A composite material laminated wood for LNG ship and preparation method thereof
By using composite laminated wood with polymer polyols, surfactants, foaming agents, catalysts and glass fiber reinforced materials, the problem of insufficient thermal insulation and mechanical properties of LNG cargo tanks in ultra-low temperature environments is solved, and the preparation process is simplified , reducing costs and improving thermal insulation performance and corrosion resistance.
Patent Information
- Application Number
- CN202311269532.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-09-28
AI Technical Summary
In the existing technology, LNG cargo tanks cannot have both thermal insulation and mechanical properties in ultra-low temperature environments, and the preparation process of laminated wood is complex, costly, and has poor corrosion resistance.
Composite laminated wood composed of polymer polyols, surfactants, foaming agents, catalysts and glass fiber reinforced materials is used through equipment such as polyurethane injection machines, guide rollers, high-frequency vibration-assisted impregnation machines and crawler machines. Preparation, simplifying processes and improving performance.
It achieves high strength and high thermal insulation performance in ultra-low temperature environments (-163°C), simplifies the preparation process, reduces costs, improves thermal insulation performance, meets the requirements for LNG cargo tanks, and has good processing performance.
Smart Images

Figure CN117261374B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of liquefied natural gas ship materials, and in particular to a composite material laminated wood for LNG ships and a preparation method thereof. Background Art
[0002] The market for liquid cargo ships represented by LNG will become larger and larger. The domestic market has a strong demand for laminated wood for liquid cargo tanks, but the market is still monopolized by foreign companies. Laminated wood is made by cutting mature red beech trees into tree segments and then sending them to thin board processing factories. After wood screening and processing, the tree segments are stripped of bark and cut into thin sheets. The sheet layers are then impregnated with phenolic resin under vacuum and densified under high temperature and pressure to form a high-quality laminated wood material. This type of laminated wood is mainly laid between the independent liquid cargo tanks and the supporting steel structure of liquid cargo transport ships. It not only has to withstand the mechanical load from the liquid cargo tanks, but also needs to provide insulation protection for the main hull structure when loading low-temperature goods to ensure that the temperature of the main hull material is always above an acceptable level.
[0003] At present, laminated wood is commonly used as an insulating pad in LNG ships. It has the advantages of high compressive and shear strength, low linear expansion coefficient, low friction coefficient, and low thermal conductivity coefficient. However, due to limited forest resources, long-term logging will cause serious environmental problems. The molding process of this type of laminated wood is relatively complicated, and the production cycle is often long, and the supply cycle is also relatively long. In addition, wooden materials are exposed to harsh environments for a long time. If the product is not protected, it will cause moisture cracking; during use, it will also be eroded by tiny organisms, causing mold and rot.
[0004] As a thermal insulation material, rigid polyurethane foam has excellent thermal insulation performance compared to other thermal insulation materials such as polystyrene foam or mineral wool, but pure polyurethane foam cannot achieve the mechanical strength required under the use conditions, so it is necessary to add certain reinforcing materials to improve its mechanical properties. Patent text CN102307922A discloses a rigid polyurethane foam using glass fiber mat as a reinforcing material, but the material is suitable for insulation under ultra-low temperature environment, but its mechanical strength is low and cannot be used for "bearing structure material". Patent No. CN107090074A discloses a preparation method of a highly flame-retardant glass fiber reinforced rigid polyurethane insulation material. Although this material can be used for insulation at ultra-low temperatures (-170 degrees), its mechanical strength is also low and cannot meet the "support" requirements. Patent No. CN115572362A discloses a method for preparing an ultra-fine glass fiber reinforced polyurethane insulation material. The insulation material with a density of 170-190kg / m3 and a compression strength of 4.98-6.39MPa also cannot achieve the mechanical properties required by the pressure-bearing area of the LNG cargo tank. It can be seen from the above that the existing polyurethane composite materials cannot achieve both thermal insulation and mechanical properties in the ultra-low temperature environment of the LNG cargo tank, so the support and transportation effect of the LNG cargo tank for liquefied natural gas cannot be broken through. Therefore, it is of great significance to study how to improve the spacing thermal insulation mechanical properties of composite materials in low temperature environments.
[0005] Patent CN112319706A mentions a multilayer polyurethane insulation system for a type C LNG cargo tank and a construction method thereof, which includes the following steps: the first metal seat and the second metal seat are installed in the ship, and the third laminated wood is installed in the second metal seat; the first support and the second support are installed at the bottom of the low-temperature medium tank, the first laminated wood is installed in the first support, the second laminated wood is installed in the second support, the bottom of the first laminated wood is installed in the first metal seat, and the lower end surface of the second laminated wood is in contact with the upper end surface of the third laminated wood; the outer wall of the upper end of the first laminated wood and the outer wall of the second laminated wood are installed with porous foam by polyurethane glue; the outer wall of the low-temperature medium tank is installed with a low-temperature insulation spacer by polyurethane glue; the outer wall of the low-temperature insulation spacer is sprayed with polyurethane to form a polyurethane spray layer, and the polyurethane is foamed on site by a sprayer using isocyanate and polyol, and the density is about 40kg / m 3 ; A waterproof coating is installed outside the polyurethane spray layer; the outer walls of the first laminated wood and the second laminated wood are sprayed with mastic. In addition, it is mentioned that the waterproof coating is formed by curing resin and glass fiber cloth or curing resin and steel wire mesh, which can improve the mechanical strength of the system to a certain extent, but the structure is complex, the preparation method is cumbersome, and the preparation cost is high. Summary of the invention
[0006] In view of this, the present invention aims to propose a composite laminated wood for LNG ships and a preparation method thereof, so as to solve the problems existing in the prior art that wooden laminated wood has poor corrosion resistance, low thermal insulation effect, and complicated and costly preparation of laminated wood; thereby achieving the goal of enabling laminated wood to have both thermal insulation and mechanical properties in the ultra-low temperature environment of LNG liquid cargo tanks, simplifying the preparation process of laminated wood, reducing the cost of laminated wood, improving the quality stability of laminated wood, enhancing the ability of laminated wood to maintain high strength and high thermal insulation performance in ultra-low temperature environments (-163°C), and having balanced performance in all directions, which can meet the use requirements of LNG liquid cargo tanks, and can reduce the thermal conductivity coefficient as required to improve the thermal insulation performance.
[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0008] The invention relates to a composite material laminated wood for LNG ships and a preparation method thereof. The composite material laminated wood for LNG ships is composed of 100 parts of polymer polyol, 0.5-3 parts of surfactant, 0.1-0.5 parts of foaming agent, 0.1-2 parts of catalyst, 90-130 parts of polymerized MDI and 50-250 parts of glass fiber reinforcement material.
[0009] Furthermore, the polymer polyol is a polyether polyol, the polyether polyol has a hydroxyl value of 300-500 mgKOH / g, a viscosity of 400-6000 mPa·s at room temperature, and a functionality of 3-6.
[0010] Furthermore, the polymeric MDI is polyphenyl polymethylene polyisocyanate MDI, the isocyanate MDI has an isocyanate content of 30-32 wt % and a functionality of 2-3.
[0011] Furthermore, the catalyst is an amine / organotin delayed-release catalyst or a trimerization catalyst.
[0012] Furthermore, the glass fiber reinforcement material is a composite of any one or more materials selected from the group consisting of glass fiber mesh cloth, biaxial cloth, and glass fiber mat.
[0013] Furthermore, the surface density of the glass fiber reinforced material is 600-1800 g / m2.
[0014] Furthermore, the preparation device of laminated wood includes a cloth rack, a glue injection box, a polyurethane glue injection machine, a guide roller, a high-frequency vibration assisted impregnation machine, a crawler machine and a sawing machine. The cloth rack, the glue injection box, the guide roller, the high-frequency vibration assisted impregnation machine, the crawler machine and the sawing machine are sequentially distributed along the moving direction of the glass fiber reinforced material. The polyurethane glue injection machine is used to transport polyurethane resin into the glue injection box.
[0015] Furthermore, the glue injection box includes a glue injection channel, which is used for the glass fiber reinforced material to pass through the glue injection channel and mix with the polyurethane resin in the glue injection channel to achieve a one-time glue dipping effect; each glue injection channel passes through 1-3 layers of fiber reinforced material.
[0016] Furthermore, a high-frequency vibration auxiliary impregnation machine is arranged between the glue injection box and the crawler machine, which is used to perform secondary vibration impregnation on the glass fiber reinforced material after the first impregnation, and heat and cure it in the mold cavity of the crawler machine.
[0017] A method for preparing composite laminated wood for LNG ships, used for preparing the composite laminated wood for LNG ships, the method comprising the following steps:
[0018] Step 1: Placement and traction of glass fiber reinforced materials;
[0019] Step 2: polyurethane resin injection;
[0020] Step 3: impregnation of glass fiber reinforced materials;
[0021] Step 4: Product curing and shaping;
[0022] Step 5: De-moulding and sawing.
[0023] Compared with the prior art, the composite laminated wood for LNG ships and the preparation method thereof described in the present invention have the following beneficial effects:
[0024] Through the preparation method, the laminated wood can have both thermal insulation and mechanical properties in the ultra-low temperature environment of the LNG liquid cargo tank, simplify the preparation process of the laminated wood, reduce the cost of the laminated wood, improve the quality of the laminated wood, enhance the laminated wood in the ultra-low temperature environment (-163 ° C) to maintain high strength and high thermal insulation performance, and the performance in all directions is balanced, which can meet the use requirements of the LNG liquid cargo tank, and the thermal conductivity can be reduced as required, and the thermal insulation performance is further improved; in addition, by using a certain surface density of glass fiber mesh cloth / biaxial glass fiber felt to prepare a polyurethane composite material, it can be used at room temperature and low temperature While ensuring the thermal insulation performance in an ultra-low temperature environment (-163°C), it maintains its mechanical strength in ultra-low temperatures, and meets the requirements of being a supporting material for LNG ships. It has the characteristics of maintaining high strength, high dimensional stability and high thermal insulation performance in an ultra-low temperature environment (-163°C), and has good punching, bonding and other processing properties similar to wood. Specifically, 1) continuous molding of lightweight and high-strength polyurethane composite materials is achieved; 2) a size-adjustable and customizable composite material sheet is prepared, which has high specific strength at low temperatures and has good thermal insulation effect and flame retardancy. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings, which constitute part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations of the present invention.
[0026] In the figure:
[0027] Figure 1 This is a schematic diagram of the structure of a device for preparing composite laminated wood for LNG ships.
[0028] Explanation of the reference numerals: 1. cloth rack; 12. auxiliary curing device; 2. glue injection box; 3. polyurethane glue injection machine; 31. polyurethane group A tank; 32. polyurethane group B tank; 33. mixer; 34. diverter; 4. guide roller; 5. high-frequency vibration auxiliary impregnation machine; 6. crawler machine; 61. lower mold; 62. upper mold; 7. sawing machine; 8. composite material type laminated wood. DETAILED DESCRIPTION
[0029] The inventive concepts of the present disclosure will be described below using terms commonly used by those skilled in the art to convey the essence of their work to other persons skilled in the art. However, these inventive concepts can be embodied in many different forms and should not be considered limited to the embodiments described herein.
[0030] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0031] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0032] In the prior art, the use of laminated wood or rigid polyurethane foam alone will have the problem of being unable to achieve both insulation and mechanical properties in the ultra-low temperature environment of the LNG liquid cargo tank. Even though some patents use laminated wood and porous foam bonded by resin, or use multiple layers of laminated wood to install porous foam by polyurethane glue, and install a low-temperature insulation spacer outside the low-temperature medium tank body, the outer wall of the low-temperature insulation spacer is sprayed with foamed polyurethane to form a polyurethane spray layer, and a waterproof coating is installed on its outside, and the coating has a glass fiber cloth solidified shape or a resin or steel mesh solidified shape, but the above method still has the problems of complex operation, cumbersome preparation structure, and low mechanical properties.
[0033] In order to solve the problem that the laminated wood in the prior art cannot achieve both thermal insulation and mechanical properties in the ultra-low temperature environment of the LNG liquid cargo tank, and the existing laminated wood preparation is cumbersome and costly; this embodiment proposes a composite laminated wood for LNG ships and a preparation method thereof, specifically: a preparation method of glass fiber reinforced polyurethane laminated wood with high mechanical properties and thermal insulation properties used at low temperatures (-163°C), the preparation method is applied to a composite laminated wood for LNG ships, the composite laminated wood for LNG ships is composed of 100 parts of polymer polyol, 0.5-3 parts of surfactant, 0.1-0.5 parts of foaming agent, 0.1-2 parts of catalyst, 90-130 parts of polymer MDI, and 50-250 parts of glass fiber reinforcement material, i.e., glass fiber mesh cloth; wherein the polymer polyol is polyether polyol, polyester polyol or a mixture of the two, and the hydroxyl value of the polymer polyol is 300-5 00mgKOH / g, the viscosity at room temperature is 400-6000mPa·s, the functionality is 3-6, preferably, the viscosity of the polymer polyol at room temperature is 500-2000mPa·s; the polymeric MDI is polyphenyl polymethylene polyisocyanate, the isocyanate content of the polymeric MDI is 30-32wt%, the viscosity at room temperature is 200±50mPa·s, and the functionality is 2-3; the catalyst is an amine / organotin delayed catalyst, or a trimerization catalyst and water, and the polyurethane composite material using the catalyst has a long milky time, which is beneficial to glass fiber impregnation, and the post-curing time is fast, which is beneficial to rapid curing and demoulding; the surfactant is a general auxiliary agent, and the foaming agent is water. The production process reacts with the polymeric MDI to release carbon dioxide gas, which is environmentally friendly and pollution-free; the glass fiber reinforcement material is a composite of any one or more materials selected from glass fiber mesh cloth, biaxial cloth, and glass fiber felt; the surface density of the glass fiber reinforcement material is 600-1800g / m 2 The laminated wood is glass fiber reinforced polyurethane laminated wood, which can be used at low temperature of -163℃ and has high mechanical properties and thermal insulation properties. Common additives are also added in the preparation process of glass fiber reinforced polyurethane laminated wood, and the common additives are any one or more of flame retardants, silicone oil, and coupling agents. The chemical foaming agent contained in the glass fiber reinforced polyurethane laminated wood includes water. The surface density of the glass fiber reinforced material is 600-1800g / m 2 In this embodiment, room temperature refers to 25°C.
[0034] In addition, through the laminated wood setting in the present application, compared with the laminated wood existing in the prior art, a polyurethane composite laminated wood is prepared by adopting a glass fiber reinforcement material with a certain surface density, namely glass fiber mesh cloth / biaxial glass fiber felt, to maintain its mechanical strength at ultra-low temperature. The polyurethane foam structure in the present application can effectively prevent heat transfer and ensure the good insulation effect of the composite laminated wood; while meeting the requirements of being used as a supporting material for LNG ships, it has the characteristics of maintaining high strength, high dimensional stability and high insulation performance in an ultra-low temperature environment (-163°C), and has good punching, bonding and other processing properties similar to wood; its beneficial effects are mainly reflected in: realizing the continuous molding of lightweight and high-strength polyurethane composite materials; preparing a composite material sheet with adjustable size and customizable shape, which has a high specific strength at low temperatures, good insulation effect and flame retardancy, and can also improve its corrosion resistance.
[0035] The preparation method comprises a device for preparing composite laminated wood for LNG ships, wherein the laminated wood preparation device comprises a cloth rack 1, a glue injection box 2, a polyurethane glue injection machine 3, a guide roller 4, a high-frequency vibration auxiliary impregnation machine 5, a crawler machine 6 and a sawing machine 7, wherein the cloth rack 1, the glue injection box 2, the guide roller 4, the high-frequency vibration auxiliary impregnation machine 5, the crawler machine 6 and the sawing machine 7 are linearly distributed in sequence along the moving direction of the glass fiber reinforced material, the polyurethane glue injection machine 3 is used to convey polyurethane resin into the glue injection box 2, the cloth rack 1 is used to support and layer the glass fiber reinforced material during the preparation of the glass fiber reinforced material, the glue injection box 2 is used to coat the polyurethane resin on the surface of the glass fiber reinforced material, the guide roller 4 is used to control the conveying direction of the glass fiber reinforced material passing through the glue injection box 2, the high-frequency vibration auxiliary impregnation machine 5 is used to make the glass fiber reinforced material after the first impregnation generate high-frequency vibration to improve the impregnation effect and realize the effect of secondary impregnation, and the crawler machine 6 is used to drive the polyurethane composite material along the crawler machine 6 The crawler 6 moves in the direction of movement of the crawler. In addition, since the crawler 6 also includes a mold, the mold is used to heat the glass fiber reinforced material coated with polyurethane resin after secondary impregnation by the high-frequency vibration assisted impregnation machine 5, so that the polyurethane resin is solidified to form a glass fiber reinforced polyurethane composite material laminated wood 8, and the sawing machine 7 is used to cut the prepared composite material laminated wood 8; the polyurethane injection machine 3 includes a mixer 33 and a diverter 34, the mixer 33 is used to mix the two components of materials output from the polyurethane A group tank 31 and the polyurethane B group tank 32, and the diverter 34 is connected to multiple injection channels after diversion to inject glue to the glass fiber reinforced material. Under the action of the crawler 6, the glass fiber reinforced material moves along the cloth rack 1, the injection box 2, the guide roller 4, the high-frequency vibration assisted impregnation machine 5, the crawler of the crawler 6 and the mold, and the sawing machine 7, and forms a composite material laminated wood 8, wherein, under the action of the sawing machine 7, it is automatically sawed according to the set product length to obtain a polyurethane composite board, that is, a composite material laminated wood 8.
[0036] The device can achieve both thermal insulation and mechanical properties of laminated wood in the ultra-low temperature environment of LNG liquid cargo tanks, simplify the preparation process of laminated wood, improve the production efficiency and product quality stability of laminated wood, enhance the high strength and high thermal insulation performance of laminated wood in ultra-low temperature environment (-163°C), meet the use requirements of LNG liquid cargo tanks, and reduce the thermal conductivity coefficient as required to improve the thermal insulation performance.
[0037] The glue injection box 2 includes a glue injection channel, which is used for the glass fiber reinforced material to pass through the glue injection channel and mix with the polyurethane resin in the glue injection channel to play a role of one-time dipping; c glue injection channels are provided, c is a positive integer, and the glue injection channels are arranged in the glue injection box 2 in a top-down manner, the upper end is the glass fiber reinforced material entry end, and the lower end is the glass fiber reinforced material output end, and the glass fiber reinforced material is arranged throughout the glue injection channel, and a layers of glass fiber reinforced material are randomly arranged in each glue injection channel, a is a positive integer, and the value range of a is 1-3 layers, that is, preferably, each glue injection channel passes through 1-3 layers of fiber reinforced material; the glue injection machine 3 evenly disperses the injected polyurethane resin among the glass fiber reinforced materials through the diverter device, and plays a role of one-time dipping in the glue injection box 2; the polyurethane glue injection machine 3 includes a glue storage tank, a mixer 33 and a glue injection flow channel, the glue storage tank is sequentially connected to the glue injection channel through the mixer 33, the diverter 34 The flow channels are connected, and the glue flowing out of the glue storage tank is transported to the inside of the glue injection box 2 through the glue injection flow channel connected to the diverter 34 through the mixer 33; the diverter 34 includes m output ports and p glue inlets, m and p are both positive integers, the glue inlet is used to add the required glue of different components, and the output port is used to uniformly inject glue for the glass fiber reinforced materials arranged in parallel during the transmission process; preferably, p=2, m≥1, which is used to facilitate the addition of two components of glue to be injected; the mixer 33 includes a mixing inlet 1 and a mixing inlet 2, and the mixing inlet 1 and the mixing inlet 2 are both connected to the glue outlet of the glue storage tank, and the mixing inlet 1 and the mixing inlet 2 are used to provide transmission entrances for glue to be injected with different components; the glue storage tank includes a polyurethane group A tank 31 and a polyurethane group B tank 32, the glue outlet of the polyurethane group A tank 31 is connected to the mixing inlet 1, and the glue outlet of the polyurethane group B tank 32 is connected to the mixing inlet 2.
[0038] Through the coordinated setting of the glue injection box 2 and the polyurethane glue injection machine 3, the glue liquids of different components to be injected can be effectively mixed, and through the setting of the various components in the polyurethane glue injection machine 3, the polyurethane glue liquids of different components can be evenly injected into the glue injection channel inside the glue injection box 2 and evenly mixed with the glass fiber reinforced material in the glue injection channel, thereby improving the uniformity and stability of the internal structure of the laminated wood, paving the way for improving the mechanical properties of the laminated wood.
[0039] The auxiliary curing device 12 includes a high-frequency vibration auxiliary impregnation machine 5 and a crawler machine 6. The high-frequency vibration auxiliary impregnation machine 5 is arranged between the injection box 2 and the crawler machine 6, and is used for secondary vibration impregnation of the glass fiber reinforced material after the first impregnation, so as to make the reinforcing material completely impregnated. The crawler machine 6 is used to heat and cure the completely impregnated glass fiber reinforced material. Specifically, the fiber reinforced material completely impregnated by the high-frequency vibration auxiliary impregnation machine 5 enters the crawler machine 6, and is heated and cured in the mold cavity of the crawler machine 6; the crawler machine 6 includes an upper mold 62 and a lower mold 61, and the upper mold 62 and the lower mold 61 are arranged in parallel, and are used to heat and cure the completely impregnated glass fiber reinforced material under the action of the traction device; there is a certain gap between the upper mold 62 and the lower mold 61; in this embodiment, the double groups in the polyurethane injection machine 3 refer to the polyurethane group A tank 31 and the polyurethane group B tank 32, and the polyurethane group A components in the polyurethane group A tank 31 The chemical foaming agent is water, and the polyurethane A group tank 31 and the polyurethane B group tank 32 are both used for glue injection; specifically, the preparation device of the laminated wood includes a cloth placing rack 1, a glue injection box 2, a polyurethane glue injection machine 3, a guide roller 4, a high-frequency vibration auxiliary impregnation machine 5, a crawler machine 6 and a sawing machine 7, the cloth placing rack 1 is used to place the glass fiber reinforced material, the glue injection box 2 is used to coat the polyurethane resin on the surface of the glass fiber reinforced material, the polyurethane glue injection machine 3 is used to transport the polyurethane resin into the glue injection box 2, the guide roller 4 is used to control the conveying direction of the glass fiber reinforced material, the high-frequency vibration auxiliary impregnation machine 5 is used to make the glass fiber reinforced material generate high-frequency vibration, the crawler machine 6 is used to pull the polyurethane composite material laminated wood to move, the crawler machine 6 is provided with a mold, the mold is used to heat the glass fiber reinforced material coated with the polyurethane resin, so that the polyurethane resin is cured to form a glass fiber reinforced polyurethane composite material laminated wood, and the sawing machine 7 is used to cut the glass fiber reinforced polyurethane composite material laminated wood.
[0040] By using glass fiber mesh cloth / biaxial composite felt reinforced polyurethane in the device for preparing laminated wood in the LNG liquid cargo tank support system, the stability of the device can be effectively improved, the structure of the device can be simplified, the reliability of the device can be improved, and the cost of preparing laminated wood can be reduced, and the preparation efficiency of the device can be improved. In addition, the secondary impregnation of the high-frequency vibration-assisted impregnation machine 5 can effectively improve the preparation efficiency of the device, and because the device structure is relatively simple, it is also easy to maintain.
[0041] A method for preparing composite laminated wood for LNG ships, used for preparing the composite laminated wood for LNG ships, the method comprising the following steps:
[0042] Step 1, glass fiber reinforced material placement and traction: according to the required product density and glass fiber reinforced material content, the required amount of glass fiber reinforced material is placed on the cloth rack 1, and driven by the traction device to pass through the lower glue injection box 2. In this embodiment, the glass fiber reinforced material is glass fiber mesh cloth / biaxial composite felt, and the biaxial composite felt is a type of biaxial cloth; specifically, according to the required product density and glass fiber content, a certain amount of glass fiber mesh cloth / biaxial composite felt is placed on the cloth rack 1 with adjustable tension, and the mesh cloth / biaxial composite felt is divided into n layers by the distribution / felt plate, which is a positive integer, generally 2-5 layers of felt are taken as a group, and the cloth / felt roller passes through the lower glue injection box 2, and is connected to the mold by the traction belt for standby use;
[0043] Step 2, polyurethane resin injection: After the polyurethane resin is evenly mixed by the polyurethane injection machine 3, it is evenly injected into the injection box 2 through the diverter 34 to achieve uniform distribution of the glass fiber reinforced material and the polyurethane resin and one-time dipping. Specifically, after the polyurethane resin is mixed by the polyurethane injection machine 3, it is evenly injected through m diverters 34, where m is a positive integer, to ensure that the resin flow and pressure of each injection flow channel are balanced and evenly distributed between the n layers of mesh cloth / biaxial composite felt;
[0044] Step 3: Impregnation of glass fiber reinforced material: After the glue injection is completed, the glass fiber reinforced material that has been impregnated once passes through the high-frequency vibration-assisted impregnation machine 5, so that the polyurethane resin completely impregnates the glass fiber reinforced material; specifically, the liquid raw material passes through the high-frequency vibration-assisted impregnation machine 5, and completely impregnates the composite glass fiber mesh cloth / biaxial glass fiber felt;
[0045] Step 4: Curing and shaping the product: Under the heating effect of the mold of the crawler machine 6, the fully impregnated glass fiber reinforced material is cured and shaped by the crawler machine 6; specifically, after the fiber reinforced material is evenly impregnated with the resin, it is pulled by the crawler machine 6 into between the upper mold 62 and the lower mold 61, and under the heating effect of the mold, the resin is triggered to foam and solidify, thereby forming a glass fiber reinforced polyurethane resin composite material;
[0046] Step 5, demoulding and sawing: the product is automatically sawed by the sawing machine 7 according to the set product length to obtain the composite material laminated wood 8; specifically, after the product is solidified and formed in the mold, it is automatically separated from the rotating mold of the crawler machine 6 at the mold outlet as the mold rotates, and is automatically transmitted forward under the push of the rotating mold. After reaching the sawing machine 7, it is automatically sawed according to the set product length to obtain a polyurethane composite board, that is, a composite material laminated wood 8. In this embodiment, the front refers to the side of the crawler machine 6 close to the sawing machine 7 and the side where the traction force is directed.
[0047] Through the steps, it is possible to achieve that laminated wood has both insulation and mechanical properties in the ultra-low temperature environment of LNG liquid cargo tanks, simplify the preparation process of laminated wood, enhance the high strength and high insulation performance of laminated wood in ultra-low temperature environments, meet the use requirements of LNG liquid cargo tanks, and can reduce the thermal conductivity as required to improve the insulation performance. In addition, through the lightweight, high-strength, low-temperature mechanical and insulation performance of glass fiber reinforced polyurethane foam composite materials and their continuous molding method described in the present application; specifically relates to a pultrusion molding process for low-temperature resistant composite material pads in the field of LNG ships, the process uses glass fiber mesh cloth as a reinforcing material, and through micro-foaming high-pressure impregnation technology, the polyurethane matrix and the glass fiber mesh cloth are tightly combined to improve the various mechanical properties of the material; specifically relates to a type B liquid cargo tank, a type C liquid cargo tank, and a liquid cargo transport ship equipped with at least one such tank using such a composite pad, which is used to support the transportation of liquid products in such a ship.
[0048] In addition, in the following embodiments, the density is measured in accordance with GB / T 1463-2005 "Test method for density and relative density of fiber reinforced plastics"; the compressive strength is measured in accordance with GB / T 1448-2005 "Test method for compression properties of fiber reinforced plastics" at 20°C (at room temperature) and -163°C; the flexural strength is measured in accordance with GB / T 1449-2005 "Test method for flexural properties of fiber reinforced plastics" at 20°C (at room temperature) and -163°C; the thermal conductivity is measured in accordance with ISO22007-4 "Determination of thermal conductivity and thermal diffusivity" at 20°C (at room temperature) and -163°C.
[0049] Embodiment 1:
[0050] Formula of component A of polyurethane resin: 100 parts of polyol resin, 10 parts of flame retardant, 2 parts of silicone oil, and 0.2 parts of composite catalyst;
[0051] Polyurethane resin B component: 120 parts of polymerized MDI;
[0052] Reinforcement material: 50 layers of glass fiber mesh cloth with a surface density of 900g / m2, a total of about 180 parts;
[0053] The product density is set to 1400kg / m3, the glass fiber content is 45%, and the resin flow of components A and B is automatically calculated according to the mold size and speed. Then, the continuously measured polyurethane combination material is added to the reinforcing material. The glass fiber reinforced material and the polyurethane two-component mixture are evenly dispersed through the injection box 2, and after being fully mixed and impregnated by high-frequency ultrasound, they enter the double-layer crawler machine 6 mold for foaming and curing. The curing time is 40-60min, and the curing temperature is controlled between 50-90°C. After demoulding, the glass fiber reinforced polyurethane foam composite board is sawed. The performance test data of the product obtained in Example 1 are shown in Table 1.
[0054] Example 2
[0055] Formula of component A of polyurethane resin: 100 parts of polyol resin, 10 parts of flame retardant, 2 parts of silicone oil, and 0.2 parts of composite catalyst;
[0056] Polyurethane resin B component: 120 parts of polymerized MDI;
[0057] Reinforcement material: 60 layers of glass fiber mesh cloth with a surface density of 900g / m2, a total of about 190 parts;
[0058] The product density is set to 1400kg / m3, the glass fiber content is 55%, and the resin flow of components A and B is automatically calculated according to the mold size and speed. Then, the continuously measured polyurethane combination material is added to the reinforcing material. The glass fiber reinforced material and the polyurethane two-component mixture are evenly dispersed through the injection box 2, and after being fully mixed and impregnated by high-frequency ultrasound, they enter the double-layer crawler machine 6 mold for foaming and curing. The curing time is 40-60min, and the curing temperature is controlled between 50-90°C. After demoulding, the glass fiber reinforced polyurethane foam composite board is sawed. The performance test data of the product obtained in Example 2 is shown in Table 1.
[0059] Example 3
[0060] Formula of component A of polyurethane resin: 100 parts of polyol resin, 10 parts of flame retardant, 2 parts of silicone oil, and 0.2 parts of composite catalyst;
[0061] Polyurethane resin B component: 120 parts of polymerized MDI
[0062] Reinforcement material: 70 layers of glass fiber mesh cloth with a surface density of 900g / m2, totaling about 200 copies;
[0063] The product density is set to 1400kg / m3, the glass fiber content is 65%, and the resin flow of components A and B is automatically calculated according to the mold size and speed. Then, the continuously measured polyurethane combination material is added to the reinforcing material. The glass fiber reinforced material and the polyurethane two-component mixture are evenly dispersed through the injection box 2, and after being fully mixed and impregnated by high-frequency ultrasound, they enter the double-layer crawler machine 6 mold for foaming and curing. The curing time is 40-60min, and the curing temperature is controlled between 50-90°C. After demoulding, the glass fiber reinforced polyurethane foam composite board is sawed. The performance test data of the product obtained in Example 1 are shown in Table 1.
[0064] Embodiment 4:
[0065] In order to verify the mechanical strength of the glass fiber mesh cloth reinforced polyurethane composite materials prepared in Examples 1-3, the existing glass fiber bundles were replaced to prepare glass fiber reinforced polyurethane composite materials of Comparative Example 1 and Comparative Example 2, respectively, as follows:
[0066] The glass fiber reinforced polyurethane composite material of Comparative Example 1: 100 parts of polyol resin, 10 parts of flame retardant, 2 parts of silicone oil, 0.2 parts of composite catalyst; 120 parts of polymerized MDI; 655 bundles of 9600tex continuous glass fibers.
[0067] The glass fiber reinforced polyurethane composite material of Comparative Example 2: 100 parts of polyol resin, 10 parts of flame retardant, 2 parts of silicone oil, 0.2 parts of composite catalyst; 120 parts of polymerized MDI; 774 bundles of 9600tex continuous glass fibers.
[0068] The glass fiber reinforced polyurethane composite materials obtained in Comparative Example 1 and Comparative Example 2 in Examples 1-3 and Example 4 were tested, and the results are shown in Table 1.
[0069] Table 1 Performance evaluation of materials in various examples
[0070]
[0071] From the results, it can be seen that compared with the unidirectional reinforcement of the commonly used glass fiber bundles, the compressive strength (perpendicular to the fiber direction) is increased by more than 6 times. This is because the glass fiber mesh cloth used in the formula of the present invention is reinforced with glass fibers in the 0° and 90° directions, which greatly improves the mechanical strength of the product in the vertical direction, and the thermal conductivity coefficient is also reduced by about 4%.
[0072] It can be seen that the glass fiber reinforced polyurethane composite materials of Examples 1-3 provided by the present invention can have excellent mechanical properties and thermal insulation properties in an ultra-low temperature environment of -163°C, and can be used as LNG ship support materials. At the same time, they have the characteristics of maintaining high strength, high dimensional stability and high thermal insulation performance in an ultra-low temperature environment (-163°C), and the product has balanced performance in all directions, and has good punching, bonding and other processing properties similar to wood; a size-adjustable and customizable composite material plate is prepared, which has a high specific strength at low temperatures, and has good thermal insulation effect and flame retardancy.
[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite laminated wood for LNG ships, characterized in that: The laminated wood is composed of 100 parts of polymer polyol, 0.5-3 parts of surfactant, 0.1-0.5 parts of foaming agent, 0.1-2 parts of catalyst, 90-130 parts of polymer MDI and 50-250 parts of glass fiber reinforcement material; wherein the catalyst is an amine / organotin delayed catalyst or a trimerization catalyst, and the surface density of the glass fiber reinforcement material is 600-1800 g / m2; the preparation device of the laminated wood comprises a cloth placing rack (1), a glue injection box (2), a polyurethane glue injection machine (3), a guide roller (4), a high-frequency vibration auxiliary impregnation machine (5), a crawler machine (6) and a sawing machine (7); the cloth placing rack (1), the glue injection box (2), the guide roller (4), the high-frequency vibration auxiliary impregnation machine (5), the crawler machine (6) and the sawing machine (7) are sequentially distributed along the moving direction of the glass fiber reinforcement material, and the polyurethane glue injection machine (3) is used to transport polyurethane resin into the glue injection box (2); The glue injection box (2) comprises a glue injection channel, through which the glass fiber reinforced material passes and is mixed with the polyurethane resin in the glue injection channel, thus achieving a primary dipping effect; each glue injection channel passes through 1 to 3 layers of fiber reinforced material; a high-frequency vibration auxiliary impregnation machine (5) is arranged between the glue injection box (2) and the crawler machine (6), and is used to perform secondary vibration impregnation on the glass fiber reinforced material after the primary dipping, and heat and solidify the material in the mold cavity of the crawler machine (6); In addition, the polyurethane glue injection machine (3) comprises a mixer (33) and a diverter (34). The mixer (33) is used to mix the two components of materials output from the polyurethane group A tank (31) and the polyurethane group B tank (32). The diverter (34) is connected to a plurality of glue injection channels after diversion to inject glue into the glass fiber reinforced material. The mixer (33) transports the glue liquid flowing out of the glue storage tank to the inside of the glue injection box (2) through the glue injection channel connected to the diverter (34). Under the action of the crawler (6), the glass fiber reinforced material moves along the cloth placing frame (1), the glue injection box (2), the guide roller (4), the high-frequency vibration auxiliary impregnation machine (5), the crawler of the crawler (6) and the mold, and the sawing machine (7), and forms a composite material type laminated wood (8).
2. The composite laminated wood for LNG ships according to claim 1, characterized in that: The polymer polyol is a polyether polyol, the hydroxyl value of the polyether polyol is 300-500 mgKOH / g, the viscosity at room temperature is 400-6000 mPa·s, and the functionality is 3-6.
3. The composite laminated wood for LNG ships according to claim 1, characterized in that: The polymeric MDI is polyphenyl polymethylene polyisocyanate MDI, the isocyanate MDI has an isocyanate content of 30-32 wt % and a functionality of 2-3.
4. The composite laminated wood for LNG ships according to claim 1, characterized in that: The glass fiber reinforcement material is a composite of any one or more materials selected from glass fiber mesh cloth, biaxial cloth, and glass fiber mat.
5. A method for preparing composite laminated wood for LNG ships, characterized in that: For preparing a composite laminated wood for LNG ships according to any one of claims 1 to 4, the method comprises the following steps: Step 1: Placement and traction of glass fiber reinforced materials; Step 2: polyurethane resin injection; Step 3: impregnation of glass fiber reinforced materials; Step 4: Product curing and shaping; Step 5: De-moulding and sawing.
Citation Information
Cited By
Epoxy resin composition for LNG storage tank supporting seat and preparation method
CN121801259A