A kind of impact and wear resistant agent for concrete and preparation method thereof
By using anti-impact and wear-resistant agents with components such as cast stone powder in concrete, the impact-resistant, wear-resistant, impermeable and anti-cracking properties of concrete are improved, and the problems of erosion and wear of concrete materials and corrosion of steel bars in water conservancy projects are solved, and safety is achieved. Environmental protection and resource saving effects.
Patent Information
- Application Number
- CN202410351304.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing concrete materials in water conservancy projects pose engineering safety threats due to erosion, wear, cavitation and other phenomena. In addition, existing anti-impact and wear-resistant agents have problems such as steel bar corrosion, high cost, and poor durability, making it difficult to effectively improve the impact and wear resistance of concrete. performance and compressive strength.
Using cast stone powder, calcium carbide slag, volcanic ash, diatomite, recycled diamond scrap micro powder, nano filler, fiber, slag material, 1,3-bis((trihydroxymethyl)methylamino)propane and imidazolidinone base Impact and wear-resistant agents composed of phenyl fluorine-containing phenyl sulfone-based polymer and other components can improve the internal structure and interface structure of concrete through mutual cooperation, thereby improving the impact and wear resistance, impermeability and crack resistance.
It significantly improves the impact and wear resistance, compressive strength, permeability and crack resistance of concrete, extends its service life, and achieves safe and environmentally friendly construction and resource conservation through the use of recycled materials and environmentally friendly polymers.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to an anti-impact and wear-resistant agent for concrete and a preparation method thereof. Background Art
[0002] With the rapid development of water conservancy engineering construction in my country, concrete materials have been widely used in hydraulic structures. Due to its advantages of abundant raw materials, low price, simple production process, high compressive strength, good durability, and wide range of strength grades, it is currently the most widely used and largest-volume building material in the world, and has long played a leading role in the materials used in water conservancy engineering construction. However, the water flow contains a large amount of suspended sediment and bedload, which, driven by high-speed water flow, have a strong destructive ability, constantly colliding and rubbing the concrete on the flow surface of hydraulic structures, causing scouring, wear, cavitation and other damage to the concrete, threatening the safety of the project. It needs to be maintained and repaired regularly, which is not only difficult to repair, but also expensive to maintain and repair. It can be seen that it is particularly important to improve the impact and wear resistance of concrete.
[0003] At present, concrete materials mainly use increasing concrete strength to improve its impact resistance and wear resistance. Although the impact resistance and wear resistance of concrete have been improved to a certain extent, the extent is not large, and it also brings various disadvantages that are difficult to overcome. The main disadvantages are the mismatch between concrete strength development and durability, poor concrete crack resistance, large shrinkage deformation, etc., which cause deformation of concrete materials and make it difficult to ensure the quality in the later stage. In addition, polymer-based impact-resistant coatings are costly and have poor durability. For example, modified epoxy-based impact-resistant mortars and protective coatings still contain a large number of volatile solvent components, and the ease of construction in humid and watery environments has not been significantly improved. The flexibility is still insufficient, and it is easy to hollow, crack, and peel off in pieces.
[0004] In order to solve the above problems, a Chinese invention patent document with publication number CN101077830A and publication date November 28, 2007 discloses a concrete anti-impact and wear-resistant agent composition and a preparation method thereof. Specifically, based on 100 parts by weight of the concrete anti-impact and wear-resistant agent composition, it contains 35 to 80 parts by weight of plasticizer, 2.0 to 6.0 parts by weight of triethanolamine, and 1.0 to 6.0 parts by weight of chloride. The composition of the invention can be a powder or liquid type. The anti-impact and wear-resistant agent of the invention has the characteristics of compactness, micro-expansion, shrinkage reduction, water reduction, plasticization, reinforcement, early strength, viscosity increase, impermeability and waterproofing, anti-freezing and anti-carbonization, significantly improves the workability of fresh concrete, improves the anti-impact and wear resistance of concrete, and prolongs its service life. However, the presence of a large amount of chloride salts can easily cause corrosion of steel bars inside the anti-impact and wear concrete, resulting in steel bar corrosion expansion, which causes the surface concrete to fall off and peel off.
[0005] It can be seen that the development of an anti-impact and wear-resistant agent for concrete that can effectively improve the impact and wear resistance, compressive strength, impermeability and crack resistance of concrete and use safe and environmentally friendly anti-impact and wear-resistant agents for concrete meets market demand, has broad market value and application prospects, and is of great significance to promoting the further application and development of concrete materials in the field of water conservancy project construction. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a safe and environmentally friendly concrete anti-impact and anti-wear agent and a preparation method thereof that can effectively improve the impact and wear resistance, compressive strength and anti-seepage and anti-cracking properties of concrete.
[0007] To achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: an impact and wear resistant agent for concrete, comprising the following components in parts by weight: 10-20 parts of cast stone powder, 8-15 parts of carbide slag, 4-8 parts of volcanic ash, 5-10 parts of diatomaceous earth, 3-5 parts of recycled diamond scrap powder, 3-5 parts of nano filler, 1-3 parts of fiber, 2-4 parts of slag, 1-3 parts of 1,3-bis((trihydroxymethyl)methylamino)propane, 3-5 parts of steel slag powder, 4-6 parts of microsilica powder, 0.5-1 parts of UEA type expansion agent, and 1-4 parts of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer.
[0008] Preferably, the particle size of the cast stone powder is 800-1200 mesh; the particle size of the carbide slag is 600-900 mesh; the particle size of the volcanic ash is 1000-1300 mesh; the particle size of the diatomaceous earth is 300-600 mesh; the particle size of the recycled diamond scrap powder is 400-700 mesh; the particle size of the steel slag powder is 3-5μm; the average particle size of the microsilica powder is 0.1-0.3μm; and the UEA type expansion agent is a UEA-6 type expansion agent.
[0009] Preferably, the nano filler is at least one of nano zinc oxide and nano aluminum oxide.
[0010] Preferably, the average particle size of the nano filler is 20-80 nm.
[0011] Preferably, the fiber is at least one of recycled boron fiber and fly ash fiber.
[0012] Preferably, the average diameter of the fibers is 3-9 μm and the length is 1-3 mm.
[0013] Preferably, the residue material is a mixture of coffee residues and apple residues in a mass ratio of (1-3):1.
[0014] Preferably, the preparation method of the imidazolidinone biphenyl fluorine-containing phenylsulfone-based polymer comprises the following steps: adding 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, and an alkaline catalyst to a high boiling point solvent, stirring and reacting at 80-90°C for 10-12 hours, and then precipitating in acetone, washing the precipitated polymer with dichloromethane 4-6 times, and then placing it in a vacuum drying oven at 80-90°C to dry to constant weight, to obtain an imidazolidinone biphenyl fluorine-containing phenylsulfone-based polymer.
[0015] Preferably, the molar ratio of the 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, alkaline catalyst and high boiling point solvent is 1:0.7:0.3:(1.6-2.0):(15-20).
[0016] Preferably, the alkaline catalyst is one or more of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate.
[0017] Preferably, the high boiling point solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone.
[0018] Another object of the present invention is to provide a method for preparing the anti-impact and wear-resistant agent for concrete, comprising the following steps: uniformly mixing the components by weight to obtain the anti-impact and wear-resistant agent for concrete.
[0019] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0020] (1) The method for preparing the impact and wear resistant agent for concrete disclosed in the present invention is to mix the components uniformly by weight, and the process is simple, the operation is convenient, the dependence on equipment is small, the preparation efficiency and the qualified rate of finished products are high, there is no pollution to the environment, it is easy to construct, and it is suitable for industrial continuous production.
[0021] (2) The impact-resistant and wear-resistant agent for concrete disclosed in the present invention comprises the following components in parts by weight: 10-20 parts of cast stone powder, 8-15 parts of carbide slag, 4-8 parts of volcanic ash, 5-10 parts of diatomaceous earth, 3-5 parts of recycled diamond scrap powder, 3-5 parts of nano filler, 1-3 parts of fiber, 2-4 parts of slag, 1-3 parts of 1,3-bis((trihydroxymethyl)methylamino)propane, 3-5 parts of steel slag powder, 4-6 parts of microsilica powder, 0.5-1 parts of UEA type expansion agent, and 1-4 parts of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer; through the mutual coordination and joint action of the components, the impact-resistant and wear-resistant agent prepared can effectively improve the impact and wear resistance, compressive strength and anti-seepage and anti-cracking performance of concrete, and is safe and environmentally friendly to use. By superimposing the particle sizes of cast stone powder, carbide slag, volcanic ash, diatomaceous earth, recycled diamond scrap powder, nano filler, steel slag powder and microsilica powder, and complementing each other's activities, adding them to concrete can effectively improve the density of the internal structure, change the microstructure of the material interface, improve durability, reduce the surface tension of the concrete interface, and thus improve impact resistance and wear resistance, improve mechanical strength and anti-seepage and crack resistance, and extend the service life of concrete.
[0022] (3) The impact and wear resistant agent for concrete disclosed by the present invention comprises at least one of recycled boron fiber and fly ash fiber as the added fiber; and the added slag material is a mixture of coffee slag and apple slag in a mass ratio of (1-3):1. These components all belong to the recycling and reuse of solid waste, which realizes the transformation of waste into treasure, not only saves resources, but also is beneficial to environmental protection. After they are added, they cooperate with other components to effectively improve mechanical strength, impact and wear resistance, and anti-seepage and anti-cracking performance; the addition of imidazolidinone biphenyl fluorinated phenyl sulfone polymer can improve the water reduction rate, and the cement particles can be dispersed by the multiple effects of the introduced imidazolidinone group, biphenyl group, fluorinated phenyl sulfone group, sulfonate group and hydroxyl group under the multiple effects of electronic effect, steric effect and conjugation effect, so as to give full play to the functions of water reduction, collapse protection and slow setting, improve the construction performance of concrete and increase the strength of concrete; at the same time, it can also improve the compatibility between the components, thereby improving the density, anti-seepage and anti-cracking and impact and wear resistance. The addition of 1,3-bis((trihydroxymethyl)methylamino)propane can not only enhance the early strength, but also improve the impermeability and density of concrete. DETAILED DESCRIPTION
[0023] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0024] Example 1
[0025] The invention discloses an impact and wear resistant agent for concrete, comprising the following components in parts by weight: 10 parts of cast stone powder, 8 parts of carbide slag, 4 parts of volcanic ash, 5 parts of diatomaceous earth, 3 parts of recycled diamond scrap powder, 3 parts of nano filler, 1 part of fiber, 2 parts of slag, 1 part of 1,3-bis((trihydroxymethyl)methylamino)propane, 3 parts of steel slag powder, 4 parts of microsilica powder, 0.5 parts of UEA type expansion agent and 1 part of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer.
[0026] The particle size of the cast stone powder is 800 mesh; the particle size of the carbide slag is 600 mesh; the particle size of the volcanic ash is 1000 mesh; the particle size of the diatomaceous earth is 300 mesh; the particle size of the recycled diamond scrap powder is 400 mesh; the particle size of the steel slag powder is 3 μm; the average particle size of the microsilica powder is 0.1 μm; and the UEA expansion agent is a UEA-6 expansion agent.
[0027] The nano filler is nano zinc oxide; the average particle size of the nano filler is 20 nm; the fiber is recycled boron fiber; the average diameter of the fiber is 3 μm and the length is 1 mm; the residue material is a mixture of coffee residue and apple residue in a mass ratio of 1:1.
[0028] The preparation method of the imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer comprises the following steps: adding 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone and an alkaline catalyst into a high boiling point solvent, stirring and reacting at 80°C for 10 hours, and then precipitating in acetone, washing the precipitated polymer with dichloromethane for 4 times, and then placing it in a vacuum dryer The polymer was dried in an oven at 80°C to a constant weight to obtain an imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer; the molar ratio of the 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, alkaline catalyst, and high boiling point solvent was 1:0.7:0.3:1.6:15; the alkaline catalyst was sodium hydroxide; and the high boiling point solvent was dimethyl sulfoxide. The polymer was tested by GPC. n =13720 g / mol, M W / M n =1.372; element quantitative analysis confirmed that the molar ratio of the structural units introduced by 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, and 3,3'-diamino-4,4'-difluorodiphenyl sulfone in the polymer was approximately 1:0.7:0.3, which was the same as the theoretical value.
[0029] A method for preparing the anti-impact and wear-resistant agent for concrete comprises the following steps: uniformly mixing the components according to weight parts to obtain the anti-impact and wear-resistant agent for concrete.
[0030] Example 2
[0031] An impact and wear resistant agent for concrete comprises the following components in parts by weight: 13 parts of cast stone powder, 10 parts of carbide slag, 5 parts of volcanic ash, 6 parts of diatomaceous earth, 3.5 parts of recycled diamond scrap powder, 3.5 parts of nano filler, 1.5 parts of fiber, 2.5 parts of slag, 1.5 parts of 1,3-bis((trihydroxymethyl)methylamino)propane, 3.5 parts of steel slag powder, 4.5 parts of microsilica powder, 0.6 parts of UEA type expansion agent, and 2 parts of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer.
[0032] The particle size of the cast stone powder is 900 mesh; the particle size of the carbide slag is 700 mesh; the particle size of the volcanic ash is 1100 mesh; the particle size of the diatomaceous earth is 400 mesh; the particle size of the recycled diamond scrap powder is 500 mesh; the particle size of the steel slag powder is 3.5μm; the average particle size of the microsilica powder is 0.15μm; the UEA type expansion agent is UEA-6 type expansion agent; the nano filler is nano alumina; the average particle size of the nano filler is 30nm; the fiber is fly ash fiber; the average diameter of the fiber is 5μm and the length is 1.5mm; the slag material is a mixture of coffee grounds and apple pomace in a mass ratio of 1.5:1.
[0033] The preparation method of the imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer comprises the following steps: adding 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone and an alkaline catalyst into a high boiling point solvent, stirring and reacting at 83°C for 10.5 hours, and then precipitating in acetone, washing the precipitated polymer with dichloromethane for 5 times, and then placing it in a vacuum drying oven for 8 hours. The mixture was dried at 3° C. to constant weight to obtain an imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer; the molar ratio of the 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, alkaline catalyst, and high boiling point solvent was 1:0.7:0.3:1.7:17; the alkaline catalyst was potassium hydroxide; and the high boiling point solvent was N,N-dimethylformamide.
[0034] A method for preparing the anti-impact and wear-resistant agent for concrete comprises the following steps: uniformly mixing the components according to weight parts to obtain the anti-impact and wear-resistant agent for concrete.
[0035] Example 3
[0036] An impact and wear resistant agent for concrete comprises the following components in parts by weight: 15 parts of cast stone powder, 12 parts of carbide slag, 6 parts of volcanic ash, 7.5 parts of diatomaceous earth, 4 parts of recycled diamond scrap powder, 4 parts of nano filler, 2 parts of fiber, 3 parts of slag, 2 parts of 1,3-bis((trihydroxymethyl)methylamino)propane, 4 parts of steel slag powder, 4 parts of microsilica powder, 0.7 parts of UEA type expansion agent, and 2.5 parts of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer.
[0037] The particle size of the cast stone powder is 1000 mesh; the particle size of the carbide slag is 750 mesh; the particle size of the volcanic ash is 1150 mesh; the particle size of the diatomaceous earth is 450 mesh; the particle size of the recycled diamond scrap powder is 550 mesh; the particle size of the steel slag powder is 4μm; the average particle size of the microsilica powder is 0.2μm; the UEA type expansion agent is UEA-6 type expansion agent; the nano filler is nano zinc oxide; the average particle size of the nano filler is 60nm; the fiber is recycled boron fiber; the average diameter of the fiber is 6μm and the length is 2mm; the slag material is a mixture of coffee grounds and apple pomace in a mass ratio of 2:1.
[0038] The preparation method of the imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer comprises the following steps: adding 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone and an alkaline catalyst into a high boiling point solvent, stirring and reacting at 85°C for 11 hours, and then precipitating in acetone, washing the precipitated polymer with dichloromethane for 5 times, and then placing it in a vacuum drying oven. The mixture is dried at 85° C. to a constant weight to obtain an imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer; the molar ratio of the 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, alkaline catalyst, and high boiling point solvent is 1:0.7:0.3:1.8:18; the alkaline catalyst is sodium carbonate; and the high boiling point solvent is N-methylpyrrolidone.
[0039] A method for preparing the anti-impact and wear-resistant agent for concrete comprises the following steps: uniformly mixing the components according to weight parts to obtain the anti-impact and wear-resistant agent for concrete.
[0040] Example 4
[0041] An impact and wear resistant agent for concrete comprises the following components in parts by weight: 18 parts of cast stone powder, 13 parts of carbide slag, 7.5 parts of volcanic ash, 9 parts of diatomaceous earth, 4.5 parts of recycled diamond scrap powder, 4.5 parts of nano filler, 2.5 parts of fiber, 3.5 parts of slag, 2.5 parts of 1,3-bis((trihydroxymethyl)methylamino)propane, 4.5 parts of steel slag powder, 5.5 parts of microsilica powder, 0.9 parts of UEA type expansion agent, and 3.5 parts of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer.
[0042] The particle size of the cast stone powder is 1100 mesh; the particle size of the carbide slag is 850 mesh; the particle size of the volcanic ash is 1250 mesh; the particle size of the diatomaceous earth is 550 mesh; the particle size of the recycled diamond scrap powder is 650 mesh; the particle size of the steel slag powder is 4.5μm; the average particle size of the microsilica powder is 0.25μm; the UEA type expansion agent is a UEA-6 type expansion agent; the nano filler is a mixture of nano zinc oxide and nano aluminum oxide in a mass ratio of 1:3; the average particle size of the nano filler is 70nm; the fiber is a mixture of recycled boron fiber and fly ash fiber in a mass ratio of 1:3; the average diameter of the fiber is 8μm and the length is 2.5mm; the slag material is a mixture of coffee grounds and apple pomace in a mass ratio of 2.5:1.
[0043] The preparation method of the imidazolidinone biphenyl fluorine-containing phenylsulfone-based polymer comprises the following steps: adding 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone and an alkaline catalyst into a high boiling point solvent, stirring and reacting at 88°C for 11.5 hours, and then precipitating in acetone, washing the precipitated polymer with dichloromethane for 6 times, and then drying it in a vacuum drying oven at 88°C to constant weight to obtain the imidazolidinone biphenyl fluorine-containing phenylsulfone-based polymer; the 5 The molar ratio of 5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, alkaline catalyst and high boiling point solvent is 1:0.7:0.3:1.9:19; the alkaline catalyst is a mixture of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate in a mass ratio of 1:1:3:2; the high boiling point solvent is a mixture of dimethyl sulfoxide, N,N-dimethylformamide and N-methylpyrrolidone in a mass ratio of 1:3:5.
[0044] A method for preparing the anti-impact and wear-resistant agent for concrete comprises the following steps: uniformly mixing the components according to weight parts to obtain the anti-impact and wear-resistant agent for concrete.
[0045] Example 5
[0046] The invention discloses an impact and wear resistant agent for concrete, comprising the following components in parts by weight: 20 parts of cast stone powder, 15 parts of carbide slag, 8 parts of volcanic ash, 10 parts of diatomaceous earth, 5 parts of recycled diamond scrap powder, 5 parts of nano filler, 3 parts of fiber, 4 parts of slag, 3 parts of 1,3-bis((trihydroxymethyl)methylamino)propane, 5 parts of steel slag powder, 6 parts of microsilica powder, 1 part of UEA type expansion agent, and 4 parts of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer.
[0047] The particle size of the cast stone powder is 1200 mesh; the particle size of the carbide slag is 900 mesh; the particle size of the volcanic ash is 1300 mesh; the particle size of the diatomaceous earth is 600 mesh; the particle size of the recycled diamond scrap powder is 700 mesh; the particle size of the steel slag powder is 5μm; the average particle size of the microsilica powder is 0.3μm; the UEA type expansion agent is UEA-6 type expansion agent; the nano filler is nano zinc oxide; the average particle size of the nano filler is 80nm; the fiber is recycled boron fiber; the average diameter of the fiber is 9μm and the length is 3mm; the slag material is a mixture of coffee grounds and apple pomace in a mass ratio of 3:1.
[0048] The preparation method of the imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer comprises the following steps: adding 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone and an alkaline catalyst into a high boiling point solvent, stirring and reacting at 90°C for 12 hours, and then precipitating in acetone, washing the precipitated polymer with dichloromethane for 6 times, and then placing it in a vacuum The mixture was dried in a drying oven at 90° C. to a constant weight to obtain an imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer; the molar ratio of the 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, alkaline catalyst, and high boiling point solvent was 1:0.7:0.3:2:20; the alkaline catalyst was potassium carbonate; and the high boiling point solvent was dimethyl sulfoxide.
[0049] A method for preparing the anti-impact and wear-resistant agent for concrete comprises the following steps: uniformly mixing the components according to weight parts to obtain the anti-impact and wear-resistant agent for concrete.
[0050] Comparative Example 1
[0051] This example provides an impact and wear resistant agent for concrete, which is basically the same as Example 1, except that no recycled diamond scrap powder and slag are added in step S1.
[0052] Comparative Example 2
[0053] This example provides an impact and wear resistant agent for concrete, which is basically the same as Example 1, except that 1,3-bis((trihydroxymethyl)methylamino)propane is not added, and BASF RHEOPLUS 420 polycarboxylate water reducer is used instead of imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer.
[0054] In order to further illustrate the beneficial technical effects of the impact and wear resistant agent for concrete involved in each embodiment of the present invention, the impact and wear resistant agent for concrete involved in Examples 1-5 and Comparative Examples 1-2 was tested for relevant performances, and the test method was as follows: the ingredients were prepared according to the following mass ratios: water (tap water): cement (PO 42.5): fly ash (grade II): impact and wear resistant agent: water reducing agent (BASF RHEOPLUS 420 polycarboxylate water reducer): sand (medium sand): fine sand (5-16mm): crushed stone (16-25mm) = 150:303:76:11.37:2:760:265:790, wherein the impact and wear resistant agent is the product of each example; the mold is installed and the compressive strength, impermeability and impact and wear resistance of concrete of different ages are measured. The performance detection method refers to DL / 5150-2017 "Experimental Procedures for Hydraulic Concrete", wherein the impact and wear resistance method is the wind sand gun method with an impact angle of 90°. The test results are shown in Table 1.
[0055] Table 1
[0056] project 28d compressive strength 28d anti-seepage grade 28d impact and abrasion resistance unit MPa class h / cm Example 1 55.3 W17 12.68 Example 2 56.2 W17 13.12 Example 3 57.5 W19 13.70 Example 4 58.0 W19 14.21 Example 5 59.1 W20 14.61 Comparative Example 1 49.5 W14 10.74 Comparative Example 2 50.7 W11 11.21
[0057] As can be seen from Table 1, the concrete obtained by adding the impact and wear resistant agent for concrete involved in each embodiment of the present invention to C35 concrete has better compressive strength, impermeability and impact and wear resistance than the comparative example product, and the addition of recycled diamond scrap powder, slag, 1,3-bis((trihydroxymethyl)methylamino)propane and imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer is beneficial to improving the above properties.
[0058] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An anti-impact and wear-resistant agent for concrete, characterized in that: The invention comprises the following components in parts by weight: 10-20 parts of cast stone powder, 8-15 parts of carbide slag, 4-8 parts of volcanic ash, 5-10 parts of diatomaceous earth, 3-5 parts of recycled diamond scrap powder, 3-5 parts of nano filler, 1-3 parts of fiber, 2-4 parts of slag, 1-3 parts of 1,3-bis((trihydroxymethyl)methylamino)propane, 3-5 parts of steel slag powder, 4-6 parts of microsilica powder, 0.5-1 parts of UEA type expansion agent, and 1-4 parts of imidazolidinone biphenyl fluorinated phenylsulfone polymer; the slag is a mixture of coffee dregs and apple dregs in a mass ratio of (1-3):1; The preparation method of the imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer comprises the following steps: adding 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone and an alkaline catalyst into a high boiling point solvent, stirring and reacting at 80-90° C. for 10-12 hours, and then precipitating in acetone, washing the precipitated polymer with dichloromethane for 4-6 hours. 6 times, and then placed in a vacuum drying oven at 80-90° C. to dry to constant weight to obtain an imidazolidinone-based biphenyl fluorinated phenylsulfone-based polymer; the molar ratio of the 5,5-dimethyl-1,3-di(oxiranylmethyl)imidazolidine-2,4-dione, benzidine disulfonic acid, 3,3'-diamino-4,4'-difluorodiphenyl sulfone, alkaline catalyst, and high boiling point solvent is 1:0.7:0.3:(1.6-2.0):(15-20).
2. The impact and wear resistant agent for concrete according to claim 1, characterized in that: The particle size of the cast stone powder is 800-1200 mesh; the particle size of the carbide slag is 600-900 mesh; the particle size of the volcanic ash is 1000-1300 mesh; the particle size of the diatomaceous earth is 300-600 mesh; the particle size of the recycled diamond scrap micropowder is 400-700 mesh; the particle size of the steel slag powder is 3-5μm; the average particle size of the microsilica powder is 0.1-0.3μm; and the UEA type expansion agent is a UEA-6 type expansion agent.
3. The impact and wear resistant agent for concrete according to claim 1, characterized in that: The nano filler is at least one of nano zinc oxide and nano aluminum oxide; the average particle size of the nano filler is 20-80nm.
4. The impact and wear resistant agent for concrete according to claim 1, characterized in that: The fiber is at least one of recycled boron fiber and fly ash fiber; the average diameter of the fiber is 3-9 μm and the length is 1-3 mm.
5. The impact and wear resistant agent for concrete according to claim 1, characterized in that: The alkaline catalyst is one or more of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate.
6. The impact and wear resistant agent for concrete according to claim 1, characterized in that: The high boiling point solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide and N-methylpyrrolidone.
7. A method for preparing the impact and wear resistant agent for concrete according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: uniformly mixing the components according to weight to obtain an anti-impact and wear-resistant agent for concrete.
Citation Information
Patent Citations
Concrete impact-resistant wearable agent composition and preparation method thereof
CN101077830A
Polyurethane acoustic adhesive film and production method thereof
CN111138987A
External wall thermal insulation material for constructional engineering
CN117125940A