A method for improving coal-rock-cement interface affinity

The coal rock-cement interface affinity agent prepared by modifying the inorganic mineral base material solves the problems of low bonding strength and poor sealing quality at the coal rock-cement interface, significantly improves the interface affinity, and enhances the strength of the coal rock-cement interface. The cementing effect improves the cementing quality of coalbed methane wells.

CN118242002BActive Publication Date: 2024-10-22NORTHEAST GASOLINEEUM UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410328609.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-21
Publication Date
2024-10-22
Estimated Expiration
2044-03-21

AI Technical Summary

Technical Problem

The interface bonding strength between coal rock and cement is low, the sealing quality is poor, and the poor hydrophilicity of the coal rock surface and the influence of residual drilling fluid in the fractures have not been effectively resolved, making it difficult to improve the coal rock-cement interface bonding problem.

Method used

The modified product of inorganic mineral base material is used to prepare the coal rock-cement interface affinity agent. By mixing the inorganic mineral base material with the modifier and heating, a C-H structure with amphiphilic Si-O, Ca-O and lipophilicity is prepared. The interface affinity agent is added to the drilling fluid to improve the hydrophilicity of the coal and rock surface, and is cemented with cement after static soaking downhole to enhance the interface bonding force.

Benefits of technology

It significantly improves the cementing strength of the coal rock-cement interface, enhances the interface affinity, solves the cementing problem of smooth surfaces and residual drilling fluid, achieves effective cementing of the coal rock-cement interface, and improves the cementing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118242002B_ABST
    Figure CN118242002B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for improving the affinity of coal-rock-cement interface, which includes: one, preparing a coal-rock-cement interface affinity agent, the coal-rock-cement interface affinity agent is composed of one or more mixed inorganic mineral base material modified products, any inorganic mineral base material modified product has an amphiphilic structure, including hydrophilic Si-O, Ca-O and lipophilic C-H; two, determining the amount of the coal-rock-cement interface affinity agent added to the on-site drilling fluid; three, drilling to 50-100m before the coal-rock layer, adding the coal-rock-cement interface affinity agent to the on-site drilling fluid through the feeding funnel according to the determined addition amount, after fully mixing in the mud pool, circulating with the drilling down to the end of the drilling, and after the subsequent flushing fluid flushes the wellbore, injecting cement slurry for cementing. The present invention solves the problems of low bonding strength and poor sealing quality of the coal-rock-cement interface, as well as the bonding problem of the smooth exposed coal-rock surface and the coal-rock surface with residual drilling fluid and cement slurry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to a technology for enhancing the cementing quality of a coalbed methane well, in particular to a method for improving the affinity of a coal rock-cement interface. Background technology:

[0002] Coalbed methane, also known as coalbed methane, is an unconventional resource. Compared with natural gas, coalbed methane has the characteristics of high calorific value and green and clean. It is a good alternative fuel to natural gas and has gradually become a hot spot for oil and gas resource exploitation.

[0003] Coalbed methane exists in the coal rock reservoir in the form of adsorption. Compared with conventional natural gas, its geological conditions are more complex. In addition, factors such as low porosity and permeability of coal seams, strong plasticity, and difficulty in extending artificial fractures make its reservoir transformation more difficult and development more difficult. In order to achieve good reservoir transformation and ensure that coal rock gas has good fracturing, drainage, gas production and a longer well life in the later stage, the cementing quality indicator is particularly important in the coal rock gas mining process. At present, most of the on-site construction processes improve the cementing quality of the coal rock section by improving the performance of cement slurry and changing the cementing construction process, ignoring the influence of the coal rock itself The characteristics of the coal rock itself are an important factor affecting the cementing quality of the coal rock section. The organic matter content in coal rock is more than 90%, and its surface is highly oleophilic, which makes it unable to effectively bond with hydrophilic cement slurry; the coal seam section wall is locally smooth, the cement hydration product has low adhesion, and the interface bonding force is poor; the coal rock has developed joints and foliations, is brittle, and is easy to form irregular wellbores, which are generally uneven, and are prone to retain a large amount of dead mud, with poor flushing efficiency, resulting in poor cement curing bonding effect at cracks and irregular wellbores, and reduced interface bonding quality. According to the above analysis, only changing the performance of cement slurry and changing the cementing construction process cannot effectively improve the coal rock-cement bonding problem.

[0004] In order to solve the problem that the coal rock surface has poor hydrophilicity and cannot be well bonded with cement slurry, there are literature reports that the hydrophilicity of the coal rock surface can be improved by using surfactants to prepare cleaning fluids to wet the well wall, thereby enhancing the bonding effect of the coal rock-cement interface. This method mainly covers a layer of amphiphilic surfactant on the coal rock surface, which is similar to the mechanism of "like dissolves like". The lipophilic group of the surfactant is adsorbed on the oil-wetted coal rock surface, while the hydrophilic group is exposed on the outside of the coal rock surface, so that the coal rock surface is transformed from lipophilic to hydrophilic, and the physical force between the coal rock and the cement slurry is enhanced, that is, the affinity is increased. This method has a certain interface enhancement effect in the early stage of cementing, but it only improves the affinity between the coal rock and cement by enhancing the physical force between the coal rock and cement. Therefore, the timeliness of this method needs further research and verification. In addition, this method ignores the influence of residual drilling fluid in fractures and irregular wellbores on interface bonding, and does not comprehensively solve the bonding problem of the coal rock-cement interface.

[0005] In view of the problems of low bonding strength and poor sealing quality of the coal-rock-cement interface caused by different surface wettability of coal rock and cement slurry and residual drilling fluid in coal rock cracks and irregular wellbores, the present invention provides a method for improving the affinity of the coal-rock-cement interface. Summary of the invention:

[0006] The purpose of the present invention is to provide a method for improving the affinity of the coal rock-cement interface. The method for improving the affinity of the coal rock-cement interface is used to solve the problems of low bonding strength and poor sealing quality of the coal rock-cement interface, as well as the bonding problem between the smooth exposed coal rock surface and the coal rock surface with residual drilling fluid and cement slurry.

[0007] The technical solution adopted by the present invention to solve the technical problem is: the method for improving the affinity of the coal rock-cement interface is:

[0008] Step 1: prepare a coal rock-cement interface affinity agent, which is composed of one or a mixture of inorganic mineral base material modified products. The preparation method of any inorganic mineral base material modified product is as follows:

[0009] The inorganic mineral base material is mixed with an appropriate amount of anhydrous ethanol, and then the mixture is poured into a three-necked flask, placed in a constant temperature water tank, heated to 50°C-100°C, and a modifier is added according to 1%-5% of the mass percentage of the inorganic mineral base material to react, and after reacting for 20-50 minutes, the inorganic mineral base material is purified and dried to obtain a modified product; the modified product of the inorganic mineral base material has an amphiphilic structure in terms of molecular structure, including hydrophilic Si-O, Ca-O and lipophilic CH;

[0010] Step 2: Determine the amount of coal rock-cement interface affinity agent added to the on-site drilling fluid:

[0011] A certain mass of drilling fluid is taken from the site and divided into multiple portions, and the coal rock-cement interface affinity agent is added to the corresponding drilling fluid in different addition amounts, and stirred evenly to obtain multiple portions of A mixed solution; a coal rock core is placed in each portion of A mixed solution, and the coal rock core is taken out after static immersion for a certain period of time at the well depth temperature. At this time, the surface of the coal rock core, including the cracks, is attached with drilling fluid, and the coal rock core attached with drilling fluid is vertically placed in the center of a cylindrical mold, and cement slurry is poured into the annular space to simulate the two-interface bonding of coal rock and cement in the well; it is cured at room temperature, and then placed at a constant temperature at the well depth temperature for curing. After the curing is completed, the maximum force of the coal rock core column pressed out of the cement ring is tested, and the maximum force pressed out is divided by the bonding area of ​​the coal rock core and the cement, that is, the coal rock-cement interface bonding strength is obtained, and compared with the blank sample, the addition amount corresponding to the maximum increase in the interface bonding strength is the appropriate addition amount of the coal rock-cement interface affinity agent in the on-site drilling fluid;

[0012] Step 3: Drill to 50-100m before the coal-rock layer, add the coal-rock-cement interface affinity agent into the on-site drilling fluid through the feeding funnel according to the amount determined in step 2, mix it fully in the mud pool, circulate it with the drill until the drilling is completed, and after flushing the wellbore with subsequent flushing fluid, inject cement slurry for cementing.

[0013] In the above scheme, the inorganic mineral base material is selected from silicon dioxide fine powder or wollastonite fine powder, and the particle sizes of silicon dioxide fine powder and wollastonite fine powder are both micro-nano level.

[0014] In the above scheme, the modifier is selected from silane coupling agents or stearic acids.

[0015] In the above scheme, the particle size of the silicon dioxide fine powder is ≥1250 mesh or the particle size of the wollastonite fine powder is ≥1250 mesh.

[0016] In the above scheme, the amount of coal rock-cement interface affinity agent added to the coalbed methane well drilling fluid is 0.5%-5%, preferably 1%-3%. After being fully stirred and mixed, it can be circulated downhole with the drilling fluid.

[0017] In the above scheme, the amount of coal rock-cement interface affinity agent added to the coalbed methane well drilling fluid is 1%-3%.

[0018] Beneficial effects:

[0019] 1. The method for improving the coal-rock-cement interface affinity provided by the present invention shows a good interface affinity enhancement effect at a temperature of 20-140°C, and can increase the bonding strength of the coal-rock-cement interface by 3-5 times, with a significant interface enhancement effect.

[0020] 2. The mechanism of enhancing the affinity of the coal rock-cement interface provided by the present invention is as follows: the inorganic mineral base material is a hydrophilic substance. After modification, part of the hydrophilic groups in its molecular structure are covered by lipophilic organic carbon chains, making it amphiphilic. When it is added to the drilling fluid, the lipophilic end is automatically adsorbed to the lipophilic coal rock surface, while the hydrophilic side is extended in the drilling fluid. The wettability modification of the lipophilic coal rock surface is achieved, and the hydrophilicity of the coal rock surface is improved. During the cementing process, the unmodified -Si-O- in the coal rock-cement interface affinity agent molecules is disconnected and activated under the action of -OH in the cement filtrate, generating hydrated silicates and gel-like substances with cementing effects. These substances are filled at the coal rock-cement interface and play a bonding role, thereby improving the strength and density of the solid phase particle accumulation zone at the coal rock fracture, making the mineral composition of the solid phase particle accumulation zone similar to the product after cement hydration, and enhancing the bonding force between the solid phase particle accumulation zone and cement stone. The method is based on simultaneously improving the affinity of the coal-rock and solid phase particle accumulation zone-cement interfaces to enhance the affinity of the coal-rock-cement interface.

[0021] 3. The method for improving the affinity of the coal rock-cement interface provided by the present invention is mainly based on the physical and chemical coupling effect at the interface, so as to achieve effective improvement of the interface affinity. The implementation is simple, and it can solve the problems of low bonding strength and poor sealing quality of the coal rock-cement interface. At the same time, it can solve the bonding problem between the smooth exposed coal rock surface and the coal rock surface with residual drilling fluid and cement slurry.

[0022] 4. The present invention provides a coal-rock-cement interface affinity agent, which is prepared by organically modifying an inorganic mineral base material with a modifier, and has an amphiphilic structure in its molecular structure, including hydrophilic Si-O, Ca-O and lipophilic CH. 0.5%-5% of the coal-rock-cement interface affinity agent provided by the present invention is added to the drilling fluid of a coalbed methane well, and the mixture is fully stirred and evenly mixed, and then circulated downhole with the drilling fluid. This method is based on the physical and chemical coupling effect at the interface, and can effectively improve the coal-rock-cement interface affinity. Description of the drawings:

[0023] Figure 1 This is a graph showing the effect of the amount of coal rock-cement interface affinity agent added on the interface bonding strength. Specific implementation method:

[0024] The present invention will be further described below in conjunction with the accompanying drawings:

[0025] The method for improving the affinity of coal rock-cement interface is:

[0026] Step 1: prepare a coal rock-cement interface affinity agent, which is composed of one or a mixture of inorganic mineral base material modified products. The preparation method of any inorganic mineral base material modified product is as follows:

[0027] The inorganic mineral base material is mixed with an appropriate amount of anhydrous ethanol, and then the mixture is poured into a three-necked flask, placed in a constant temperature water tank, heated to 50°C-100°C, and a modifier is added according to 1%-5% of the mass percentage of the inorganic mineral base material for reaction. After reacting for 20-50 minutes, the modified product of the inorganic mineral base material is purified and dried to obtain the modified product of the inorganic mineral base material; the modified product of the inorganic mineral base material has an amphiphilic structure in terms of molecular structure, including hydrophilic Si-O, Ca-O and lipophilic CH; during the preparation process, the reaction conditions are controlled, including the reaction temperature, material ratio and reaction time, so that the surface of the inorganic mineral base material is partially grafted with an organic carbon chain, and the product with the smallest difference between the water contact angle and 90° is preferably the coal rock-cement interface affinity agent provided by the present invention, and the agent has amphiphilicity.

[0028] Step 2: Determine the amount of coal rock-cement interface affinity agent added to the on-site drilling fluid:

[0029] Take a certain mass of on-site drilling fluid, add the amphiphilic coal rock-cement interface affinity agent provided by the present invention to the drilling fluid in different addition amounts (mass ratio), and stir evenly; then put the coal rock core column cut in advance into the above-mentioned drilling fluid and soak it statically at the well depth temperature for a certain period of time, take out the coal rock core, at this time, a certain amount of drilling fluid is attached to the surface of the coal rock core including the cracks, place the coal rock core attached with drilling fluid in the center of a cylindrical mold, and pour cement slurry in the annular space to simulate the two-interface bonding of coal rock and cement in the well. Curing for a certain time at room temperature, and then placed at a constant temperature for a certain time at the well depth temperature. After the curing is completed, the maximum force of the coal rock core column being pressed out of the cement ring is tested, and the coal rock-cement interface bonding strength can be obtained by dividing the force by the bonding area of ​​the coal rock core and cement. Compared with the blank sample, the addition amount corresponding to the maximum increase in the interface bonding strength is the appropriate addition amount of the amphiphilic coal rock-cement interface affinity agent of the present invention in the on-site drilling fluid;

[0030] Step 3: Drill to 50-100m before the coal-rock layer, add the coal-rock-cement interface affinity agent into the on-site drilling fluid through the feeding funnel according to the amount determined in step 2. After being fully mixed in the mud pool, circulate it down the well until the drilling is completed. After the wellbore is flushed with subsequent flushing fluid, cement slurry is injected for cementing.

[0031] Embodiment 1:

[0032] The coal rock-cement interface affinity agent was prepared according to the following method:

[0033] 1250 mesh wollastonite fine powder was used as the base material, and silane coupling agent KH-550 was selected as the modifier. 5g of wollastonite fine powder was mixed with 100mL of anhydrous ethanol, and then the mixture was poured into a three-necked flask, placed in a constant temperature water tank, heated to 60°C, and 4% KH-550 was added for reaction. After 40 minutes of reaction, centrifugal separation was performed, and the mixture was extracted by a vacuum pump and placed in an electric constant temperature blast drying oven for air drying to obtain a coal rock-cement interface affinity agent. The prepared interface affinity agent was measured for wetting angle using an SD-360A wetting angle measuring instrument to evaluate its surface wettability.

[0034] Table 1 Determination of wetting angle of coal rock-cement interface affinity agent of the present invention

[0035] sample Water wetting angle (°) Lipophilicity Increased Multiples 1250 mesh wollastonite 19 —— Coal rock-cement interface affinity agent 87 4.6

[0036] It can be seen from Table 1 that the water wetting angle of the prepared coal rock-cement interface affinity agent is significantly increased, indicating that compared with the base material, the wetting angle of the prepared coal rock-cement interface affinity agent is close to 90°, its hydrophilicity decreases, its lipophilicity increases, and finally it has amphiphilicity.

[0037] Embodiment 2:

[0038] The coal rock-cement interface affinity agent was prepared according to the following method:

[0039] 2500 mesh silica fine powder was used as the base material, and stearic acid was selected as the modifier. 5g of wollastonite fine powder was mixed with 100mL of anhydrous ethanol, and then the mixture was poured into a three-necked flask, placed in a constant temperature water tank, heated to 80°C, and 2% stearic acid was added for reaction. After the reaction for 30 minutes, centrifugal separation was performed, and the mixture was extracted by a vacuum pump and placed in an electric constant temperature blast drying oven for air drying to obtain a coal rock-cement interface affinity agent. The prepared interface affinity agent was measured for wetting angle using an SD-360A wetting angle measuring instrument to evaluate its surface wettability.

[0040] Table 2 Determination of wetting angle of coal rock-cement interface affinity agent of the present invention

[0041] sample Water wetting angle (°) Lipophilicity Increased Multiples 2500 mesh silica 19 —— Coal rock-cement interface affinity agent 91 4.8

[0042] It can be seen from Table 2 that the water wetting angle of the prepared coal rock-cement interface affinity agent is significantly increased, indicating that compared with the base material, the water wetting angle of the prepared coal rock-cement interface affinity agent is 92°, its hydrophilicity decreases, its lipophilicity increases, and finally it has amphiphilicity.

[0043] Embodiment 3:

[0044] The interface bonding indoor test was carried out according to the following method: ① The coal rock-cement interface affinity agents prepared in Examples 1 and 2 were mixed in a ratio of 1:1 and added to the drilling fluid (the main formula of the drilling fluid is: 3% bentonite + 0.4% polymer inhibitor + 0.75% salt-resistant fluid loss agent + 15% fluid loss agent + 0.75% polyol + 9% KCL + 12.5% ​​organic salt + 4% lubricant + 0.15% viscosity enhancer + 2.5% emulsified asphalt + 3% lime powder + 4% ultrafine calcium) in different amounts and stirred evenly. Then the φ25mm coal rock core column was soaked in the above drilling fluid for 30 minutes at a soaking temperature of 80°C. After being treated by the above method, the coal rock core column was taken out, and the soaked and modified coal rock core column was placed in a φ70mm*30mm cylindrical mold, and cement slurry was injected into the annular space between the core and the mold, and placed at room temperature for 24 hours. The mold was then placed at 80°C for 7 days to test the coal-rock-cement interface bonding strength. Figure 1 .

[0045] Depend on Figure 1 It can be seen that when the amount of coal rock-cement interface affinity agent added in the drilling fluid is 1.0%, the interface bonding strength is the largest, which is 4.56 times that of the blank sample. It is determined that the appropriate amount of coal rock-cement interface affinity agent added in the drilling fluid is 1.0%.

[0046] Comparative Example 3:

[0047] The interface bonding indoor test was carried out according to the following method: First, the coal rock was treated by the following method: the φ25mm coal rock core column was soaked in the surfactant CM-S solution with a concentration of 0.3% proposed in the literature for 0.5min, and the soaking temperature was 80℃, so as to modify the surface of the coal rock. The coal rock core column was taken out, and the soaked and modified coal rock core column was placed in a φ70mm*30mm cylindrical mold, and cement slurry was injected into the annular space between the core and the mold, and placed at room temperature for 24h. Then the mold was placed at 80℃ for 7 days, and the coal rock-cement interface bonding strength was measured and compared with the interface enhancement effect of the coal rock-cement interface affinity agent in Example 3. The results are shown in Table 3.

[0048] Table 3 Comparison of effects of different interface enhancement methods

[0049]

[0050] It can be seen from Table 3 that compared with the method of wetting and modifying coal rock with a surfactant, the method for improving the coal rock-cement interface affinity provided by the present invention can improve the coal rock-cement interface bonding strength more significantly. The latter's enhancement effect is 3.5 times that of the former, which is feasible and has a good interface enhancement effect.

[0051] Embodiment 5:

[0052] The compatibility evaluation of the amphiphilic coal rock-cement interface affinity agent provided by the present invention with on-site drilling fluid and on-site cement slurry. The amphiphilic coal rock-cement interface affinity agent is added to the drilling fluid in an appropriate amount determined in (1), and after being fully mixed, the density, water loss and rheological parameters of the drilling fluid are measured to evaluate the compatibility of the amphiphilic coal rock-cement interface affinity agent with the on-site drilling fluid; the amphiphilic coal rock-cement interface affinity agent is added to the cement slurry in an appropriate amount determined in (1), and after being fully mixed, the thickening time and the compressive strength of the cement paste are measured to evaluate the compatibility of the amphiphilic coal rock-cement interface affinity agent with the on-site cement slurry system.

[0053] Specifically, the basic performance test of drilling fluid and cement slurry was carried out according to the following method to evaluate the compatibility of the coal rock-cement interface affinity agent of the present invention with the drilling fluid and cement slurry: the coal rock-cement interface affinity agent in Example 3 of the present invention was added in an amount of 1.0% and fully mixed with the drilling fluid and cement slurry respectively, and the performance tests of the drilling fluid and cement slurry were carried out according to the drilling fluid laboratory test GB / T 29170-2012 and the oil well cement test method GB / T 19139-2003, including the density, filtration loss, rheological properties and the thickening time and compressive strength test results of the cement slurry are shown in Tables 4, 5 and 6.

[0054] Table 4 Effect of the coal rock-cement interface affinity agent of the present invention on the main properties of drilling fluid

[0055]

[0056] Table 5 Effect of the coal rock-cement interface affinity agent of the present invention on the thickening time of cement slurry

[0057]

[0058] Table 6 Effect of the coal rock-cement interface affinity agent of the present invention on the 24h compressive strength of cement slurry

[0059]

[0060] It can be seen from Table 4 that the coal rock-cement interface affinity agent provided by the present invention has no significant effect on the basic physical parameters of the drilling fluid and has good compatibility with the drilling fluid.

[0061] As can be seen from Table 5 and Table 6, the coal rock-cement interface affinity agent provided by the present invention has a relatively large effect on the thickening time and compressive strength of the first slurry, but it only reduces 3% and 4.5%, and has little effect on the tail propeller and the intermediate slurry. In the coalbed methane cementing process, the coal rock-cement interface affinity agent provided by the present invention is mainly in contact with the coal seam section, the intermediate slurry and the tail slurry section, so it can be determined that the coal rock-cement interface affinity agent provided by the present invention does not affect the thickening time and compressive strength of the cement slurry after being added to the cement slurry, and has good compatibility with the cement slurry.

[0062] Embodiment 6:

[0063] The coalbed methane well field test was carried out and the cementing quality was determined according to the following method: when drilling to 70 meters before the coal rock layer, the coal rock-cement interface affinity agent in Example 3 of the present invention was added to the mud pool at an amount of 1.0% through the feeding funnel, and the agitator was fully stirred and mixed and then circulated while drilling. The drilling fluid performance was continuously monitored during the drilling process. If fluctuations occurred, timely adjustments were made. After the drilling was completed, the flushing fluid was flushed into the wellbore for 8 minutes, and then cementing was performed by injecting cement slurry. After seven days, acoustic logging was performed to evaluate the cementing quality, and the cementing quality was compared with that of the adjacent well that did not adopt the coal rock-cement interface enhancement method proposed by the present invention, as shown in Table 7.

[0064] Table 7 Cementing quality measurement results

[0065] Test well Pass rate Coalbed methane wells that do not use the interface enhancement method proposed by the present invention 87% Coalbed methane well using the interface enhancement method proposed by the present invention 100%

[0066] The present invention improves the strength and density of the solid-phase particle accumulation zone at the coal-rock fracture, makes the mineral composition of the solid-phase particle accumulation zone similar to the product of cement hydration, and enhances the bonding force between the solid-phase particle accumulation zone and cement stone. The method is based on simultaneously improving the affinity of the coal-rock and solid-phase particle accumulation zone-cement interfaces to enhance the affinity of the coal-rock-cement interface.

Claims

1. A method for improving coal rock-cement interface affinity, characterized in that The steps include: Step 1: prepare a coal rock-cement interface affinity agent, which is composed of one or a mixture of inorganic mineral base material modified products. The preparation method of any inorganic mineral base material modified product is as follows: The inorganic mineral base material is mixed with an appropriate amount of anhydrous ethanol, and then the mixture is poured into a three-necked flask, placed in a constant temperature water tank, heated to 50°C-100°C, and a modifier is added according to 1%-5% of the mass percentage of the inorganic mineral base material to react, and after reacting for 20-50 minutes, the inorganic mineral base material is purified and dried to obtain an inorganic mineral base material modified product, wherein the inorganic mineral base material is selected from wollastonite fine powder; the inorganic mineral base material modified product has an amphiphilic structure in terms of molecular structure, including hydrophilic Si-O, Ca-O and lipophilic CH; Step 2: Determine the amount of coal rock-cement interface affinity agent added to the on-site drilling fluid: A certain mass of drilling fluid is taken from the site and divided into multiple portions, and the coal rock-cement interface affinity agent is added to the corresponding drilling fluid in different addition amounts, and stirred evenly to obtain multiple portions of A mixed solution; a coal rock core is placed in each portion of A mixed solution, and the coal rock core is taken out after static immersion for a certain period of time at the well depth temperature. At this time, the surface of the coal rock core, including the cracks, is attached with drilling fluid, and the coal rock core attached with drilling fluid is vertically placed in the center of a cylindrical mold, and cement slurry is poured into the annular space to simulate the two-interface bonding of coal rock and cement in the well; it is cured at room temperature, and then placed at a constant temperature at the well depth temperature for curing. After the curing is completed, the maximum force of the coal rock core column pressed out of the cement ring is tested, and the maximum force pressed out is divided by the bonding area of ​​the coal rock core and the cement, that is, the coal rock-cement interface bonding strength is obtained, and compared with the blank sample, the addition amount corresponding to the maximum increase in the interface bonding strength is the appropriate addition amount of the coal rock-cement interface affinity agent in the on-site drilling fluid; Step 3: Drill to 50-100m before the coal rock layer, add the coal rock-cement interface affinity agent to the on-site drilling fluid through the feeding funnel according to the addition amount determined in step 2, and after being fully mixed in the mud pool, circulate it down the well until the end of drilling. When it is added to the drilling fluid, the oleophilic end is automatically adsorbed to the oleophilic coal rock surface, while the hydrophilic side extends in the drilling fluid, thereby realizing the wetting modification of the oleophilic coal rock surface and improving the hydrophilicity of the coal rock surface; after the subsequent flushing fluid flushes the wellbore, cement slurry is injected for cementing. During the cementing process, the unmodified -Si-O- in the coal rock-cement interface affinity agent molecules is disconnected and activated under the action of -OH in the cement filtrate to generate hydrated silicates and gel-like substances with cementing effect. These hydrated silicates and gel-like substances are filled at the coal rock-cement interface to play a bonding role, thereby improving the strength and density of the solid phase particle accumulation zone at the coal rock fracture, and enhancing the bonding force between the solid phase particle accumulation zone and the cement stone.

2. The method for improving coal rock-cement interface affinity according to claim 1, characterized in that: The particle size of the wollastonite fine powder is micro-nano level.

3. The method for improving coal rock-cement interface affinity according to claim 2, characterized in that: The modifier is selected from silane coupling agents or stearic acids.

4. The method for improving coal rock-cement interface affinity according to claim 3, characterized in that: The particle size of the wollastonite fine powder is ≥1250 mesh.