Antibacterial and mildew-proof sanitary packaging bag and preparation process thereof
By uniformly adding and stirring antibacterial and anti-mold resin particles in the film body, the agglomeration problem of resin particles is solved, the antibacterial effect and stability of the packaging bag are improved, the shelf life is extended, and the mechanical properties of the film are enhanced.
Patent Information
- Application Number
- CN202410349109.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing antibacterial and anti-mold resin particles are prone to agglomeration in the film, resulting in a decrease in antibacterial effect and affecting the shelf life and stability of the packaging bag.
Antibacterial and anti-mold resin particles made of submicron glass, silver ion salt, zinc ion salt and copper ion salt are uniformly added to the membrane, and stirred at a rotation speed of 400-500rpm for 4-5 hours to form a uniformly distributed resin particle The antibacterial layer increases the chance of contact between particles and PE substrates, breaks agglomerated particles, and improves the stability and antibacterial effect of the membrane.
The uniform distribution of antibacterial and anti-mold resin particles in the film body is achieved, the antibacterial effect and durability of the film body is improved, the antibacterial and anti-mold time of the packaging bag is extended, and the mechanical properties and stability of the film are enhanced.
Smart Images

Figure CN118181913B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging bags, in particular to an antibacterial and mildew-proof hygienic packaging bag and a preparation process thereof. Background Art
[0002] At present, most of the films used for daily sanitation products and food packaging have no antibacterial effect, especially the films used for medicine and food packaging, which are used to achieve various barrier functions and generally adopt co-extruded films; and daily sanitation products are only packaged in simple single-layer or multi-layer single non-barrier and antibacterial film product packaging bags. Since there is no packaging film with good antibacterial effect at present, the products are exposed after the bags are opened, which is easy to breed bacteria, expire and deteriorate, and have a short shelf life.
[0003] For example, a Chinese patent with announcement number CN113183573B discloses an antibacterial and mildew-proof sanitary packaging bag and its preparation process, wherein the ink layer printed on the surface of the film contains an antibacterial agent; the content of the antibacterial agent in the ink layer accounts for 3.0-5.0% of the total weight of the ink layer; the film contains antibacterial and mildew-proof resin particles. The beneficial effects of this invention are: a mixture of three antibacterial and mildew-proof components, namely, silver ion salt, zinc ion salt, and copper ion salt, is used, and zinc ion salt and copper ion salt are attached to the surface of silver ion salt particles, which can effectively reduce and control the migration and loss rate of the silver ion salt, thereby extending the antibacterial and mildew-proof time of the packaging bag.
[0004] However, the diameter of the antibacterial and anti-mildew resin particles in the comparative documents is less than 0.5 microns, which makes them easily aggregated, causing them to aggregate in the membrane body, reducing the antibacterial effect and affecting the efficacy of the membrane. Summary of the invention
[0005] The embodiment of the present application solves the agglomeration problem of antibacterial and mildew-proof resin particles in the prior art by providing an antibacterial and mildew-proof hygienic packaging bag and a preparation process thereof, thereby achieving better dispersion and improving the antibacterial effect.
[0006] The present application provides an antibacterial and mildew-proof hygienic packaging bag and a preparation process thereof, and the specific steps include:
[0007] S1, adding antibacterial and mildew-proof resin particles composed of 60 parts by weight of submicron glass, 15 parts by weight of silver ion salt, 13 parts by weight of zinc ion salt and 10 parts by weight of copper ion salt evenly into the film body, stirring evenly at a speed of 400-500 rpm for 4-5 hours, the added amount accounting for 1-1.5% of the total added amount of the film body, and blowing the film according to the above ratio;
[0008] S2, printing colored ink and varnish ink on the surface of the film in sequence, wherein the ink contains antibacterial ingredients;
[0009] S3, compounding the two printed films and forming an ink layer between the two films;
[0010] S4, cutting into packaging bags with a film thickness of 23-110 microns.
[0011] Furthermore, in step S1, the diameter of the submicron glass is 0.2-0.5 microns.
[0012] Furthermore, in step S1, the silver ion salt is a mixture of silver carbonate and silver bromide in a weight ratio of 2:1, and the silver ion salt particle diameter is 50-100 nanometers, the zinc ion salt is zinc oxide, and the copper ion salt is cuprous oxide. The weight ratio between the zinc ion salt and the copper ion salt is 2:1, and the particle diameters of the zinc ion salt and the copper ion salt are 3-10 nanometers.
[0013] Furthermore, in step S1, the film body is composed of 100 parts by weight of PE substrate and 1-1.5 parts by weight of antibacterial and antifungal resin particles.
[0014] Furthermore, in step S2, the antibacterial component is an antibacterial agent, the components are 40 parts by weight of n-butylisothiazolinone, 55 parts by weight of dipropylene glycol, and 5 parts of a stabilizer, and the added amount is 1-1.5% of the total mass of the ink.
[0015] Furthermore, in step S2, the antibacterial component is antibacterial and mildew-proof resin particles, and the added amount is 1-1.5% of the total mass of the ink. After adding the antibacterial and mildew-proof resin particles, the ink is stirred evenly at a speed of 400-500 rpm for 4-5 hours.
[0016] Furthermore, in step S2, the colored ink and the varnish ink are printed on the surface of the film in sequence; the printing is performed twice on the surface of the film to form two layers of ink;
[0017] The ink layer near the film body contains antibacterial and anti-mildew resin particles, and its components include, by weight: 60 parts of submicron glass, 10 parts of silver ion salt, 13 parts of zinc ion salt and 10 parts of copper ion salt;
[0018] The ink layer away from the film body contains antibacterial and anti-mildew resin particles, and its components include 60 parts of submicron glass, 15 parts of silver ion salt, 6 parts of zinc ion salt and 5 parts of copper ion salt by weight.
[0019] Furthermore, in step S3, the film body printed with two layers of ink in step S2 is compounded with the film body not printed with ink, so that an intermediate ink layer is formed between the two films.
[0020] Furthermore, in step S2, the film without ink printed thereon comprises by weight: 100 parts of submicron glass, 10 parts by weight of silver ion salt, 13 parts by weight of zinc ion salt and 10 parts by weight of copper ion salt; wherein the diameter of the submicron glass is 0.5-1.0 micrometer.
[0021] An antibacterial and mildew-proof sanitary packaging bag is made by the above-mentioned preparation process of the antibacterial and mildew-proof sanitary packaging bag.
[0022] One or more technical solutions provided in the embodiments of the present application have at least the following technical effects or advantages:
[0023] First, break up the agglomerated particles to make them more evenly distributed in the film. Long-term stirring can increase the contact opportunities between the antibacterial and mildew-proof resin particles and the PE substrate, thereby promoting their compatibility and bonding strength, reducing the shedding or migration of particles during use, and improving the stability and durability of the film.
[0024] Secondly, adding antibacterial and mildew-proof resin particles to the ink can improve the antibacterial and mildew-proof capabilities of the film surface. Through long-term stirring, the antibacterial and mildew-proof resin particles can be more evenly distributed in the ink, forming a uniform and continuous antibacterial layer during the printing process, thereby improving the overall antibacterial effect of the film. Stirring promotes the compatibility between the antibacterial and mildew-proof resin particles and the ink, ensuring that the particles can be stably suspended in the ink without sedimentation or agglomeration, thereby maintaining the stability of the printing process and the uniformity of the ink. Adding antibacterial and mildew-proof resin particles to the ink can seal the antibacterial and mildew-proof resin particles to prevent them from falling off or becoming ineffective during use, thereby maintaining the aesthetics and functionality of the film. At the same time, the antibacterial and mildew-proof resin particles in the ink adsorb the antibacterial and mildew-proof resin particles in the inner and outer layers, thereby reducing the possibility of outer layer particles falling off, and the particles in the middle layer can also maintain a longer antibacterial effect.
[0025] Third, the ink layer close to the outer film uses a lower content of silver ion salt and a higher content of zinc ion salt and copper ion salt. This ratio can ensure the antibacterial effect while absorbing more antibacterial and mildew-proof resin particles in the outer layer and the ink layer far away from the outer film, so that more of them are kept in the film body, and the silver ion migration caused by external environmental changes or air oxygen is prevented. The ink layer far away from the outer film uses a higher content of silver ion salt and a lower content of zinc ion salt and copper ion salt, so that it is in a more stable area, enhancing the antibacterial ability of the inner layer of ink and ensuring the overall antibacterial effect of the film. At the same time, brushing two layers of ink on a film can better protect the ink layer, reduce possible damage or defects during the composite process, and maintain the integrity and functionality of the ink layer.
[0026] Fourth, glass particles with larger diameters can provide stronger support, increase the tensile strength and tear resistance of the film, and when ink penetrates into the gaps between these glass particles, a more continuous and solid network structure will be formed, further improving the mechanical properties of the film. After the ink penetrates into the gaps between the glass in the inner film, it can increase the internal bonding force of the film and reduce the risk of peeling between layers. This means that the composite film can better maintain its integrity and functionality when used for a long time or subjected to external pressure. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a flow chart of an antibacterial and mildew-proof sanitary packaging bag and its preparation process. DETAILED DESCRIPTION
[0028] To facilitate the understanding of the present invention, the present application will be described more comprehensively below with reference to the relevant drawings; the drawings show preferred embodiments of the present invention, but the present invention can be implemented in many different forms and is not limited to the embodiments described herein; on the contrary, the purpose of providing these embodiments is to enable a more thorough and comprehensive understanding of the disclosed content of the present invention.
[0029] It should be noted that the terms “vertical”, “horizontal”, “up”, “down”, “left”, “right” and similar expressions used in this document are only for illustrative purposes and do not represent the only implementation method.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the term "and / or" used herein includes any and all combinations of one or more related listed items.
[0031] Embodiment 1
[0032] The present application discloses an antibacterial and mildew-proof hygienic packaging bag and a preparation process thereof, comprising the following steps:
[0033] S1, adding antibacterial and mildew-proof resin particles composed of 60 parts by weight of submicron glass, 15 parts by weight of silver ion salt, 13 parts by weight of zinc ion salt and 10 parts by weight of copper ion salt evenly into the film body, stirring evenly at a speed of 400-500 rpm for 4-5 hours, the added amount accounting for 1-1.5% of the total added amount of the film body, and blowing the film according to the above ratio;
[0034] The diameter of the mid-submicron glass is 0.2-0.5 microns, the silver ion salt is a mixture of silver carbonate and silver bromide in a weight ratio of 2:1, and the diameter of the silver ion salt particles is 50-100 nanometers, the zinc ion salt is zinc oxide, the copper ion salt is cuprous oxide, the weight ratio between the zinc ion salt and the copper ion salt is 2:1, and the particle diameters of the zinc ion salt and the copper ion salt are 3-10 nanometers; the membrane body is composed of 100 parts by weight of PE substrate and 1-1.5 parts by weight of antibacterial and mildew-proof resin particles;
[0035] S2, printing colored ink and varnish ink on the surface of the film in sequence, wherein the ink contains an antibacterial agent accounting for 1-1.5% of the total weight of the ink; the components of the antibacterial agent are 40 parts by weight of n-butylisothiazolinone, 55 parts by weight of dipropylene glycol, and 5 parts of a stabilizer;
[0036] S3, compounding the two printed films and forming an ink layer between the two films;
[0037] S4, cutting into packaging bags with a film thickness of 23-110 microns;
[0038] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0039] Break up the agglomerated particles and make them more evenly distributed in the film. Long-term stirring can increase the contact opportunities between the antibacterial and mildew-proof resin particles and the PE substrate, thereby promoting their compatibility and bonding, reducing the shedding or migration of particles during use, and improving the stability and durability of the film. At a stirring speed of 400-500rpm, the flow force and shear force break up the agglomeration of particles, but will not break up the metal ions, thereby increasing the uniformity of the film and maintaining the antibacterial effect. Adding only 1-1.5% antibacterial and mildew-proof resin particles can also achieve the original effect.
[0040] Embodiment 2
[0041] The above embodiment improves the uniformity of the film by breaking up the agglomeration of particles, thereby reducing the amount of antibacterial and mildew-proof resin particles while maintaining the antibacterial effect, and further improves the antibacterial time.
[0042] S2, printing colored ink and varnish ink on the surface of the film in sequence;
[0043] The ink contains 1-1.5% of the total weight of the ink in antibacterial and mildew-proof resin particles; after adding the antibacterial and mildew-proof resin particles, the ink is stirred evenly at a speed of 400-500 rpm for 4-5 hours;
[0044] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0045] Adding antibacterial and mildew-proof resin particles to the ink can improve the antibacterial and mildew-proof capabilities of the film surface. Through long-term stirring, the antibacterial and mildew-proof resin particles are ensured to be more evenly distributed in the ink, forming a uniform and continuous antibacterial layer during the printing process, improving the overall antibacterial effect of the film. Stirring promotes the compatibility between the antibacterial and mildew-proof resin particles and the ink, ensuring that the particles can be stably suspended in the ink without sedimentation or agglomeration, maintaining the stability of the printing process and the uniformity of the ink;
[0046] Adding antibacterial and mildew-proof resin particles to the ink can seal the antibacterial and mildew-proof resin particles to prevent them from falling off or becoming ineffective during use, thereby maintaining the aesthetics and functionality of the film. At the same time, the antibacterial and mildew-proof resin particles in the ink adsorb the antibacterial and mildew-proof resin particles in the inner and outer layers, reducing the possibility of outer layer particles falling off, and the particles in the middle layer can also maintain a longer-lasting antibacterial effect.
[0047] Embodiment 3
[0048] Embodiment 2 adds antibacterial and antifungal resin particles to the ink of the middle layer to increase the antibacterial time, thereby further improving the stability of silver ions.
[0049] S2, printing colored ink and varnish ink on the surface of the outer film in sequence; and printing twice;
[0050] The ink contains 1-1.5% of the total weight of the ink antibacterial and mildew-proof resin particles; after adding the antibacterial and mildew-proof resin particles, the ink is stirred evenly at a speed of 400-500 rpm for 4-5 hours; the antibacterial and mildew-proof resin particles in the ink layer close to the outer film include, by weight, 60 parts of submicron glass, 10 parts of silver ion salt, 13 parts of zinc ion salt and 10 parts of copper ion salt; the antibacterial and mildew-proof resin particles in the ink layer away from the outer film include, by weight, 60 parts of submicron glass, 15 parts of silver ion salt, 6 parts of zinc ion salt and 5 parts of copper ion salt;
[0051] S3, compounding the film body printed with two layers of ink in step S2 with the film body not printed with ink, so that an ink layer is formed between the two films;
[0052] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0053] The ink layer close to the outer film uses a lower content of silver ion salt and a higher content of zinc ion salt and copper ion salt. This ratio can ensure the antibacterial effect while absorbing more antibacterial and mildew-proof resin particles in the outer layer and the ink layer away from the outer film, so that more of them are kept in the film body, and the silver ion migration caused by external environmental changes or air oxygen is prevented. The ink layer away from the outer film uses a higher content of silver ion salt and a lower content of zinc ion salt and copper ion salt, so that it is in a more stable area, enhancing the antibacterial ability of the inner layer of ink and ensuring the overall antibacterial effect of the film. At the same time, brushing two layers of ink on a film can better protect the ink layer, reduce possible damage or defects during the composite process, and maintain the integrity and functionality of the ink layer.
[0054] Embodiment 4
[0055] Embodiment 3: By brushing two layers of different inks in the outer layer of ink, the antibacterial effect is ensured while the action time of silver ions is increased, thereby further improving the stability and durability of the packaging bag.
[0056] S2, printing colored ink and varnish ink on the surface of the outer film in sequence; and printing twice;
[0057] The ink contains 1-1.5% of the total weight of the ink antibacterial and mildew-proof resin particles; after adding the antibacterial and mildew-proof resin particles, the ink is stirred evenly at a speed of 400-500 rpm for 4-5 hours; the antibacterial and mildew-proof resin particles in the ink layer close to the outer film include, by weight, 60 parts of submicron glass, 10 parts of silver ion salt, 13 parts of zinc ion salt and 10 parts of copper ion salt; the antibacterial and mildew-proof resin particles in the ink layer away from the outer film include, by weight, 60 parts of submicron glass, 15 parts of silver ion salt, 6 parts of zinc ion salt and 5 parts of copper ion salt;
[0058] The diameter of the submicron glass in the inner layer is increased to 0.5-1.0 microns; and the inner layer film comprises, by weight: 100 parts of submicron glass, 10 parts by weight of silver ion salt, 13 parts by weight of zinc ion salt and 10 parts by weight of copper ion salt;
[0059] S3, compounding the outer film printed with two layers of ink in step S2 with the inner film body without ink printed and containing a larger glass diameter, so that an ink layer is formed between the two films;
[0060] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0061] Glass particles with larger diameters form a tighter bond with the ink layer during the compounding process, thereby improving the overall strength and durability of the film. The ink will enter the gaps formed by the glass in the inner film, thereby improving the antibacterial properties of the inner film and ensuring the sterility of the items packaged in the packaging bag. Glass particles with larger diameters can provide stronger support, increase the tensile strength and tear resistance of the film, and when the ink penetrates into the gaps between these glass particles, a more continuous and solid network structure will be formed, further improving the mechanical properties of the film. After the ink penetrates into the gaps between the glass in the inner film, the internal bonding force of the film can be increased, reducing the risk of peeling between layers, so that the composite film can better maintain its integrity and functionality when used for a long time or subjected to external pressure.
[0062] Comparative Example
[0063] The only difference from the first embodiment is that no stirring is performed when the antibacterial and mildew-proof resin particles are added in step S2.
[0064] The packaging bags prepared in the above examples and comparative examples were tested for uniformity, initial, 6-month, and 10-month antibacterial performance. The uniformity was the test of the uniformity of the antibacterial and mildew-proof resin particles in randomly selected films of the same area, and the standard deviation was used for calculation. The antibacterial performance test was the antibacterial rate test, and the test strain was Escherichia coli. The specific results are shown in Table 1.
[0065] Table 1 Test results of packaging bags obtained in various embodiments and comparative examples
[0066] Uniformity (%) Initial antibacterial rate (%) Antibacterial rate after 6 months (%) Initial antibacterial rate after 10 months (%) Embodiment 1 12.05 99.99 98.95 93.25 Embodiment 2 10.64 99.99 99.15 97.53 Embodiment 3 9.65 99.99 99.99 99.31 Embodiment 4 9.67 99.99 99.99 99.67 Comparative Example 86.12 76.58 75.15 56.21
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations, such as adding a base fabric outside the membrane to increase durability. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A preparation process for an antibacterial and mildew-proof hygienic packaging bag, It is characterized in that The specific steps include: S1, adding antibacterial and mildew-proof resin particles composed of 60 parts by weight of submicron glass, 15 parts by weight of silver ion salt, 13 parts by weight of zinc ion salt and 10 parts by weight of copper ion salt evenly into the film body, stirring evenly at a speed of 400-500 rpm, stirring for 4-5 hours, the added amount accounts for 1-1.5% of the total added amount of the film body, and blowing the film according to the above ratio; Among them, the diameter of submicron glass is 0.2-0.5 microns; The silver ion salt is a mixture of silver carbonate and silver bromide in a weight ratio of 2:1, and the diameter of the silver ion salt particles is 50-100 nanometers, the zinc ion salt is zinc oxide, and the copper ion salt is cuprous oxide, the weight ratio between the zinc ion salt and the copper ion salt is 2:1, and the diameters of the zinc ion salt and the copper ion salt particles are 3-10 nanometers; S2. Printing colored ink and varnish ink on the surface of the film in sequence to form two layers of ink, wherein the ink contains an antibacterial component, the antibacterial component is antibacterial and mildew-proof resin particles, and the addition amount is 1-1.5% of the total mass of the ink. After adding the antibacterial and mildew-proof resin particles, the ink is stirred evenly at a speed of 400-500 rpm for 4-5 hours; In the two layers of ink formed, the antibacterial and anti-mildew resin particles in the ink layer close to the film body include, by weight, 60 parts of submicron glass, 10 parts by weight of silver ion salt, 13 parts by weight of zinc ion salt and 10 parts by weight of copper ion salt; The antibacterial and mildew-proof resin particles in the ink layer away from the film body include, by weight, 60 parts of submicron glass, 15 parts of silver ion salt, 6 parts of zinc ion salt and 5 parts of copper ion salt; S3, compounding the film body printed with two layers of ink in step S2 with the film body not printed with ink, and forming an ink layer between the two films; The antibacterial and mildew-proof resin particles of the film body without ink printing include, by weight: 100 parts of submicron glass, 10 parts by weight of silver ion salt, 13 parts by weight of zinc ion salt and 10 parts by weight of copper ion salt, wherein the diameter of the submicron glass is 0.5-1.0 microns; S4, cutting into packaging bags with a film thickness of 23-110 microns.
2. A process for preparing an antibacterial and mildew-proof hygienic packaging bag as claimed in claim 1, It is characterized in that The film in step S1 is composed of 100 parts by weight of PE substrate and 1-1.5 parts by weight of antibacterial and antifungal resin particles. 3.An antibacterial and mildew-proof hygienic packaging bag, It is characterized in that The antibacterial and mildew-proof hygienic packaging bag is made by the preparation process of the antibacterial and mildew-proof hygienic packaging bag according to any one of claims 1-2.