Carburizing and quenching strengthening process of 20Cr2Ni4 piston for hydraulic breaker

By simplifying and optimizing the carburizing and quenching process of the 20Cr2Ni4 piston, the problems of large deformation and long production cycle caused by the cumbersome carburizing and quenching process are solved, the hardness and performance of the piston are improved, and more efficient production is achieved.

CN117448833BActive Publication Date: 2024-11-05XUZHOU BUT CONSTR MASCH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311403556.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2024-11-05
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

The carburizing and quenching process of the existing 20Cr2Ni4 pistons is cumbersome, resulting in long production cycles, large deformations, uneven grinding, and uneven hardness, which affects the service performance.

Method used

Simplify the carburizing and quenching process, eliminate high-temperature tempering processes, adopt cycle processes of pre-oxidation, carburizing, slow cooling, quenching, cold treatment and low-temperature tempering, and optimize process parameters such as heating temperature, carbon potential control and atmosphere protection. Reduce the secondary heating process.

Benefits of technology

Significantly reduce the deformation of the piston, improve the surface hardness and uniformity of the carburized layer, enhance the martensite and austenite levels, improve the hardness of the core and impact absorption performance, shorten the production cycle, reduce costs, and improve economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117448833B_ABST
    Figure CN117448833B_ABST
Patent Text Reader

Abstract

The present invention discloses a carburizing and quenching strengthening process for a 20Cr2Ni4 piston for a hydraulic breaker, comprising the following steps: step 1, pre-oxidation treatment, placing the 20Cr2Ni4 piston for a hydraulic breaker in a preheating furnace, heating and heat preservation, and then taking it out of the furnace for carburizing; step 2, carburizing treatment, including three stages of heating, strong permeation, and diffusion; step 3, slow cooling treatment, placing the piston in the front chamber of the carburizing furnace, slow cooling; step 4, quenching treatment, heating and heat preservation of the piston, and then oil cooling; step 5, cold treatment, placing the piston in a cold treatment furnace, cooling and heat preservation, placing it at room temperature, and waiting for it to return to room temperature; step 6, low-temperature tempering treatment, placing the piston in a tempering furnace, heat preservation, and then air cooling; step 7, repeating steps 5 and 6, and the number of repetitions is 0-2 times. The present invention reduces the deformation of the 20Cr2Ni4 piston for a hydraulic breaker and shortens the production cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment of low-carbon alloy structural steel, in particular to a carburizing and quenching strengthening process for a 20Cr2Ni4 piston for a hydraulic breaker. Background Art

[0002] The complex service conditions and failure forms of the hydraulic breaker piston determine that it must have high surface wear resistance and sufficient impact fatigue resistance. Low-carbon alloy steel, such as 20Cr2Ni4, is selected as the material for manufacturing the piston. Through surface carburizing treatment, it can meet the requirements of high toughness and surface wear resistance of the core. At present, the carburizing and quenching strengthening treatment of 20Cr2Ni4 pistons at home and abroad includes carburizing, air cooling, high temperature tempering, quenching, low temperature tempering and other processes. Since the carburizing and quenching process is cumbersome, it requires two heating processes and a long production cycle, which not only causes high consumption costs, but also causes problems such as large deformation of the piston. For cylindrical pistons, due to large deformation and large amount of grinding in the later stage of the piston, the piston carburizing layer after grinding is seriously uneven, the hardness is uneven and reduced, and the service performance is reduced. Therefore, it is necessary to improve the carburizing and quenching strengthening process of 20Cr2Ni4 pistons for hydraulic breaker hammers, simplify the process, and optimize the process parameters in the process to reduce the deformation of the piston workpiece. Summary of the invention

[0003] The purpose of the invention is to provide a carburizing and quenching strengthening process for a 20Cr2Ni4 piston for a hydraulic breaker, so as to reduce the deformation of the 20Cr2Ni4 piston for a hydraulic breaker and shorten the production cycle.

[0004] To achieve the above object, the present invention adopts the following technical solution:

[0005] A carburizing and quenching strengthening process for a 20Cr2Ni4 piston for a hydraulic breaker comprises the following steps:

[0006] Step 1, pre-oxidation treatment, placing the 20Cr2Ni4 piston for hydraulic breaker in a preheating furnace, heating and heat preservation, and then taking it out of the furnace for carburizing;

[0007] Step 2, carburizing treatment, including three stages: heating, strong carburizing, and diffusion;

[0008] Step 3, slow cooling treatment, placing the piston in the front chamber of the carburizing furnace and slow cooling;

[0009] Step 4: quenching treatment, heating and keeping the piston warm, and then oil cooling;

[0010] Step 5, cold treatment, placing the piston in a cold treatment furnace, cooling and keeping the temperature, and then placing it at room temperature until it returns to room temperature;

[0011] Step 6, low temperature tempering treatment, placing the piston in a tempering furnace, keeping warm, and then air cooling;

[0012] Step 7, repeat steps 5 and 6, the number of repetitions is 0-2 times.

[0013] Furthermore, in the step 1, heating is performed in an air atmosphere at a heating temperature of 500° C. and a heat preservation time of 60 minutes.

[0014] Furthermore, in step 2, the heating stage is to keep the piston at 750°C after entering the carburizing furnace, and the holding time is calculated as "piston diameter / 1.5mm" minutes, and then keep it at 850°C, and the holding time is calculated as "piston diameter / 1.5mm" minutes, and the carburizing atmosphere is controlled to maintain the carbon potential at 0.6% in the heating stage; the temperature of the strong carburizing and diffusion stages is 935°C~950°C, the holding time of the strong carburizing stage is 630-1000 minutes, the carbon potential is 1.1~1.25%, and the holding time of the diffusion stage is 670~800 minutes, and the carbon potential is 0.75%; then the piston is kept at 850±10°C, the holding time is calculated as "piston diameter / 1.5mm" minutes, and the carbon potential is 0.75%.

[0015] Furthermore, in step 2, the carburizing atmosphere is nitrogen, methanol and propane.

[0016] Furthermore, in the step 3, the temperature is slowly cooled to 400° C. under the protection of a nitrogen atmosphere.

[0017] Furthermore, in step 4, the piston is kept at 850±10°C, the holding time is calculated as "piston diameter / 0.75mm" minutes, the carbon potential is 0.75%, and then oil-cooled, the quenching oil temperature is 60°C, and the holding time in the quenching oil is calculated as "piston diameter / 1.5mm" minutes.

[0018] Furthermore, in step 4, the quenching oil used in the quenching treatment should be stirred in advance, and the stirring should be stopped 10 minutes before the piston is quenched, and the quenching oil should continue to be stirred 20 seconds after the piston enters the quenching oil for quenching, and the stirring frequency is 20-30 Hz.

[0019] Furthermore, in step 5, the piston is placed in a cold treatment furnace, the temperature is lowered to -100°C, and after being kept warm for "piston diameter / 1.5 mm" minutes, it is placed at room temperature and allowed to return to room temperature.

[0020] Furthermore, in step 6, the piston is placed in a tempering furnace at a temperature of 190° C., and the holding time is calculated as “piston diameter / 0.6 mm” minutes, followed by air cooling.

[0021] Furthermore, the chemical composition of the material of the 20Cr2Ni4 piston meets the requirements of GB / T3077-2015 standard; the smelting method of the material of the 20Cr2Ni4 piston is electric furnace smelting, electroslag remelting and refining, forging adopts free forging, forging ratio ≥3, 880-940℃ normalizing.

[0022] Beneficial effect: The carburizing and quenching strengthening process of the 20Cr2Ni4 piston for a hydraulic breaker provided by the present invention is not only applicable to the large-diameter carburizing and quenching 20Cr2Ni4 piston of the hydraulic breaker, but also applicable to the carburizing and quenching 20Cr2Ni4 piston of other hydraulic breakers, and also applicable to all other workpieces of 20Cr2Ni4 materials that need to be carburized and quenched. The carburizing and quenching strengthening process of the 20Cr2Ni4 piston for a hydraulic breaker provided by the present invention optimizes the carburizing and quenching process parameters of the 20Cr2Ni4 piston, and simplifies the carburizing and quenching process of the 20Cr2Ni4 piston, that is, the "high temperature tempering" process after carburizing air cooling is omitted, and it is changed to quenching after carburizing slow cooling, combined with the cyclic cold treatment process, so that the deformation of the 20Cr2Ni4 piston is greatly reduced, and the performance indicators of the 20Cr2Ni4 piston such as the surface hardness, thickness of the carburized layer, martensite level, residual austenite level, core hardness, and core impact absorption work can also meet the requirements of the piston. The invention solves the problems of serious uneven carburized layer, uneven and decreased hardness, and decreased service performance caused by large deformation in carburizing and quenching process, thereby improving the quality, surface hardness, and wear resistance of 20Cr2Ni4 piston; reduces the secondary heating process, shortens the production cycle, improves production efficiency, reduces production cost, and thus improves economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 1;

[0024] Figure 2 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 1;

[0025] Figure 3 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 2;

[0026] Figure 4 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 2;

[0027] Figure 5 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 3;

[0028] Figure 6 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 3;

[0029] Figure 7 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 4;

[0030] Figure 8 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 4;

[0031] Fig. 9 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 5;

[0032] Fig.10 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 5;

[0033] Fig.11 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 6;

[0034] Fig.12 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 6;

[0035] Fig.13 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 7;

[0036] Fig.14 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 7;

[0037] Fig.15 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 8;

[0038] Fig.16 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 8;

[0039] Fig.17 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 9;

[0040] Fig.18 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 9;

[0041] Fig.19 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in Example 10;

[0042] Fig. 20 This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in Example 10;

[0043] Fig.21 This is a metallographic photograph of the surface of the 20Cr2Ni4 piston obtained in the comparative example;

[0044] Fig. 22This is a metallographic photograph of the core of the 20Cr2Ni4 piston obtained in the comparative example. DETAILED DESCRIPTION

[0045] The present invention provides a carburizing and quenching strengthening process for a 20Cr2Ni4 piston for a hydraulic breaker. The chemical composition of the material of the 20Cr2Ni4 piston meets the requirements of the GB / T3077-2015 standard. The smelting method of the material of the 20Cr2Ni4 piston is electric furnace smelting, electroslag remelting and refining, free forging is used for forging, the forging ratio is ≥3, and the 880-940℃ normalizing is used.

[0046] The carburizing and quenching strengthening process of a 20Cr2Ni4 piston for a hydraulic breaker of the present invention comprises the following steps:

[0047] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0048] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston is kept at 750°C after entering the carburizing furnace, and the holding time is calculated as "piston diameter / 1.5 mm" minutes. Then the piston is kept at 850°C, and the holding time is calculated as "piston diameter / 1.5 mm" minutes. Nitrogen, methanol and propane are introduced into the carburizing furnace to maintain the carbon potential at 0.6% during the heating stage. The temperature of the strong carburizing and diffusion stages is 935°C to 950°C. The holding time of the strong carburizing stage is 630-1000 minutes, and the carbon potential is 1.1-1.25%. The holding time of the diffusion stage is 670-800 minutes, and the carbon potential is 0.75%. Then the piston is kept at 850±10°C, and the holding time is calculated as "piston diameter / 1.5 mm" minutes, and the carbon potential is 0.75%;

[0049] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0050] (4) Quenching treatment: after the slow cooling stage, the piston is kept at 850±10°C for a holding time calculated as “piston diameter / 0.75 mm” minutes, with a carbon potential of 0.75%, and then immersed in quenching oil for cooling. The quenching oil temperature is 60°C, and the holding time in the quenching oil is calculated as “piston diameter / 1.5 mm” minutes;

[0051] The quenching oil used in the quenching treatment should be stirred in advance. The stirring should be stopped 10 minutes before the piston is quenched. The quenching oil should be stirred again 20 seconds after the piston enters the quenching oil for quenching. The stirring frequency is 20-30Hz.

[0052] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for "piston diameter / 1.5 mm" minutes, place it at room temperature, and wait for it to return to room temperature;

[0053] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at a temperature of 190°C for a holding time calculated as "piston diameter / 0.6 mm" minutes, and then air cool to room temperature;

[0054] (7) Repeat steps 5 and 6 0-2 times.

[0055] The present invention will be further described below in conjunction with the embodiments.

[0056] Example 1

[0057] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0058] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0059] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The holding time in the strong carburizing stage is 1000 minutes, and the carbon potential is 1.1%. The holding time in the diffusion stage is 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0060] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0061] (4) Quenching treatment: keep at 850°C for 240 minutes, carbon potential is 0.75%, then immerse in quenching oil for cooling, quenching oil temperature is 60°C, keep in quenching oil for 120 minutes, and stir the quenching oil at a frequency of 25 Hz;

[0062] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0063] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature.

[0064] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 1 were tested. The performance test results are shown in Table 1, and the metallographic photos of the surface and the core are shown in Table 1. Figure 1 and Figure 2 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0065] Table 1 Performance index of Example 1

[0066]

[0067] Example 2

[0068] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0069] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0070] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The holding time in the strong carburizing stage is 1000 minutes, and the carbon potential is 1.1%. The holding time in the diffusion stage is 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0071] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0072] (4) Quenching treatment: keep warm at 840°C for 240 minutes, with a carbon potential of 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, and keep warm in the quenching oil for 120 minutes. The quenching oil stirring frequency is 20 Hz.

[0073] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0074] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature.

[0075] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 2 were tested. The performance test results are shown in Table 2, and the metallographic photos of the surface and the core are shown in Table 2. Figure 3 and Figure 4 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0076] Table 2 Performance index of Example 2

[0077]

[0078] Example 3

[0079] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0080] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0081] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The holding time in the strong carburizing stage is 1000 minutes, and the carbon potential is 1.1%. The holding time in the diffusion stage is 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0082] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0083] (4) Quenching treatment: keep the temperature at 860°C for 240 minutes, the carbon potential is 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, keep the temperature in the quenching oil for 120 minutes, and the quenching oil stirring frequency is 30 Hz.

[0084] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0085] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature.

[0086] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 3 were tested. The performance test results are shown in Table 3, and the metallographic photos of the surface and the core are shown in Table 3. Figure 5 and Figure 6 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0087] Table 3 Performance index of Example 3

[0088]

[0089] Example 4

[0090] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0091] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0092] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The strong carburizing stage is kept for 900 minutes, and the carbon potential is 1.15%. The diffusion stage is kept for 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0093] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0094] (4) Quenching treatment: keep warm at 850°C for 240 minutes, with a carbon potential of 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, and keep warm in the quenching oil for 120 minutes. The quenching oil stirring frequency is 25 Hz.

[0095] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0096] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature.

[0097] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 4 were tested. The performance test results are shown in Table 4, and the metallographic photos of the surface and the core are shown in Table 4. Figure 7 and Figure 8 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0098] Table 4 Performance index of Example 4

[0099]

[0100] Example 5

[0101] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0102] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0103] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The strong carburizing stage is kept for 760 minutes, and the carbon potential is 1.25%. The diffusion stage is kept for 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0104] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0105] (4) Quenching treatment: keep warm at 850°C for 240 minutes, with a carbon potential of 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, and keep warm in the quenching oil for 120 minutes. The quenching oil stirring frequency is 25 Hz.

[0106] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0107] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature.

[0108] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 5 were tested. The performance test results are shown in Table 5. The metallographic photos of the surface and the core are shown in Table 5. Fig. 9 and Fig.10 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0109] Table 5 Performance index of Example 5

[0110]

[0111] Example 6

[0112] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0113] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0114] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 940°C. The strong carburizing stage is kept for 860 minutes, and the carbon potential is 1.15%. The diffusion stage is kept for 760 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0115] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0116] (4) Quenching treatment: keep warm at 850°C for 240 minutes, with a carbon potential of 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, and keep warm in the quenching oil for 120 minutes. The quenching oil stirring frequency is 25 Hz.

[0117] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0118] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature.

[0119] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 6 were tested. The performance test results are shown in Table 6. The metallographic photos of the surface and the core are shown in Table 6. Fig.11 and Fig.12 As shown, its performance indicators meet the requirements and the diameter increases by 7-12μm.

[0120] Table 6 Performance index of Example 6

[0121]

[0122] Example 7

[0123] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0124] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0125] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 950°C. The strong carburizing stage is kept for 630 minutes, and the carbon potential is 1.25%. The diffusion stage is kept for 680 minutes, and the carbon potential is 0.75%. The piston is kept at 850°C for 120 minutes, and the carbon potential is 0.75%.

[0126] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0127] (4) Quenching treatment: keep warm at 850°C for 240 minutes, with a carbon potential of 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, and keep warm in the quenching oil for 120 minutes. The quenching oil stirring frequency is 25 Hz.

[0128] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0129] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature.

[0130] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 7 were tested. The performance test results are shown in Table 7. The metallographic photos of the surface and the core are shown in Table 7. Fig.13 and Fig.14 As shown, its performance indicators meet the requirements and the diameter increases by 7-13μm.

[0131] Table 7 Performance index of Example 7

[0132]

[0133] Example 8

[0134] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0135] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0136] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The strong carburizing stage is kept for 900 minutes, and the carbon potential is 1.15%. The diffusion stage is kept for 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0137] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0138] (4) Quenching treatment: keep warm at 850°C for 240 minutes, with a carbon potential of 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, and keep warm in the quenching oil for 120 minutes. The quenching oil stirring frequency is 25 Hz.

[0139] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0140] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature;

[0141] (8) Repeat steps 4 and 5.

[0142] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 8 were tested. The performance test results are shown in Table 8, and the metallographic photos of the surface and the core are shown in Table 8. Fig.15 and Fig.16 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0143] Table 8 Performance index of Example 8

[0144]

[0145] Example 9

[0146] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0147] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0148] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The strong carburizing stage is kept for 900 minutes, and the carbon potential is 1.15%. The diffusion stage is kept for 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 120 minutes, and the carbon potential is 0.75%.

[0149] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0150] (4) Quenching treatment: keep warm at 850°C for 240 minutes, with a carbon potential of 0.75%, and then immerse in quenching oil for cooling. The quenching oil temperature is 60°C, and keep warm in the quenching oil for 120 minutes. The quenching oil stirring frequency is 25 Hz.

[0151] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it warm for 120 minutes, place it at room temperature, and wait for it to return to room temperature;

[0152] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes and then air cool to room temperature;

[0153] (7) Repeat steps 4 and 5 two more times.

[0154] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 9 were tested. The performance test results are shown in Table 9, and the metallographic photos of the surface and the core are shown in Table 9. Fig.17 and Fig.18 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0155] Table 9 Performance index of Example 9

[0156]

[0157] Example 10

[0158] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 210mm is carburized and quenched to strengthen the process, including the following steps:

[0159] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0160] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 140 minutes, and then kept at 850°C for 140 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The strong carburizing stage is kept for 900 minutes, and the carbon potential is 1.15%. The diffusion stage is kept for 800 minutes, and the carbon potential is 0.75%. The piston is kept at 850 for 140 minutes, and the carbon potential is 0.75%.

[0161] (3) Slow cooling treatment: place the piston in the antechamber of the carburizing furnace and slowly cool it to 400°C under the protection of nitrogen atmosphere;

[0162] (4) Quenching treatment: keep at 850°C for 280 minutes, carbon potential is 0.75%, then immerse in quenching oil for cooling, quenching oil temperature is 60°C, keep in quenching oil for 140 minutes, and stir the quenching oil at a frequency of 25 Hz;

[0163] (5) Cold treatment: place the piston in a cold treatment furnace, lower the temperature to -100°C, keep it at that temperature for 140 minutes, and then place it at room temperature until it returns to room temperature;

[0164] (6) Low-temperature tempering treatment: the piston is placed in a tempering furnace at 190°C for 350 minutes and then air-cooled to room temperature;

[0165] (7) Repeat steps 4 and 5.

[0166] The performance indicators of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in Example 10 were tested. The performance test results are shown in Table 10, and the metallographic photos of the surface and the core are shown in Table 10. Fig.19 and Fig. 20 As shown, its performance indicators meet the requirements and the diameter increases by 5-9μm.

[0167] Table 10 Performance index of embodiment 10

[0168]

[0169] Comparative Example

[0170] The 20Cr2Ni4 piston material for the breaker has the following chemical compositions: C: 0.194wt.%; Mn: 0.531wt.%; Si: 0.271wt.%; P: 0.005wt.%; S: 0.001wt.%; Cr: 1.631wt.%; Ni: 3.579wt.%; Cu: 0.028wt.%. The piston with a diameter of 180mm is carburized and quenched, and the following steps are included:

[0171] (1) Pre-oxidation treatment: the piston is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0172] (2) carburizing treatment, including three stages: heating, strong carburizing and diffusion. The heating stage is that the piston enters the carburizing furnace and is kept at 750°C for 120 minutes, and then kept at 850°C for 120 minutes. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 935°C. The holding time in the strong carburizing stage is 1000 minutes, and the carbon potential is 1.1%. The holding time in the diffusion stage is 800 minutes, and the carbon potential is 0.75%.

[0173] (3) Cooling treatment: first keep the temperature at 860℃ for 2h, then cool to 500℃ with nitrogen blowing, and then air cool to room temperature after taking out of the furnace;

[0174] (4) High temperature tempering treatment: keep the temperature at 630℃ for 300 minutes, cool to 500℃ with nitrogen blowing, and then take out of the furnace and air cool;

[0175] (5) Quenching treatment: first keep it at 750°C for 120 minutes, then keep it at 850°C for 120 minutes, the carbon potential is 0.6%, and then immerse it in quenching oil for cooling, the quenching oil temperature is 60°C, keep it in the quenching oil for 120 minutes, and the quenching oil stirring frequency is 25 Hz.

[0176] (6) Low-temperature tempering treatment: place the piston in a tempering furnace at 190°C for 300 minutes, then air cool to room temperature and repeat the low-temperature tempering process.

[0177] The performance indexes of the 20Cr2Ni4 piston obtained after carburizing and quenching heat treatment in the comparative example were tested. The performance test results are shown in Table 11, and the metallographic photos of the surface and the core are shown in Table 11. Fig.21 and Fig. 22 As shown, the carbide level is relatively high, the diameter increases by 7-22 μm, and the deformation is much greater than the piston obtained in the embodiment.

[0178] Table 11 Comparative Examples Performance Index

[0179]

[0180] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A carburizing and quenching strengthening process for a 20Cr2Ni4 piston for a hydraulic breaker, characterized in that: The following steps are involved: Step 1, pre-oxidation treatment, placing the 20Cr2Ni4 piston for hydraulic breaker in a preheating furnace, heating it in an air atmosphere at a heating temperature of 500°C for 60 minutes, and then taking it out of the furnace for carburizing; Step 2, carburizing treatment, including three stages: heating, strong carburizing, and diffusion; The heating stage is that the piston is kept at 750°C after entering the carburizing furnace, and the holding time is calculated as "piston diameter / 1.5mm" minutes, and then kept at 850°C, and the holding time is calculated as "piston diameter / 1.5mm" minutes, and the carburizing atmosphere is controlled to maintain the carbon potential at 0.6% in the heating stage; the temperature of the strong carburizing and diffusion stages is 935°C~950°C, the holding time of the strong carburizing stage is 630-1000 minutes, the carbon potential is 1.1~1.25%, the holding time of the diffusion stage is 670~800 minutes, and the carbon potential is 0.75%; then the piston is kept at 850±10°C, the holding time is calculated as "piston diameter / 1.5mm" minutes, and the carbon potential is 0.75%; the carburizing atmosphere is nitrogen, methanol and propane; Step 3, slow cooling treatment, placing the piston in the antechamber of the carburizing furnace and slowly cooling it to 400° C. under the protection of a nitrogen atmosphere; Step 4: quenching treatment, heating and keeping the piston warm, and then oil cooling; Step 5, cold treatment, placing the piston in a cold treatment furnace, cooling and keeping the temperature, and then placing it at room temperature until it returns to room temperature; Step 6, low temperature tempering treatment, placing the piston in a tempering furnace, keeping warm, and then air cooling; Step 7, repeat steps 5 and 6, the number of repetitions is 0-2 times.

2. The carburizing and quenching strengthening process of a 20Cr2Ni4 piston for a hydraulic breaker according to claim 1 is characterized in that: In step 4, the piston is kept at 850±10°C for a holding time calculated as "piston diameter / 0.75mm" minutes, the carbon potential is 0.75%, and then oil-cooled, the quenching oil temperature is 60°C, and the holding time in the quenching oil is calculated as "piston diameter / 1.5mm" minutes.

3. The carburizing and quenching strengthening process of a 20Cr2Ni4 piston for a hydraulic breaker according to claim 1 or 2, characterized in that: In step 4, the quenching oil used in the quenching treatment should be stirred in advance, and the stirring is stopped 10 minutes before the piston is quenched. The quenching oil is continued to be stirred 20 seconds after the piston enters the quenching oil for quenching, and the stirring frequency is 20-30 Hz.

4. The carburizing and quenching strengthening process of a 20Cr2Ni4 piston for a hydraulic breaker according to claim 1 is characterized in that: In the step 5, the piston is placed in a cold treatment furnace, the temperature is lowered to -100°C, and the temperature is kept for "piston diameter / 1.5 mm" minutes, and then placed at room temperature to be restored to room temperature.

5. The carburizing and quenching strengthening process of a 20Cr2Ni4 piston for a hydraulic breaker according to claim 1 is characterized in that: In step 6, the piston is placed in a tempering furnace at a temperature of 190° C., the holding time is calculated as “piston diameter / 0.6 mm” minutes, and then air-cooled.

6. The carburizing and quenching strengthening process of a 20Cr2Ni4 piston for a hydraulic breaker according to claim 1 is characterized in that: The chemical composition of the material of the 20Cr2Ni4 piston meets the requirements of GB / T3077-2015 standard; the smelting method of the material of the 20Cr2Ni4 piston is electric furnace smelting, electroslag remelting and refining, forging adopts free forging, forging ratio ≥3, 880-940℃ normalizing.