-40 mL of the metal ruthenium precursor solution, and the obtained 60-120 mL of the ruthenium-containing carbon nitride suspension is mixed with 10-40 mL of the metal palladium precursor solution.
[0026] The preparation method of the catalyst for synthesizing alicyclic amines from nitro aromatic compounds in one step has a simple process and is easy to industrialize.
[0027] In the present invention, the solvent used in preparing the solution is water or other replaceable solvents.
[0028] In the present invention, the precursor solution and the carbon nitride suspension are dispersed solutions by ultrasonic dispersion, and the dispersion time is 0.5-12h, for example, 0.5h, 1h, 2h, 4h, 6h, 8h, 10h, 11h or 12h, etc., but are not limited to the listed values, and other combinations not listed within this range are also applicable.
[0029] As a preferred technical solution of the present invention, the metal ruthenium precursor solution in step (1) is a solution containing a ruthenium salt.
[0030] Preferably, the ruthenium salt comprises ruthenium trichloride and / or ruthenium acetate.
[0031] Preferably, the mass concentration of ruthenium salt in the metal ruthenium precursor solution in step (1) is 0.001-0.2 g / mL, for example, 0.001 g / mL, 0.005 g / mL, 0.01 g / mL, 0.05 g / mL, 0.1 g / mL, 0.15 g / mL or 0.2 g / mL, but is not limited to the listed values, and other values not listed within this range are also applicable.
[0032] As a preferred technical solution of the present invention, the carbon nitride suspension in step (1) is a solution containing graphite phase carbon nitride after thermal exfoliation treatment;
[0033] Preferably, the solid-to-liquid ratio of the carbon nitride suspension in step (1) is 1:(10-40) g / mL, for example 1:10 g / mL, 1:15 g / mL, 1:20 g / mL, 1:25 g / mL, 1:30 g / mL, 1:35 g / mL or 1:40 g / mL, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0034] Preferably, the temperature of the thermal stripping treatment is 400-600°C.
[0035] Preferably, the atmosphere of the thermal stripping treatment is air and / or an inert gas.
[0036] Preferably, in step (1), the first reducing agent comprises sodium borohydride and / or hydrazine hydrate.
[0037] Preferably, in step (1), the first mixing is ultrasonic mixing, and the mixing time is 0.5-24 h, for example, 0.5 h, 1 h, 2 h, 4 h, 6 h, 8 h, 10 h, 12 h, 16 h, 18 h, 20 h, 22 h or 24 h, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0038] As a preferred technical solution of the present invention, the metal palladium precursor solution in step (2) is a solution containing a palladium salt.
[0039] Preferably, the palladium salt comprises palladium dichloride and / or sodium tetrachloropalladate.
[0040] Preferably, the mass concentration of palladium salt in the metallic palladium precursor solution in step (2) is 0.001-0.2 g / mL, for example, 0.001 g / mL, 0.005 g / mL, 0.01 g / mL, 0.05 g / mL, 0.1 g / mL, 0.15 g / mL or 0.2 g / mL, but is not limited to the listed values, and other combinations not listed within this range are also applicable.
[0041] Preferably, in step (2), the second mixing is ultrasonic mixing, and the mixing time is 0.5-24 h, for example, 0.5 h, 1 h, 2 h, 4 h, 6 h, 8 h, 10 h, 12 h, 16 h, 18 h, 20 h, 22 h or 24 h, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0042] Preferably, in step (2), the second reducing agent comprises sodium borohydride and / or hydrazine hydrate.
[0043] Preferably, the drying temperature in step (2) is 80-120°C, for example 80°C, 90°C, 100°C, 110°C or 120°C; the drying time is 6-12h, for example 6h, 7h, 8h, 9h, 10h, 11h or 12h, etc., but is not limited to the listed values, and other combinations not listed within this range are also applicable.
[0044] Preferably, the drying time in step (2) is 6-12 h, for example 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h, but is not limited to the listed values, and other combinations not listed within the range are also applicable.
[0045] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0046] (1) A ruthenium precursor solution and a carbon nitride suspension are first mixed according to a formula, and then a first reducing agent is added to obtain a ruthenium-containing carbon nitride suspension; the ruthenium precursor solution is a solution containing a ruthenium salt; the ruthenium salt includes ruthenium trichloride and / or ruthenium acetate; the mass concentration of the ruthenium salt in the ruthenium precursor solution is 0.001-0.2 g / mL; the carbon nitride suspension is a solution containing graphite phase carbon nitride after thermal stripping treatment; the solid-liquid ratio of the carbon nitride suspension is 1:(10-40) g / mL; the temperature of the thermal stripping treatment is 400-600°C; the atmosphere of the thermal stripping treatment is air and / or an inert gas; the first reducing agent includes sodium borohydride and / or hydrazine hydrate; the first mixing is ultrasonic mixing, and the mixing time is 0.5-24 h;
[0047] (2) The ruthenium-containing carbon nitride suspension obtained in step (1) and the metal palladium precursor solution are subjected to a second mixing, and then a second reducing agent is added to obtain a ruthenium-palladium carbon nitride suspension, and the catalyst is obtained by solid-liquid separation and drying; the metal palladium precursor solution is a solution containing a palladium salt; the palladium salt includes palladium dichloride and / or sodium tetrachloropalladate; the mass concentration of the palladium salt in the metal palladium precursor solution is 0.001-0.2 g / mL; the second mixing is ultrasonic mixing, and the mixing time is 0.5-24 h; the second reducing agent includes sodium borohydride and / or hydrazine hydrate; the drying temperature is 80-120° C.; and the drying time is 6-12 h.
[0048] In a third aspect, the present invention provides a method for synthesizing alicyclic amines from nitroaromatic compounds in one step, the method comprising: using the nitroaromatic compound as a raw material, using the catalyst as described in the first aspect, and reacting in a hydrogen atmosphere to obtain the alicyclic amine.
[0049] As a preferred technical solution of the present invention, the nitroaromatic compound includes any one or a combination of at least two of the compounds represented by formula (I), formula (II), formula (III) or formula (IV):
[0050]
[0051] wherein R1 and R2 are independently selected from H or C1-C4 alkyl; and X is selected from F, Cl or Br.
[0052] In the present invention, the C1-C4 alkyl group may be methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, etc., but is not limited to the listed alkyl groups, and other alkyl groups not listed within the scope are also applicable.
[0053] As a preferred technical solution of the present invention, the reaction is carried out in a solvent;
[0054] Preferably, the solvent includes any one or a combination of at least two of water, tetrahydrofuran, methanol, isopropanol, ethanol, cyclohexane, cyclohexylamine, n-butanol, toluene, N-methylpyrrolidone or tert-butanol. The combination of at least two is, for example, a combination of tetrahydrofuran and methanol, a combination of isopropanol and ethanol, a combination of cyclohexane and cyclohexylamine, etc., but is not limited to the listed combinations, and other combinations not listed within the scope are also applicable.
[0055] Preferably, the amount of the catalyst is 1-30% of the mass of the nitroaromatic compound, such as 1%, 2%, 5%, 10%, 15%, 20%, 25% or 30%, etc., but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0056] Preferably, the reaction temperature is 50-200°C, such as 50°C, 100°C, 150°C or 200°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0057] In the present invention, the reaction time is 0.5-48h, such as 0.5h, 1h, 5h, 10h, 24h, 30h, 36h or 48h, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0058] Preferably, the initial pressure of the reaction is 0.5-10 MPa, for example 0.5 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa or 10 MPa, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0059] As a preferred technical solution of the present invention, the method comprises: using a nitroaromatic compound as a raw material, using the catalyst as claimed in claim 1, reacting in a hydrogen atmosphere to obtain an alicyclic amine;
[0060] The nitro aromatic compound includes any one or a combination of at least two of the compounds represented by formula (I), formula (II), formula (III) or formula (IV)
[0061]
[0062] Wherein R1 and R2 are independently selected from H or C1-C4 alkyl; X is selected from F, Cl or Br;
[0063] The solvent comprises any one of water, tetrahydrofuran, methanol, isopropanol, ethanol, cyclohexane, cyclohexylamine, n-butanol, toluene, N-methylpyrrolidone or tert-butanol, or a combination of at least two of them; the amount of the catalyst is 1-30% of the mass of the nitroaromatic compound; the reaction temperature is 50-200° C.; and the initial pressure of the reaction is 0.5-10 MPa.
[0064] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0065] (1) Using graphite carbon nitride after air thermal exfoliation as a carrier and ruthenium palladium loaded on the carrier as an active component, on the one hand, bulk graphite carbon nitride has a two-dimensional nanosheet structure after air thermal exfoliation, and the specific surface area of the carrier is increased, which is conducive to the loading and dispersion of bimetallic ruthenium palladium. At the same time, carbon nitride has abundant basic sites, which can effectively inhibit condensation side reactions and reduce the generation of by-products such as dicyclohexylamine and azo compounds.
[0066] (2) The synergistic effect between ruthenium and palladium can effectively enhance the hydrogen adsorption and dissociation capabilities. In the tandem hydrogenation reaction, they can exert their respective competitive adsorption advantages for the substrate, thus achieving a highly active and highly selective one-step hydrogenation conversion of nitroaromatic compounds into alicyclic amines. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 is a transmission electron microscope image of the catalyst obtained in Example 1;
[0068] Figure 2 is the gas chromatogram of the supernatant in Application Example 1;
[0069] Figure 3 is the gas chromatogram of the supernatant in Application Example 4;
[0070] Figure 4 This is the gas chromatogram of the supernatant in Application Example 6.
[0071] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0072] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0073] Example 1
[0074] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0075] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0076] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0077] (3) Dissolve 0.0638 g of RuCl3 in 20 mL of deionized water to obtain a metal ruthenium precursor solution with a concentration of 0.00319 g / mL; dissolve 0.0858 g of Na2PdCl4 in 20 mL of deionized water to obtain a metal palladium precursor solution with a concentration of 0.00429 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0078] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0079] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0080] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst. The transmission electron microscopy photo of the obtained catalyst is shown in Figure 1 .
[0081] Example 2
[0082] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0083] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0084] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0085] (3) Dissolve 0.1148 g of RuCl3 in 20 mL of deionized water to obtain a metal ruthenium precursor solution with a concentration of 0.00574 g / mL; dissolve 0.0172 g of Na2PdCl4 in 20 mL of deionized water to obtain a metal palladium precursor solution with a concentration of 0.00086 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0086] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0087] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0088] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst.
[0089] Example 3
[0090] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0091] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0092] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0093] (3) Dissolve 0.1063 g of RuCl3 in 20 mL of deionized water to obtain a metal ruthenium precursor solution with a concentration of 0.00532 g / mL; dissolve 0.0286 g of Na2PdCl4 in 20 mL of deionized water to obtain a metal palladium precursor solution with a concentration of 0.00143 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0094] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0095] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0096] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst.
[0097] Example 4
[0098] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0099] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0100] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0101] (3) Dissolve 0.0851 g of RuCl3 in 20 mL of deionized water to obtain a ruthenium precursor solution with a concentration of 0.00425 g / mL; dissolve 0.0572 g of Na2PdCl4 in 20 mL of deionized water to obtain a palladium precursor solution with a concentration of 0.00286 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0102] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0103] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0104] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst.
[0105] Example 5
[0106] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0107] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0108] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0109] (3) Dissolve 0.0766 g of RuCl3 in 20 mL of deionized water to obtain a metal ruthenium precursor solution with a concentration of 0.00383 g / mL; dissolve 0.0686 g of Na2PdCl4 in 20 mL of deionized water to obtain a metal palladium precursor solution with a concentration of 0.00343 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0110] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0111] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0112] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst.
[0113] Example 6
[0114] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0115] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0116] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0117] (3) Dissolve 0.0425 g of RuCl3 in 20 mL of deionized water to obtain a metal ruthenium precursor solution with a concentration of 0.00213 g / mL; dissolve 0.1144 g of Na2PdCl4 in 20 mL of deionized water to obtain a metal palladium precursor solution with a concentration of 0.00572 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0118] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0119] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0120] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst.
[0121] Example 7
[0122] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0123] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0124] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0125] (3) Dissolve 0.0213 g of RuCl3 in 20 mL of deionized water to obtain a metal ruthenium precursor solution with a concentration of 0.00106 g / mL; dissolve 0.1430 g of Na2PdCl4 in 20 mL of deionized water to obtain a metal palladium precursor solution with a concentration of 0.00715 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0126] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0127] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0128] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst.
[0129] Example 8
[0130] This embodiment provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, and the preparation method thereof is as follows:
[0131] (1) placing urea in a crucible, covering it with a lid, and calcining it in a muffle furnace at 600° C. for 4 h. The obtained solid was rinsed three times with deionized water and ethanol respectively, and then dried in a forced air drying oven at 100° C. for 12 h to obtain bulk graphite carbon nitride;
[0132] (2) calcining the bulk graphite phase carbon nitride obtained in step (1) at 550° C. for 2 h in a muffle furnace without covering it, to obtain graphite phase carbon nitride after air thermal exfoliation treatment;
[0133] (3) Dissolve 0.0062 g of RuCl3 in 20 mL of deionized water to obtain a metal ruthenium precursor solution with a concentration of 0.00064 g / mL; dissolve 0.1544 g of Na2PdCl4 in 20 mL of deionized water to obtain a metal palladium precursor solution with a concentration of 0.00772 g / mL; disperse 2.00 g of the graphite phase carbon nitride powder obtained in step (2) after air thermal exfoliation in 60 mL of deionized water, and ultrasonicate for 30 min to obtain a carbon nitride suspension;
[0134] (4) mixing the metal ruthenium precursor solution obtained in step (3) with the carbon nitride suspension at a volume ratio of 1:3, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing carbon nitride suspension;
[0135] (5) mixing the metal palladium precursor solution obtained in step (3) with the ruthenium-containing carbon nitride suspension obtained in step (4) at a volume ratio of 1:4, and immersing under ultrasound for 12 hours; adding sodium borohydride for reduction to obtain a ruthenium-containing palladium carbon nitride suspension;
[0136] (6) The suspension after impregnation was filtered and the solid was dried at 80° C. for 8 h to obtain the catalyst.
[0137] Comparative Example 1
[0138] This comparative example provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, using bulk graphite-phase carbon nitride as a carrier. That is, the solid phase in the carbon nitride suspension is bulk graphite-phase carbon nitride powder. The catalyst is then obtained according to the preparation process of Example 1.
[0139] Comparative Example 2
[0140] This comparative example provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, using activated carbon as a carrier. That is, the solid phase in the carbon nitride suspension is activated carbon. The catalyst is then obtained according to the preparation process of Example 1.
[0141] Comparative Example 3
[0142] This comparative example provides a catalyst for one-step synthesis of alicyclic amines from nitroaromatic compounds, using aluminum oxide as a carrier. That is, the solid phase in the carbon nitride suspension is aluminum oxide. The catalyst is then obtained according to the preparation process of Example 1.
[0143] Comparative Example 4
[0144] The only difference from Example 1 is that the active components in the catalyst are all replaced with an equal amount of metallic ruthenium. Then, the catalyst is obtained according to the preparation process of Example 1.
[0145] Comparative Example 5
[0146] The only difference from Example 1 is that the active components in the catalyst are all replaced by an equal amount of metal palladium. Then, the catalyst is obtained according to the preparation process of Example 1.
[0147] Application Example 1
[0148] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials, as follows:
[0149] 0.1230g of nitrobenzene, 0.0307g of the catalyst prepared in Example 1, and 10mL of tetrahydrofuran were added to a stainless steel autoclave, and the autoclave was replaced with nitrogen and hydrogen three times respectively, and finally filled with 3MPaH2. After confirming that it was well sealed, the autoclave was heated to 80°C and kept warm for 4h. After the reaction was completed, the autoclave was cooled to 20°C with cold water, and after releasing the gas in the autoclave, the autoclave was opened, the catalyst was separated by centrifugation, and the supernatant was analyzed for composition by gas chromatography. The results are listed in Table 1. Its gas chromatography analysis spectrum is shown in Table 1. Figure 2 As shown (from left to right in the figure are ethanol peak, tetrahydrofuran peak, cyclohexylamine peak, cyclohexanol, biphenyl, and dicyclohexylamine peak).
[0150] Application Example 2
[0151] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of application example 1 only in that the catalyst is the catalyst prepared in example 2, and the other conditions are the same as those of application example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0152] Application Example 3
[0153] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of application example 1 only in that the catalyst is the catalyst prepared in Example 3, and the other conditions are the same as those of application example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0154] Application Example 4
[0155] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of application example 1 only in that the catalyst is the catalyst prepared in Example 4, and the other conditions are the same as those of application example 1. The supernatant was analyzed by gas chromatography, and the results are listed in Table 1. The gas chromatography analysis spectrum is shown in Table 1. Figure 3 As shown (from left to right in the figure are ethanol peak, tetrahydrofuran peak, cyclohexylamine peak, cyclohexanol, biphenyl, and dicyclohexylamine peak).
[0156] Application Example 5
[0157] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of application example 1 only in that the catalyst is the catalyst prepared in Example 5, and the other conditions are the same as those of application example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0158] Application Example 6
[0159] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of application example 1 only in that the catalyst is the catalyst prepared in Example 6, and the other conditions are the same as those of application example 1. The supernatant is analyzed by gas chromatography, and the results are listed in Table 1. The gas chromatography analysis spectrum is shown in Table 1. Figure 4 As shown (from left to right in the figure are ethanol peak, tetrahydrofuran peak, cyclohexylamine peak, cyclohexanol, biphenyl, and dicyclohexylamine peak).
[0160] Application Example 7
[0161] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of application example 1 only in that the catalyst is the catalyst prepared in Example 7, and the other conditions are the same as those of application example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0162] Application Example 8
[0163] This application example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of application example 1 only in that the catalyst is the catalyst prepared in Example 8, and the other conditions are the same as those of application example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0164] Comparative Example 1
[0165] This comparative example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of Application Example 1 only in that the catalyst prepared in Example 1 is replaced by the catalyst prepared in Comparative Example 1, and the other conditions are the same as those of Application Example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0166] Comparative Example 2
[0167] This comparative example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of Application Example 1 only in that the catalyst prepared in Example 1 is replaced by the catalyst prepared in Comparative Example 2, and the other conditions are the same as those of Application Example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0168] Comparative Example 3
[0169] This comparative example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of Application Example 1 only in that the catalyst prepared in Example 1 is replaced by the catalyst prepared in Comparative Example 3, and the other conditions are the same as those of Application Example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0170] Comparative Example 4
[0171] This comparative example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of Application Example 1 only in that the catalyst prepared in Example 1 is replaced by the catalyst prepared in Comparative Example 4, and the other conditions are the same as those of Application Example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0172] Comparative Example 5
[0173] This comparative example provides a method for preparing alicyclic amines using nitroaromatic compounds as raw materials. The operation is different from that of Application Example 1 only in that the catalyst prepared in Example 1 is replaced by the catalyst prepared in Comparative Example 5, and the other conditions are the same as those of Application Example 1. The composition of the supernatant is analyzed by gas chromatography, and the results are listed in Table 1.
[0174] The conditions of gas chromatography analysis in the above application example are as follows: chromatographic column model GsBP-1; column temperature initially 80°C, retained for 1 min, increased to 125°C at 10°C / min, retained for 2 min, then increased to 230°C at 20°C / min, retained at 230°C for 5 min; control mode is pressure control, pressure 50 kPa, purge flow rate 3 mL / min, split ratio 30; vaporization temperature 250°C.
[0175] Table 1
[0176]
[0177]
[0178] It can be seen from the data in Table 1 that the ruthenium-palladium bimetallic catalyst prepared by the method of the present invention utilizes the synergistic effect of ruthenium-palladium hydrogenation catalysis. When the palladium loading ratio is (0.9-1.1):1, the catalyst characteristic activity (mol alicyclic amine / molRu·Pd / h) is significantly higher than that of catalysts loaded at other ratios and single metal loaded catalysts at the same ratio, but it is not equivalent to other catalysts having no catalytic performance. The one-step series hydrogenation of nitroaromatic compounds to alicyclic amines under a mild kit is realized. It is used to catalyze the one-step synthesis of alicyclic amines from nitroaromatic compounds, and the conversion rate of nitroaromatic compounds is 100%, and the selectivity of alicyclic amines is greater than 90%. The main reason is that the catalyst prepared by the present invention makes full use of the high activity of ruthenium-palladium to benzene ring hydrogenation and nitro hydrogenation, realizes the coupling of metal hydrogenation functions, and allows the reaction to proceed under milder conditions. At the same time, the thermally stripped carbon nitride is used as a carrier, and the basic nitrogen groups on it serve as Lewis basic sites to inhibit deamination and condensation side reactions, improve the selectivity of the target product, avoid the addition of basic additives, and realize the one-step tandem hydrogenation of nitroaromatic compounds to prepare alicyclic amines under mild conditions.
[0179] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0180] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0181] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0182] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for synthesizing alicyclic amines from nitroaromatic compounds in one step, characterized in that: The method comprises: using a nitro aromatic compound as a raw material, using a catalyst, and reacting in a hydrogen atmosphere to obtain an alicyclic amine; The catalyst comprises a carrier and an active component supported on the carrier; The carrier is graphite phase carbon nitride with a two-dimensional nanosheet structure, and the active components are metal ruthenium and metal palladium, with 0.01-7% palladium and 0.01-7% ruthenium in mass percentage, and the rest being the carrier.
2. The method according to claim 1, characterized in that The preparation method of the catalyst comprises the following steps: (1) mixing a metal ruthenium precursor solution and a carbon nitride suspension according to a formula, and then adding a first reducing agent to obtain a ruthenium-containing carbon nitride suspension; (2) The ruthenium-containing carbon nitride suspension obtained in step (1) and the metal palladium precursor solution are mixed for a second time, and then a second reducing agent is added to obtain a ruthenium-palladium carbon nitride suspension, and the catalyst is obtained by solid-liquid separation and drying.
3. The method according to claim 2, characterized in that The metal ruthenium precursor solution in step (1) is a solution containing ruthenium salt.
4. The method according to claim 3, characterized in that The ruthenium salt includes ruthenium trichloride and / or ruthenium acetate.
5. The method according to claim 3, characterized in that The mass concentration of ruthenium salt in the metal ruthenium precursor solution in step (1) is 0.001-0.2 g / mL.
6. The method according to claim 2, characterized in that The carbon nitride suspension in step (1) is a solution containing graphite phase carbon nitride after thermal exfoliation treatment.
7. The method according to claim 2, characterized in that The solid-to-liquid ratio of the carbon nitride suspension in step (1) is 1:(10-40) g / mL.
8. The method according to claim 6, characterized in that The temperature of the thermal stripping treatment is 400-600°C.
9. The method according to claim 6, characterized in that The atmosphere of the thermal stripping treatment is air and / or an inert gas.
10. The method according to claim 2, characterized in that In step (1), the first reducing agent comprises sodium borohydride and / or hydrazine hydrate.
11. The method according to claim 2, characterized in that The first mixing in step (1) is ultrasonic mixing, and the mixing time is 0.5-24h.
12. The method according to claim 2, characterized in that The metal palladium precursor solution in step (2) is a solution containing a palladium salt.
13. The method according to claim 12, characterized in that The palladium salt includes palladium dichloride and / or sodium tetrachloropalladate.
14. The method according to claim 12, characterized in that The mass concentration of palladium salt in the metal palladium precursor solution in step (2) is 0.001-0.2 g / mL.
15. The method according to claim 2, characterized in that In step (2), the second mixing is ultrasonic mixing, and the mixing time is 0.5-24h.
16. The method according to claim 2, characterized in that Step (2) The second reducing agent comprises sodium borohydride and / or hydrazine hydrate.
17. The method according to claim 2, characterized in that The drying temperature in step (2) is 80-120°C.
18. The method according to claim 2, characterized in that The drying time in step (2) is 6-12 hours.
19. The method according to claim 2, characterized in that The preparation method of the catalyst comprises the following steps: (1) A ruthenium precursor solution and a carbon nitride suspension are first mixed according to a formula, and then a first reducing agent is added to obtain a ruthenium-containing carbon nitride suspension; the ruthenium precursor solution is a solution containing a ruthenium salt; the ruthenium salt includes ruthenium trichloride and / or ruthenium acetate; the mass concentration of the ruthenium salt in the ruthenium precursor solution is 0.001-0.2 g / mL; the carbon nitride suspension is a solution containing graphite phase carbon nitride after thermal stripping treatment; the solid-liquid ratio of the carbon nitride suspension is 1:(10-40) g / mL; the temperature of the thermal stripping treatment is 400-600°C; the atmosphere of the thermal stripping treatment is air and / or an inert gas; the first reducing agent includes sodium borohydride and / or hydrazine hydrate; the first mixing is ultrasonic mixing, and the mixing time is 0.5-24 h; (2) The ruthenium-containing carbon nitride suspension obtained in step (1) and the metal palladium precursor solution are subjected to a second mixing, and then a second reducing agent is added to obtain a ruthenium-palladium carbon nitride suspension, and the catalyst is obtained by solid-liquid separation and drying; the metal palladium precursor solution is a solution containing a palladium salt; the palladium salt includes palladium dichloride and / or sodium tetrachloropalladate; the mass concentration of the palladium salt in the metal palladium precursor solution is 0.001-0.2 g / mL; the second mixing is ultrasonic mixing, and the mixing time is 0.5-24 h; the second reducing agent includes sodium borohydride and / or hydrazine hydrate; the drying temperature is 80-120° C.; and the drying time is 6-12 h.
20. The method of claim 1, wherein: The nitro aromatic compound includes any one or a combination of at least two of the compounds represented by formula (I), formula (II), formula (III) or formula (IV) wherein R1 and R2 are independently selected from H or C1-C4 alkyl; and X is selected from F, Cl or Br.
21. The method of claim 1, wherein: The reaction is carried out in a solvent.
22. The method according to claim 21, characterized in that The solvent includes any one or a combination of at least two of water, tetrahydrofuran, methanol, isopropanol, ethanol, cyclohexane, cyclohexylamine, n-butanol, toluene, N-methylpyrrolidone or tert-butanol.
23. The method of claim 1, wherein: The amount of the catalyst used is 1-30% of the mass of the nitro aromatic compound.
24. The method of claim 1, wherein: The reaction temperature is 50-200°C.
25. The method of claim 1, wherein: The initial pressure of the reaction is 0.5-10 MPa.
26. The method of claim 1, wherein: The method comprises: using a nitro aromatic compound as a raw material, using a catalyst, and reacting in a hydrogen atmosphere to obtain an alicyclic amine; The nitro aromatic compound includes any one or a combination of at least two of the compounds represented by formula (I), formula (II), formula (III) or formula (IV) Wherein R1 and R2 are independently selected from H or C1-C4 alkyl; X is selected from F, Cl or Br; The solvent comprises any one of water, tetrahydrofuran, methanol, isopropanol, ethanol, cyclohexane, cyclohexylamine, n-butanol, toluene, N-methylpyrrolidone or tert-butanol, or a combination of at least two of them; the amount of the catalyst is 1-30% of the mass of the nitroaromatic compound; the reaction temperature is 50-200° C.; and the initial pressure of the reaction is 0.5-10 MPa.