Thermoplastic polyolefin elastomer plastic steel tile and preparation method thereof

By using internally enhanced waterproof coils in thermoplastic polyolefin elastomer plastic steel tiles and adjusting the ratio of polyolefin resin to grafted modified polyolefin resin, the thermoplastic polyolefin elastomer layer is solved by the use of internal reinforced waterproof coils in thermoplastic polyolefin elastomer tiles and adjusting the ratio of polyolefin resin to graft modified polyolefin resins, the thermoplastic polyolefin elastomer layer is crimped during the hot press bonding process. The problem of burning may improve the adhesion and stability of the waterproof coil material and metal plate, and extend the service life.

CN118269440BActive Publication Date: 2024-11-08KESHUN WATERPROOF TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410459086.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2024-11-08
Estimated Expiration
2044-04-16

AI Technical Summary

Technical Problem

When the thermoplastic polyolefin elastomer waterproof coil is hot pressed and bonded with the metal plate, the thermoplastic polyolefin elastomer layer is prone to cause the problem of being crimped or broken, and the bonding effect is poor, which affects the service life.

Method used

Using an inner reinforced waterproof coil material, including a first thermoplastic polyolefin elastomer layer, an inner reinforced layer and a second thermoplastic polyolefin elastomer layer arranged in the first direction, the composition of the second thermoplastic polyolefin elastomer layer is adjusted. and proportion, increase the ratio of polyolefin resin and graft modified polyolefin resin, and set up a glass fiber mesh cloth or polyester fiber mesh cloth in the waterproof roll to form a mutual embedded structure, improve adhesion and Dimensional stability.

Benefits of technology

It reduces the situation where the thermoplastic polyolefin elastomer layer is crimped or damaged during the hot press bonding process, improves the adhesion and dimensional stability between the waterproof coil and the metal plate, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118269440B_ABST
    Figure CN118269440B_ABST
Patent Text Reader

Abstract

The present application discloses a thermoplastic polyolefin elastomer plastic steel tile and a preparation method thereof. The thermoplastic polyolefin elastomer plastic steel tile comprises an internally reinforced waterproof coiled material, a metal plate and an optional anti-corrosion bottom film stacked along a first direction; the internally reinforced waterproof coiled material comprises a first thermoplastic polyolefin elastomer layer, an internally reinforced layer and a second thermoplastic polyolefin elastomer layer stacked along a first direction, and the second thermoplastic polyolefin elastomer layer is located on the side close to the metal plate; the anti-corrosion bottom film is arranged on the side of the metal plate away from the second thermoplastic polyolefin elastomer layer; based on the total mass of the second thermoplastic polyolefin elastomer layer as 100 parts, the second thermoplastic polyolefin elastomer layer comprises 50-70 parts of polyolefin resin, 20-40 parts of grafted modified polyolefin resin, and 3-11 parts of additives. The plastic steel tile of the present application and its preparation method can reduce the situation where the thermoplastic polyolefin elastomer layer is wrinkled or damaged during the hot pressing bonding process, and improve the adhesion between the waterproof coiled material and the metal plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of waterproof materials, and in particular to a thermoplastic polyolefin elastomer plastic steel tile and a preparation method thereof. Background Art

[0002] Metal roofs are widely used in civil and industrial buildings. Due to the design methods, construction methods and materials used, after a certain number of years of use, metal roofs will continue to rust due to various factors such as temperature changes, corrosion and oxidation, and aging of the surface coating film, eventually causing the metal roof to leak and shorten its service life.

[0003] The service life of exposed thermoplastic polyolefin (TPO) waterproofing membrane is up to 30 years. Compounding it with the metal plate of the metal roof can effectively prevent the metal roof from corrosion and leakage. At present, the main ways to compound thermoplastic polyolefin waterproofing membrane with metal plate are: fixing the thermoplastic polyolefin waterproofing membrane on the metal plate by mechanical fixing; bonding the thermoplastic polyolefin waterproofing membrane to the metal plate by hot pressing; applying adhesive on the metal plate to bond the thermoplastic polyolefin waterproofing membrane; or using butyl self-adhesive thermoplastic polyolefin waterproofing membrane to bond it to the metal plate.

[0004] When the thermoplastic polyolefin elastomer waterproof membrane is hot-pressed and bonded to the metal plate, there is a risk of the thermoplastic polyolefin elastomer layer being wrinkled or damaged due to the thin thermoplastic polyolefin elastomer layer and the high hot-pressing bonding temperature. There is also the problem of poor bonding between the thermoplastic polyolefin elastomer waterproof membrane and the metal plate. Summary of the invention

[0005] The present application provides a thermoplastic polyolefin elastomer plastic steel tile and a preparation method thereof, which can reduce the situation where the thermoplastic polyolefin elastomer layer is wrinkled or damaged during the hot pressing bonding process and improve the adhesion between the waterproof coiled material and the metal plate.

[0006] In the first aspect, an embodiment of the present application proposes a thermoplastic polyolefin elastomer plastic steel tile, which includes an internally reinforced waterproof membrane, a metal plate and an optional anti-corrosion base membrane stacked along a first direction; the internally reinforced waterproof membrane includes a first thermoplastic polyolefin elastomer layer, an internal reinforcement layer and a second thermoplastic polyolefin elastomer layer stacked along the first direction, and the second thermoplastic polyolefin elastomer layer is located on the side close to the metal plate; the anti-corrosion base membrane is arranged on the side of the metal plate away from the second thermoplastic polyolefin elastomer layer; based on the total mass parts of the second thermoplastic polyolefin elastomer layer as 100 parts, the second thermoplastic polyolefin elastomer layer includes the following components: polyolefin resin: 50-70 parts, grafted modified polyolefin resin: 20-40 parts, additives: 3-11 parts.

[0007] According to one aspect of an embodiment of the present application, in the second thermoplastic polyolefin elastomer layer, the mass ratio of the polyolefin resin to the graft-modified polyolefin resin is (1.35-2.92):1.

[0008] According to one aspect of the embodiment of the present application, the grafting rate of the graft-modified polyolefin resin is 0.6%-5%.

[0009] According to one aspect of the embodiment of the present application, the melting point of the second thermoplastic polyolefin elastomer layer is 150-170°C.

[0010] According to one aspect of the embodiment of the present application, based on 100 parts by total mass of the first thermoplastic polyolefin elastomer layer, the first thermoplastic polyolefin elastomer layer includes the following components: polyolefin resin: 74-90 parts, additives: 10-26 parts.

[0011] According to one aspect of an embodiment of the present application, the additive includes one or more of an antioxidant material, a flame retardant material, and a pigment.

[0012] According to one aspect of the embodiment of the present application, the grafting monomer of the graft-modified polyolefin resin includes one or more of maleic anhydride, acrylic acid, glycidyl methacrylate and styrene.

[0013] According to one aspect of the embodiment of the present application, the grafting monomer of the graft-modified polyolefin resin includes maleic anhydride and / or acrylic acid.

[0014] According to one aspect of the embodiment of the present application, the main resin of the graft-modified polyolefin resin includes one or more of polyethylene, polypropylene, polybutadiene and ethylene-octene copolymer.

[0015] According to one aspect of the embodiment of the present application, the main resin of the graft-modified polyolefin resin includes one or more of polyethylene, polypropylene and ethylene-octene copolymer.

[0016] According to one aspect of the embodiment of the present application, the inner reinforcement layer includes one or more of glass fiber mesh cloth and polyester fiber mesh cloth.

[0017] According to one aspect of the embodiment of the present application, the mesh number of the glass fiber mesh cloth is 1-5 meshes, and the mesh number of the polyester fiber mesh cloth is 1-5 meshes.

[0018] According to one aspect of an embodiment of the present application, the metal plate includes one or more of a galvanized steel plate, an aluminum-zinc-coated steel plate, an aluminum plate, an aluminum-manganese plate, a copper plate, an iron plate and a tin plate.

[0019] According to one aspect of an embodiment of the present application, the anti-corrosion base film includes one or more of a modified polyvinyl chloride film and a modified polyolefin film.

[0020] According to one aspect of the embodiment of the present application, the thickness of the first thermoplastic polyolefin elastomer layer is greater than the thickness of the second thermoplastic polyolefin elastomer layer.

[0021] According to one aspect of the embodiment of the present application, the thickness of the first thermoplastic polyolefin elastomer layer is 0.7-0.9 mm.

[0022] According to one aspect of the embodiment of the present application, the thickness of the second thermoplastic polyolefin elastomer layer is 0.6-0.7 mm.

[0023] In a second aspect, the present application embodiment provides a method for preparing the thermoplastic polyolefin elastomer plastic steel tile of the first aspect of the present application, comprising the following steps:

[0024] Compounding the first thermoplastic polyolefin elastomer layer, the inner reinforcement layer, and the second thermoplastic polyolefin elastomer layer to obtain an inner reinforcement waterproof membrane;

[0025] The internally reinforced waterproof membrane and the metal plate are hot-pressed and bonded under the first condition to obtain a composite body;

[0026] The optional anti-corrosion base film and the composite body are hot-pressed and bonded under the second condition to obtain a thermoplastic polyolefin elastomer plastic steel tile.

[0027] According to another aspect of the embodiment of the present application, the temperature of the first condition is 180-220° C., the pressure of the first condition is 0.3-0.6 MPa, and the time of the first condition is 10-60 s.

[0028] According to another aspect of the embodiment of the present application, the temperature of the second condition is 130-200° C., the pressure of the second condition is 0.3-0.6 MPa, and the time of the second condition is 10-30 s.

[0029] The embodiment of the present application provides an inner reinforcement layer in the waterproof membrane, and adjusts the composition and ratio of the second thermoplastic polyolefin elastomer layer so that the second thermoplastic polyolefin elastomer layer includes a certain ratio of polyolefin resin and grafted modified polyolefin resin, thereby reducing the possibility of the thermoplastic polyolefin elastomer layer being wrinkled or damaged during the hot pressing bonding process, improving the dimensional stability of the waterproof membrane, and improving the adhesion between the waterproof membrane and the metal plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The features, advantages and technical effects of exemplary embodiments of the present application will be described below with reference to the accompanying drawings.

[0031] Figure 1 This is a schematic diagram of the structure of the thermoplastic polyolefin elastomer plastic steel tile provided in an embodiment of the present application.

[0032] in:

[0033] 10. Internally reinforced waterproof membrane; 11. First thermoplastic polyolefin elastomer layer; 12. Internal reinforcement layer; 13. Second thermoplastic polyolefin elastomer layer; 21. Metal plate; 31. Anticorrosive base membrane. DETAILED DESCRIPTION

[0034] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In the detailed description below, many specific details are proposed to provide a comprehensive understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating examples of the present application. In the accompanying drawings and the following description, at least some of the known structures and technologies are not shown to avoid unnecessary ambiguity in the present application; and, for clarity, the size of some structures may be exaggerated. In addition, the features, structures or characteristics described below may be combined in one or more embodiments in any suitable manner.

[0035] It should be noted that, in this application, the terms "first", "second", etc. are used to distinguish similar objects, and are not used to describe a specific order or sequence. Moreover, the term "comprising" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprising..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0036] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured by various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application). Unless otherwise specified, the test temperature of the parameters mentioned in this application is 25° C. and the test pressure is standard atmospheric pressure.

[0037] A list of items connected by the term "one or more of" may mean any combination of the listed items. The term "plurality" means more than two.

[0038] The endpoints and any values ​​of the ranges disclosed in this application are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this application.

[0039] In the related art, a thermoplastic polyolefin elastomer waterproof membrane is fixed on a metal plate by mechanical fixing. The mechanical fixing method usually adopts a perforation method or a non-perforation fixing method. Since a full adhesion effect cannot be achieved, the thermoplastic polyolefin elastomer waterproof membrane is prone to hollowing and water leakage.

[0040] The thermoplastic polyolefin elastomer waterproof membrane is bonded to the metal plate by brushing adhesive. The thermoplastic polyolefin elastomer waterproof membrane needs to be rolled flat and the air can be exhausted after the adhesive is dried. Therefore, this process is time-consuming and not conducive to rapid construction. If the air is not exhausted, hollowing may occur.

[0041] The glue used in butyl self-adhesive thermoplastic polyolefin elastomer waterproof membrane is butyl glue, but the initial viscosity of butyl glue is low, which brings certain difficulties to the construction.

[0042] Hot-press bonding of thermoplastic polyolefin elastomer waterproofing membrane to metal plate is also a common composite method. In conventional composite methods, there may be a hot-melt adhesive film layer between the thermoplastic polyolefin elastomer waterproofing membrane and the metal plate, and when the thermoplastic polyolefin elastomer waterproofing membrane and the metal plate are hot-pressed, there is a risk of the thermoplastic polyolefin elastomer layer being wrinkled or damaged, and the bonding effect between the thermoplastic polyolefin elastomer waterproofing membrane and the metal plate is poor.

[0043] Figure 1 This is a schematic diagram of the structure of the thermoplastic polyolefin elastomer plastic steel tile provided in an embodiment of the present application. Figure 1 The y direction is the first direction, and the x direction is the second direction.

[0044] like Figure 1 As shown, in the first aspect, the embodiment of the present application proposes a thermoplastic polyolefin elastomer steel tile, the thermoplastic polyolefin elastomer steel tile comprises an internally reinforced waterproof coiled material 10, a metal plate 21 and an optional anti-corrosion bottom membrane 31 stacked along a first direction;

[0045] The internally reinforced waterproof membrane 10 comprises a first thermoplastic polyolefin elastomer layer 11, an internal reinforcement layer 12 and a second thermoplastic polyolefin elastomer layer 13 stacked along a first direction, wherein the second thermoplastic polyolefin elastomer layer 13 is located on a side close to the metal plate;

[0046] The anti-corrosion base film 31 is disposed on a side of the metal plate 21 away from the second thermoplastic polyolefin elastomer layer 13;

[0047] Based on 100 parts by weight of the second thermoplastic polyolefin elastomer layer, the second thermoplastic polyolefin elastomer layer includes the following components: 50-70 parts of polyolefin resin, 20-40 parts of graft-modified polyolefin resin, and 3-11 parts of additives.

[0048] The embodiment of the present application provides an inner reinforcement layer in the waterproof membrane, and adjusts the composition and ratio of the second thermoplastic polyolefin elastomer layer so that the second thermoplastic polyolefin elastomer layer includes a certain ratio of polyolefin resin and grafted modified polyolefin resin, thereby reducing the possibility of the thermoplastic polyolefin elastomer layer being wrinkled or damaged during the hot pressing bonding process, improving the dimensional stability of the waterproof membrane, and improving the adhesion between the waterproof membrane and the metal plate.

[0049] The first thermoplastic polyolefin elastomer layer may be referred to as a first TPO layer, and the second thermoplastic polyolefin elastomer layer may be referred to as a second TPO layer.

[0050] By providing an inner reinforcement layer, the embodiment of the present application can form an interlocking structure among the first thermoplastic polyolefin elastomer layer 11, the inner reinforcement layer 12 and the second thermoplastic polyolefin elastomer layer 13, thereby improving the stability of the waterproof membrane structure, making the waterproof membrane less likely to deform under extreme environments, and making the waterproof membrane less likely to peel off from the metal plate in an environment of alternating high and low temperatures.

[0051] Polyolefin resin is a non-polar material. By grafting and modifying the polyolefin resin, polar groups or functional side chains can be introduced into the polyolefin molecular chain, so that the second thermoplastic polyolefin elastomer layer can have good adhesion during hot pressing bonding.

[0052] Continue to refer Figure 1 In the embodiment of the present application, the first thermoplastic polyolefin elastomer layer 11, the inner reinforcement layer 12 and the second thermoplastic polyolefin elastomer layer 13 are all extended along the second direction.

[0053] In some optional embodiments, in the second thermoplastic polyolefin elastomer layer, the mass ratio of the polyolefin resin to the graft-modified polyolefin resin may be (1.35-2.92):1, and may be (1.5-2.14):1.

[0054] The embodiment of the present application can further improve the adhesion of the second thermoplastic polyolefin elastomer layer and improve the compatibility of the second thermoplastic polyolefin elastomer layer and the first thermoplastic polyolefin elastomer layer by setting the mass ratio of the polyolefin resin to the grafted modified polyolefin resin in the second thermoplastic polyolefin elastomer layer within the above range.

[0055] In some optional embodiments, the melting point of the second thermoplastic polyolefin elastomer layer may be 150-170°C.

[0056] The embodiment of the present application can improve the adhesion between the second thermoplastic polyolefin elastomer layer and the inner reinforcement layer and the first thermoplastic polyolefin elastomer layer by controlling the melting point of the second thermoplastic polyolefin elastomer layer within the above range, and can further improve the adhesion between the second thermoplastic polyolefin elastomer layer and the metal plate.

[0057] The melting point test method of the second thermoplastic polyolefin elastomer layer in the embodiment of the present application can be tested by differential scanning calorimetry. Exemplarily, the test conditions include: weighing about 5 mg of the sample, testing in a nitrogen atmosphere, heating at a rate of 10°C / min, heating from 25°C to 200°C, keeping the temperature for 5 minutes, eliminating the thermal history, cooling to 30°C, and finally heating to 200°C.

[0058] In some optional embodiments, the grafting rate of the graft-modified polyolefin resin may be 0.6%-5%.

[0059] In the embodiment of the present application, the grafting rate of the graft-modified polyolefin resin is controlled within the above range, so that the polyolefin resin and the graft-modified polyolefin resin have a better matching effect, and the adhesion between the second thermoplastic polyolefin elastomer layer and the metal plate is further improved.

[0060] In some optional embodiments, based on 100 parts by weight of the first thermoplastic polyolefin elastomer layer, the first thermoplastic polyolefin elastomer layer may include the following components: 74-90 parts by weight of polyolefin resin, and 10-26 parts by weight of additives.

[0061] In some optional embodiments, the polyolefin resin may include one or more of polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-octene copolymer and polybutadiene. For example, the polyolefin resin may include one or more of CA10A of Anderbasel Industries of the Netherlands, CA60A of Anderbasel Industries of the Netherlands, NS06 of Sinopec, 3020 of ExxonMobil Corporation of the United States, 6102 of ExxonMobil Corporation of the United States and 3000 of ExxonMobil Corporation of the United States.

[0062] In some optional embodiments, the additive may include one or more of an antioxidant material, a flame retardant material, and a pigment.

[0063] In some optional embodiments, the additives of the first thermoplastic polyolefin elastomer layer may include antioxidant materials, flame retardant materials, and pigments.

[0064] In some optional embodiments, based on the total mass parts of the first thermoplastic polyolefin elastomer layer being 100 parts, the additives of the first thermoplastic polyolefin elastomer layer may include: antioxidant material: 2-6 parts, flame retardant material 5-15 parts, pigment 1-5 parts. The antioxidant material, flame retardant material and pigment in the embodiments of the present application may be materials commonly used in the art. For example, the antioxidant material may be an antioxidant masterbatch, the flame retardant material may be a flame retardant masterbatch, and the pigment may be a color masterbatch. Those skilled in the art may select according to actual needs.

[0065] In some optional embodiments, the additives of the second thermoplastic polyolefin elastomer layer may include antioxidant materials and pigments.

[0066] In some optional embodiments, based on 100 parts by weight of the second thermoplastic polyolefin elastomer layer, the additives of the second thermoplastic polyolefin elastomer layer may include: 2-6 parts by weight of antioxidant material, and 1-5 parts by weight of pigment.

[0067] In some optional embodiments, the anti-oxidation material may include an antioxidant 1010 and an antioxidant 2020 .

[0068] In some optional embodiments, the flame retardant material may include one or more of a phosphorus-based flame retardant, a nitrogen-based flame retardant, an inorganic flame retardant, and a halogen-based flame retardant. For example, the inorganic flame retardant may be a magnesium hydroxide flame retardant.

[0069] The antioxidant masterbatch in the embodiment of the present application can be obtained by mixing, extruding and granulating an antioxidant and a polyolefin resin, wherein the total weight of the antioxidant masterbatch is 100 parts, and the antioxidant masterbatch can include: 70-80 parts of antioxidant and 20-30 parts of polyolefin resin. The flame retardant masterbatch can be obtained by mixing, extruding and granulating a flame retardant and a polyolefin resin, wherein the total weight of the flame retardant masterbatch is 100 parts, and the flame retardant masterbatch can include: 75-85 parts of flame retardant and 15-25 parts of polyolefin resin. The masterbatch can be obtained by mixing, extruding and granulating titanium dioxide or carbon black, polyolefin resin, lubricant, filler, etc. wherein the total weight of the masterbatch is 100 parts, and the masterbatch can include: 15-20 parts of titanium dioxide or 15-20 parts of carbon black, 75-85 parts of polyolefin resin, and 1-5 parts of lubricant and filler.

[0070] In some optional embodiments, the graft monomer of the graft-modified polyolefin resin may include one or more of maleic anhydride, acrylic acid, glycidyl methacrylate and styrene.

[0071] In some optional embodiments, the grafting monomer of the graft-modified polyolefin resin may include maleic anhydride and / or acrylic acid.

[0072] In some optional embodiments, the main resin of the graft-modified polyolefin resin may include one or more of polyethylene, polypropylene, polybutadiene and ethylene-octene copolymer.

[0073] In some optional embodiments, the main resin of the graft-modified polyolefin resin may include one or more of polyethylene, polypropylene and ethylene-octene copolymer.

[0074] In some optional embodiments, the grafted modified polyolefin resin may include one or more of maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified polybutadiene, maleic anhydride grafted modified ethylene-octene copolymer, acrylic acid grafted modified polyethylene, acrylic acid grafted modified polypropylene, methacrylate glycidyl grafted modified polyethylene, methacrylate glycidyl grafted modified polypropylene, styrene grafted modified polyethylene and styrene grafted modified polypropylene.

[0075] In some optional embodiments, the graft-modified polyolefin resin may include one or more of maleic anhydride graft-modified polyethylene, maleic anhydride graft-modified polypropylene, maleic anhydride graft-modified polybutadiene, maleic anhydride graft-modified ethylene-octene copolymer, acrylic acid graft-modified polyethylene and acrylic acid graft-modified polypropylene.

[0076] In the embodiment of the present application, by selecting the graft-modified polyolefin resin within the above range, the adhesion of the second thermoplastic polyolefin elastomer layer can be further improved.

[0077] In some optional embodiments, the inner reinforcement layer may have a grid structure.

[0078] In some optional embodiments, the inner reinforcement layer may include one or more of glass fiber mesh and polyester fiber mesh.

[0079] In some optional embodiments, the mesh number of the glass fiber mesh cloth may be 1-5 meshes, and the mesh number of the polyester fiber mesh cloth may be 1-5 meshes.

[0080] The embodiment of the present application can improve the adhesion between the inner reinforcement layer and the first thermoplastic polyolefin elastomer layer and the second thermoplastic polyolefin elastomer layer by controlling the mesh size of the inner reinforcement layer material within the above range, thereby further improving the adhesion between the inner reinforced waterproof membrane and the metal plate.

[0081] Exemplarily, the mesh size of the glass fiber mesh cloth is 9 mm×9 mm, and the mesh size of the polyester fiber mesh cloth is 9 mm×9 mm.

[0082] In some optional embodiments, the metal plate may include one or more of a galvanized steel plate, an aluminum-zinc-coated steel plate, an aluminum plate, an aluminum-manganese plate, a copper plate, an iron plate, a tin plate, a steel plate, and a stainless steel plate.

[0083] In some optional embodiments, the anti-corrosion base film may include one or more of a modified polyvinyl chloride film and a modified polyolefin film.

[0084] In the embodiment of the present application, by disposing an anti-corrosion base film made of the above material on the side of the metal plate away from the second thermoplastic polyolefin elastomer layer, the corrosion resistance of the metal plate can be further improved.

[0085] In the embodiments of the present application, there is no limitation on the specific modification method of the modified polyvinyl chloride film and the modified polyolefin film, and the modification method may be a conventional modification method in the art.

[0086] In some optional embodiments, the thickness of the first thermoplastic polyolefin elastomer layer may be greater than the thickness of the second thermoplastic polyolefin elastomer layer.

[0087] The embodiment of the present application can improve the deformation resistance of the first thermoplastic polyolefin elastomer layer by setting the thickness of the first thermoplastic polyolefin elastomer layer to be greater than the thickness of the second thermoplastic polyolefin elastomer layer, thereby further reducing the possibility of the first thermoplastic polyolefin elastomer layer being wrinkled or damaged during the hot pressing bonding process.

[0088] In some optional embodiments, the thickness of the first thermoplastic polyolefin elastomer layer may be 0.7-0.9 mm, for example, 0.7 mm, 0.75 mm, 0.8 mm, 0.85 mm, 0.9 mm, or a range consisting of any two of the above values.

[0089] In some optional embodiments, the thickness of the second thermoplastic polyolefin elastomer layer may be 0.6-0.7 mm, for example, 0.6 mm, 0.65 mm, 0.7 mm, or a range consisting of any two of the above values.

[0090] The embodiment of the present application sets the thickness of the first thermoplastic polyolefin elastomer layer and the thickness of the second thermoplastic polyolefin elastomer layer within the above range, thereby further improving the deformation resistance of the first thermoplastic polyolefin elastomer layer, thereby further reducing the possibility of the first thermoplastic polyolefin elastomer layer being wrinkled or damaged during the hot pressing bonding process.

[0091] In a second aspect, the present application embodiment provides a method for preparing the thermoplastic polyolefin elastomer plastic steel tile of the first aspect of the present application, comprising the following steps:

[0092] Compounding the first thermoplastic polyolefin elastomer layer, the inner reinforcement layer, and the second thermoplastic polyolefin elastomer layer to obtain an inner reinforcement waterproof membrane;

[0093] The internally reinforced waterproof membrane and the metal plate are hot-pressed and bonded under the first condition to obtain a composite body;

[0094] The optional anti-corrosion base film and the composite body are hot-pressed and bonded under the second condition to obtain a thermoplastic polyolefin elastomer plastic steel tile.

[0095] The types and amounts of the various components involved in the second aspect of the present application are the same as the types and amounts of the corresponding components of the thermoplastic polyolefin elastomer plastic steel tile in the first aspect of the present application, and will not be repeated here.

[0096] It should be noted that the composite method of the internally reinforced waterproof membrane in the present application is not limited, and a composite method commonly used in the art can be used. For example, the first thermoplastic polyolefin elastomer layer and the internal reinforcement layer can be composited first, and then composited with the second thermoplastic polyolefin elastomer layer.

[0097] In some optional embodiments, the first thermoplastic polyolefin elastomer layer and the inner reinforcement layer are compounded, and then compounded with the second thermoplastic polyolefin elastomer layer by thermal compression bonding.

[0098] Continue to refer Figure 1When the thermoplastic polyolefin elastomer plastic steel tile in the embodiment of the present application is hot-pressed and bonded, the high-temperature heat source is transferred from the metal plate 21 side to the inner reinforced waterproof membrane 10 side, and the heat passes through the second thermoplastic polyolefin elastomer layer 13 and the inner reinforcement layer 12 in turn to reach the first thermoplastic polyolefin elastomer layer 11. Since the inner reinforcement layer 12 is provided in the waterproof membrane in the embodiment of the present application, the first thermoplastic polyolefin elastomer layer 11 can be protected during hot-pressing and bonding to prevent it from wrinkling or folding due to heat.

[0099] In some optional embodiments, the temperature of the first condition may be 180-220° C., the pressure of the first condition may be 0.3-0.6 MPa, and the time of the first condition may be 10-60 s.

[0100] The embodiment of the present application sets the temperature, pressure and time of the first condition within the above range, so that the temperature of the first condition and the melting point of the second thermoplastic polyolefin elastomer layer can cooperate with each other, so that the surface of the second thermoplastic polyolefin elastomer layer is in a slightly molten state in a relatively short time, which is beneficial to its bonding with the metal plate, thereby further improving the adhesion of the second thermoplastic polyolefin elastomer layer.

[0101] In some optional embodiments, the temperature of the second condition may be 130-200° C., the pressure of the second condition may be 0.3-0.6 MPa, and the time of the second condition may be 10-30 s.

[0102] The thermoplastic polyolefin elastomer plastic steel tile of the embodiment of the present application can be applied to the building materials industry.

[0103] Example

[0104] The following examples describe the disclosure of the present application in more detail, and these examples are for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present application are apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further treatment, and the instruments used in the examples are commercially available.

[0105] Example 1

[0106] (1) Preparation of internally reinforced waterproof membrane

[0107] Raw materials for the first thermoplastic polyolefin elastomer layer: 84 parts of polyolefin resin, wherein the polyolefin resin includes 70 parts of CA10A and 14 parts of CA60A; 10 parts of flame retardant masterbatch; 3 parts of antioxidant masterbatch; and 3 parts of color masterbatch.

[0108] The inner reinforcement layer is made of polyester fiber mesh cloth.

[0109] Raw materials for the second thermoplastic polyolefin elastomer layer: 14 parts of maleic anhydride grafted modified polyethylene, with a grafting rate of 1.0%-1.3%; 20 parts of maleic anhydride grafted modified polypropylene, with a grafting rate of 1.0%-1.3%; 60 parts of polyolefin resin, wherein the polyolefin resin includes 30 parts of NS06, 20 parts of 3000, and 10 parts of CA10A; 3 parts of antioxidant masterbatch; and 3 parts of color masterbatch.

[0110] The materials of the first thermoplastic polyolefin elastomer layer are mixed to obtain a mixed material, the mixed material is introduced into a screw extruder for melt extrusion, and the melt extruded material and one side of the polyester fiber mesh cloth are calendered and shaped. The raw materials of the second thermoplastic polyolefin elastomer layer are mixed to obtain a mixed material, the mixed material is introduced into a screw extruder for melt extrusion, and the melt extruded material and the other side of the polyester fiber mesh cloth are calendered and shaped to obtain an internally reinforced waterproof coiled material.

[0111] The total thickness of the fabric-reinforced thermoplastic polyolefin elastomer waterproof membrane is 1.5 mm, the thickness of the first TPO layer is 0.85 mm, and the thickness of the second TPO layer is 0.65 mm.

[0112] (2) Preparation of thermoplastic polyolefin elastomer plastic steel tiles

[0113] The metal plate is made of galvanized steel.

[0114] The anti-corrosion base film is made of modified PVC film.

[0115] The internally reinforced waterproof membrane and the metal plate are hot-pressed and bonded at a temperature of 190°C and a pressure of 0.6 MPa for 30 seconds to obtain a composite. The composite is then hot-pressed and bonded to the anti-corrosion base film under the same hot-pressing bonding conditions as in the previous step to obtain a thermoplastic polyolefin elastomer plastic steel tile.

[0116] Example 2

[0117] (1) Preparation of internally reinforced waterproof membrane

[0118] Raw materials for the first thermoplastic polyolefin elastomer layer: 84 parts of polyolefin resin, wherein the polyolefin resin includes 60 parts of CA10A, 14 parts of CA60A, and 10 parts of 3020; 10 parts of flame retardant masterbatch; 3 parts of antioxidant masterbatch; and 3 parts of color masterbatch.

[0119] The inner reinforcement layer is made of polyester fiber mesh cloth.

[0120] Raw materials for the second thermoplastic polyolefin elastomer layer: 20 parts of maleic anhydride grafted modified polybutadiene, with a grafting rate of 4%-5%; 14 parts of maleic anhydride grafted modified POE, with a grafting rate of 0.8%-1.5%; 60 parts of polyolefin resin, wherein the polyolefin resin includes 30 parts of NS06, 20 parts of 3020, and 10 parts of CA10A; 3 parts of antioxidant masterbatch and 3 parts of color masterbatch.

[0121] The total thickness of the fabric-reinforced thermoplastic polyolefin elastomer waterproof membrane is 1.5 mm, the thickness of the first TPO layer is 0.85 mm, and the thickness of the second TPO layer is 0.65 mm.

[0122] (2) Preparation of thermoplastic polyolefin elastomer plastic steel tiles

[0123] The preparation process of the thermoplastic polyolefin elastomer plastic steel tile in Example 2 is the same as that in Example 1.

[0124] Example 3

[0125] (1) Preparation of internally reinforced waterproof membrane

[0126] Raw materials for the first thermoplastic polyolefin elastomer layer: 84 parts of polyolefin resin, wherein the polyolefin resin includes 50 parts of CA10A, 24 parts of CA60A, and 10 parts of 6102; 10 parts of flame retardant masterbatch; 3 parts of antioxidant masterbatch; and 3 parts of color masterbatch.

[0127] The inner reinforcement layer is made of glass fiber mesh cloth.

[0128] Raw materials for the second thermoplastic polyolefin elastomer layer: 14 parts of acrylic acid grafted modified polyethylene, the grafting rate of acrylic acid grafted modified polyethylene is 2.5%-3.2%, 20 parts of acrylic acid grafted modified polypropylene, the grafting rate of acrylic acid grafted modified polypropylene is 1.1%-1.3%; 60 parts of polyolefin resin, wherein the polyolefin resin includes 40 parts of NS06 and 20 parts of 3020; 3 parts of antioxidant masterbatch; 3 parts of masterbatch.

[0129] The total thickness of the fabric-reinforced thermoplastic polyolefin elastomer waterproof membrane is 1.5 mm, the thickness of the first TPO layer is 0.85 mm, and the thickness of the second TPO layer is 0.65 mm.

[0130] (2) Preparation of thermoplastic polyolefin elastomer plastic steel tiles

[0131] The metal plate is made of aluminum.

[0132] The anti-corrosion base film is made of modified POE film, manufacturer: Guangzhou Lushan New Materials Co., Ltd., model: FN5110.

[0133] The internally reinforced waterproof membrane and the metal plate are hot-pressed and bonded at a temperature of 190°C and a pressure of 0.6 MPa for 30 seconds to obtain a composite. The composite is then hot-pressed and bonded to the anti-corrosion base film at a temperature of 140°C and a pressure of 0.6 MPa for 20 seconds to obtain a thermoplastic polyolefin elastomer plastic steel tile.

[0134] Example 4

[0135] (1) Preparation of internally reinforced waterproof membrane

[0136] Raw materials for the first thermoplastic polyolefin elastomer layer: 84 parts of polyolefin resin, wherein the polyolefin resin includes 50 parts of CA10A, 24 parts of CA60A, and 10 parts of 3020; 10 parts of flame retardant masterbatch; 3 parts of antioxidant masterbatch; and 3 parts of color masterbatch.

[0137] The inner reinforcement layer is made of polyester fiber mesh cloth;

[0138] Raw materials for the second thermoplastic polyolefin elastomer layer: 34 parts of maleic anhydride grafted modified POE, with a grafting rate of 0.8%-1.5%; 60 parts of polyolefin resin, wherein the polyolefin resin includes 30 parts of NS06, 20 parts of 3000, and 10 parts of 6102; 3 parts of antioxidant masterbatch; and 3 parts of color masterbatch.

[0139] The total thickness of the fabric-reinforced thermoplastic polyolefin elastomer waterproof membrane is 1.5 mm, the thickness of the first TPO layer is 0.85 mm, and the thickness of the second TPO layer is 0.65 mm.

[0140] (2) Preparation of thermoplastic polyolefin elastomer plastic steel tiles

[0141] The preparation process of the thermoplastic polyolefin elastomer plastic steel tile in Example 4 is the same as that in Example 3.

[0142] Example 5

[0143] The preparation process is the same as that of Example 1 except that the mass ratio of the polyolefin resin to the graft-modified polyolefin resin in the second thermoplastic polyolefin elastomer layer is different in the preparation of the internally reinforced waterproof membrane.

[0144] Raw materials for the second thermoplastic polyolefin elastomer layer: 16.5 parts of maleic anhydride grafted modified polyethylene, with a grafting rate of 1.0%-1.3%; 23.5 parts of maleic anhydride grafted modified polypropylene, with a grafting rate of 1.0%-1.3%; 54 parts of polyolefin resin, wherein the polyolefin resin includes 27 parts of NS06, 18 parts of 3000, and 9 parts of CA10A; 3 parts of antioxidant masterbatch; and 3 parts of masterbatch.

[0145] Example 6

[0146] The preparation process is the same as that of Example 1 except that the mass ratio of the polyolefin resin to the graft-modified polyolefin resin in the second thermoplastic polyolefin elastomer layer is different in the preparation of the internally reinforced waterproof membrane.

[0147] Raw materials for the second thermoplastic polyolefin elastomer layer: 9.9 parts of maleic anhydride grafted modified polyethylene, with a grafting rate of 1.0%-1.3%; 14.1 parts of maleic anhydride grafted modified polypropylene, with a grafting rate of 1.0%-1.3%; 70 parts of polyolefin resin, wherein the polyolefin resin includes 35 parts of NS06, 23.3 parts of 3000, and 11.7 parts of CA10A; 3 parts of antioxidant masterbatch; and 3 parts of masterbatch.

[0148] Example 7

[0149] The preparation process is the same as that of Example 1 except that the mass ratio of the polyolefin resin to the graft-modified polyolefin resin in the second thermoplastic polyolefin elastomer layer is different in the preparation of the internally reinforced waterproof membrane.

[0150] Raw materials for the second thermoplastic polyolefin elastomer layer: 12.4 parts of maleic anhydride grafted modified polyethylene, with a grafting rate of 1.0%-1.3%; 17.6 parts of maleic anhydride grafted modified polypropylene, with a grafting rate of 1.0%-1.3%; 64 parts of polyolefin resin, wherein the polyolefin resin includes 32 parts of NS06, 21.3 parts of 3000, and 10.7 parts of CA10A; 3 parts of antioxidant masterbatch; and 3 parts of masterbatch.

[0151] Example 8

[0152] Except that in the preparation of the internally reinforced waterproof membrane, the grafting rate of the graft-modified polyolefin resin in the second thermoplastic polyolefin elastomer layer is different from that in the embodiment 1, the rest of the preparation process is the same as that of Example 1.

[0153] In the second thermoplastic polyolefin elastomer layer, the grafting rate of maleic anhydride graft-modified polyethylene is 0.1%-0.2%; the grafting rate of maleic anhydride graft-modified polypropylene is 0.2%-0.3%.

[0154] Example 9

[0155] Except that in the preparation of the internally reinforced waterproof membrane, the total thickness of the textile internally reinforced thermoplastic polyolefin elastomer waterproof membrane, the thickness of the first TPO layer and the second TPO layer are different from those in Example 1, the rest of the preparation process is the same as that in Example 1. The total thickness of the textile internally reinforced thermoplastic polyolefin elastomer waterproof membrane is 1.6 mm, the thickness of the first TPO layer is 0.9 mm, and the thickness of the second TPO layer is 0.7 mm.

[0156] Comparative Example 1

[0157] Except that the internally reinforced waterproof membrane does not contain glass fiber mesh cloth, the rest of the preparation process is the same as that of Example 1.

[0158] Comparative Example 2

[0159] Except that the waterproof membrane does not contain polyester fiber mesh cloth in the preparation of the internally reinforced waterproof membrane, the rest of the preparation process is the same as that of Example 3.

[0160] Comparative Example 3

[0161] Except that the second thermoplastic polyolefin elastomer layer is different in the preparation of the internally reinforced waterproof membrane, the rest of the preparation process is the same as that of Example 1.

[0162] The second thermoplastic polyolefin elastomer layer includes the following components: 24 parts of maleic anhydride grafted modified polyethylene, the grafting rate of maleic anhydride grafted modified polyethylene is 1.0%-1.3%; 30 parts of maleic anhydride grafted modified polypropylene, the grafting rate of maleic anhydride grafted modified polypropylene is 1.0%-1.3%; 40 parts of polyolefin resin, wherein the polyolefin resin includes 20 parts of NS06, 10 parts of 3000, and 10 parts of CA10A; 3 parts of antioxidant masterbatch; and 3 parts of masterbatch.

[0163] Test part:

[0164] (1) High and low temperature alternating test: The test is carried out in accordance with the requirements of GB / T 9535-1998 "Design, Identification and Finalization of Crystalline Silicon Photovoltaic Modules for Terrestrial Use". After taking out the samples, the test is carried out according to the post-aging test items specified in the standard. The test chamber temperature completes 50 cycles from 85°C to -40°C. The highest and lowest temperatures should be within ±2°C of the set value. At temperatures above 25°C, the relative humidity should be maintained within 85% ±5% of the set value. In one cycle, at the highest temperature, it should be kept stable for a minimum of 20 hours, and at the lowest temperature, it should be kept stable for a maximum of 10 hours and a minimum of 0.5 hours.

[0165] (2) 23°C peel strength: The test is conducted in accordance with the requirements of GB / T 2790-1995 “Test method for 180° peel strength of adhesives - Flexible materials to rigid materials”.

[0166] Heat treatment (135°C, 28d) peel strength: Place the sample in a 135°C oven for heat treatment for 28 days. After taking it out and naturally cooling it to room temperature, test it according to the requirements of GB / T 2790-1995 "Adhesive 180° Peel Strength Test Method - Flexible Materials to Rigid Materials".

[0167] (3) Weldability: The test method for weldability is to use a hot air welding gun to weld the overlapping edges at a uniform welding speed and a welding temperature of approximately 300°C.

[0168] The test results of the thermoplastic polyolefin elastomer plastic steel tiles of Examples 1-9 and Comparative Examples 1-3 are shown in Table 1.

[0169] Table 1

[0170]

[0171]

[0172] It can be seen from Examples 1-9 and Comparative Examples 1-3 that providing an inner reinforcement layer in the waterproof membrane can reduce the risk of the thermoplastic polyolefin elastomer layer being wrinkled or damaged during hot pressing and bonding, improve the dimensional stability of the waterproof membrane, and improve the adhesion between the waterproof membrane and the metal plate.

[0173] It can also be seen from Examples 1-9 and Comparative Examples 1-3 that the composition and ratio of the second thermoplastic polyolefin elastomer layer are different, and the test results are slightly different. When the mass ratio of the polyolefin resin and the grafted modified polyolefin resin in the second thermoplastic polyolefin elastomer layer is between (1.35-2.92): 1, the 23°C peel strength and heat treatment (135°C, 28d) peel strength of the waterproof membrane can be further improved, thereby reducing the thermoplastic polyolefin elastomer layer from being wrinkled or damaged during the hot pressing bonding process, and can also improve the dimensional stability of the waterproof membrane and improve the adhesion between the waterproof membrane and the metal plate.

[0174] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A thermoplastic polyolefin elastomer plastic steel tile, characterized in that: The thermoplastic polyolefin elastomer plastic steel tile comprises an internally reinforced waterproof coiled material, a metal plate and an anti-corrosion base membrane stacked along a first direction; The inner reinforced waterproof membrane comprises a first thermoplastic polyolefin elastomer layer, an inner reinforcement layer and a second thermoplastic polyolefin elastomer layer stacked along a first direction, wherein the second thermoplastic polyolefin elastomer layer is located on a side close to the metal plate; The anti-corrosion base film is arranged on a side of the metal plate away from the second thermoplastic polyolefin elastomer layer; Based on 100 parts by weight of the second thermoplastic polyolefin elastomer layer, the second thermoplastic polyolefin elastomer layer comprises the following components: Polyolefin resin: 50-70 parts, graft modified polyolefin resin: 20-40 parts, additives: 3-11 parts; In the second thermoplastic polyolefin elastomer layer, the mass ratio of the polyolefin resin to the grafted modified polyolefin resin is (1.35-2.92): 1; the grafting rate of the grafted modified polyolefin resin is 0.6%-5%; the melting point of the second thermoplastic polyolefin elastomer layer is 150-170°C; The inner reinforcement layer includes one or more of glass fiber mesh cloth and polyester fiber mesh cloth.

2. The thermoplastic polyolefin elastomer plastic steel tile according to claim 1, characterized in that: Based on 100 parts by weight of the first thermoplastic polyolefin elastomer layer, the first thermoplastic polyolefin elastomer layer includes the following components: 74-90 parts by weight of polyolefin resin and 10-26 parts by weight of additives.

3. The thermoplastic polyolefin elastomer plastic steel tile according to claim 2, characterized in that: The additives include one or more of antioxidant materials, flame retardant materials and pigments.

4. The thermoplastic polyolefin elastomer plastic steel tile according to claim 1, characterized in that: The grafting monomer of the graft-modified polyolefin resin includes one or more of maleic anhydride, acrylic acid, glycidyl methacrylate and styrene; and / or, The main resin of the graft-modified polyolefin resin includes one or more of polyethylene, polypropylene, polybutadiene and ethylene-octene copolymer.

5. The thermoplastic polyolefin elastomer plastic steel tile according to claim 1, characterized in that: The mesh number of the glass fiber mesh cloth is 1-5 meshes, and the mesh number of the polyester fiber mesh cloth is 1-5 meshes; and / or, The metal plate includes one or more of galvanized steel plate, galvanized steel plate, aluminum plate, aluminum manganese plate, copper plate, iron plate and tin plate; and / or, The anti-corrosion base film includes one or more of a modified polyvinyl chloride film and a modified polyolefin film.

6. The thermoplastic polyolefin elastomer plastic steel tile according to claim 1, characterized in that: The thickness of the first thermoplastic polyolefin elastomer layer is greater than the thickness of the second thermoplastic polyolefin elastomer layer; and / or, The thickness of the first thermoplastic polyolefin elastomer layer is 0.7-0.9 mm; and / or, The thickness of the second thermoplastic polyolefin elastomer layer is 0.6-0.7 mm.

7. A method for preparing the thermoplastic polyolefin elastomer plastic steel tile according to any one of claims 1 to 6, characterized in that: The following steps are involved: Compounding the first thermoplastic polyolefin elastomer layer, the inner reinforcement layer, and the second thermoplastic polyolefin elastomer layer to obtain an inner reinforcement waterproof membrane; The internally reinforced waterproof coiled material and the metal plate are hot-pressed and bonded under the first condition to obtain a composite body; The anti-corrosion base film and the composite are hot-pressed and bonded under the second condition to obtain a thermoplastic polyolefin elastomer plastic steel tile.

8. The preparation method according to claim 7, characterized in that: The temperature of the first condition is 180-220° C., the pressure of the first condition is 0.3-0.6 MPa, and the time of the first condition is 10-60 s; and / or, The temperature of the second condition is 130-200° C., the pressure of the second condition is 0.3-0.6 MPa, and the time of the second condition is 10-30 s.