Antibacterial and deodorizing textile fabric and preparation method thereof
Through response surface simulation optimization model and double-layer glass reactor technology, combined with specific additives and electrospinning technology, efficient, environmentally friendly antibacterial and deodorant textile fabrics are prepared, which solves the environmental pollution, washability and poor antibacterial effect of traditional fabrics. problem, achieving stronger antibacterial and deodorizing properties and washability.
Patent Information
- Application Number
- CN202410313909.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-19
AI Technical Summary
Traditional antibacterial and deodorizing textile fabrics have problems such as environmental pollution, intolerance to washing, and poor antibacterial and deodorizing effects during use. There is a need for a textile fabric that is more environmentally friendly, washable, and has stronger antibacterial and deodorizing functions.
The response surface simulation optimization model is used to preset and optimize the proportion of raw materials, combined with a double-layer glass reactor for automatic heating and mixing, adding long-staple cotton, zinc nitrate hexahydrate, 2-methylimidazole, naringenin, Deionized water, methanol solution, polyvinylpyrrolidone, β-cyclodextrin, polycaprolactone, quaternized chitosan, and polyester are used to prepare composite nanofibers through electrospinning technology to improve the antibacterial and deodorizing properties of textile fabrics.
It achieves the preparation of high-quality, high-efficiency, environmentally friendly antibacterial and deodorizing textile fabrics, improves the antibacterial effect and washability, reduces manual operation difficulty and labor intensity, and has high commercialization and industrial production potential.
Smart Images

Figure CN118272986B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of material science and textile, and more specifically to a method for preparing an antibacterial and deodorizing textile fabric. Background Art
[0002] Textile fabrics with excellent antibacterial and deodorizing functions can be used in various scenarios, such as school uniforms, home textiles, pet products, etc., and provide consumers with a comfortable and healthy living environment. Most general antibacterial and deodorizing textile fabrics are made of pure cotton, blended, chemical fiber and other textile fabrics with good antibacterial properties. The preparation process generally uses the antibacterial finishing agent Texnology FCG002 silver ion antibacterial agent. In the preparation of antibacterial fabrics, padding or impregnation processes are often used, that is, the fabric is immersed in an aqueous solution containing an antibacterial finishing agent, so that the antibacterial finishing agent is evenly adsorbed on the surface of the fabric; the fabric impregnated with the antibacterial finishing agent is dried to allow the antibacterial finishing agent to fully penetrate into the fabric fiber; the dried fabric is baked to improve the fixing effect of the antibacterial finishing agent. In terms of deodorization treatment, a deodorant can be used in combination. The main component of the deodorant is a dispersion of organic silicate minerals, which can effectively eliminate and reduce acidic odors in fabrics, such as hydrogen sulfide, methyl mercaptan, isovaleric acid and alkaline odors, such as ammonia and trimethylamine.
[0003] However, the traditional antibacterial and deodorizing fabrics involve a certain degree of environmental pollution, poor washability, poor antibacterial and deodorizing effects, etc. in the process of using a large amount of treatment agents. Therefore, on the basis of solving the above problems, it is necessary to develop a textile fabric that reduces environmental pollution and has stronger antibacterial and deodorizing functions and strong washability than traditional antibacterial and deodorizing fabrics. This textile fabric with antibacterial and deodorizing functions uses antibacterial nanomaterials added to the fiber to make permanent antibacterial fibers, and microporous adsorption nanomaterials added to the fiber to make fibers. The two fibers are mixed together to achieve antibacterial and deodorizing effects.
[0004] Therefore, the present invention discloses a method for preparing an antibacterial and deodorizing textile fabric. The preparation process is simple, convenient and efficient, and the textile fabric with excellent antibacterial and deodorizing properties can be obtained, which has high commercialization and industrial production potential. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention discloses a method for preparing an antibacterial and deodorizing textile fabric. The preparation process is simple, convenient, and efficient, and a textile fabric with excellent antibacterial and deodorizing properties can be obtained, which has high commercialization and industrial production potential. The response surface simulation optimization model is used to preset and optimize the ratio, which can achieve accurate control of the raw material ratio, improve the quality and production efficiency of the product, and make the preparation process more efficient and cost-saving. At the same time, a double-layer glass reactor is used for automatic heating and mixing and stirring, which greatly reduces the difficulty and labor intensity of manual operation, and also ensures the uniformity and efficiency of the reaction, making the reaction process more stable and uniform. In addition, long-staple cotton, zinc nitrate hexahydrate, 2-methylimidazole, naringenin, deionized water, methanol solution, polyvinyl pyrrolidone, β-cyclodextrin, polycaprolactone, quaternized chitosan, and polyester are added to improve the antibacterial and deodorizing properties of the textile fabric; high quality, high efficiency, and environmental protection.
[0006] The present invention adopts the following technical solutions:
[0007] A method for preparing an antibacterial and deodorizing textile fabric, the method comprising:
[0008] Step 1, preparing the raw materials and reaction device for the preparation of the antibacterial and deodorizing textile fabric, wherein the raw materials for the preparation of the antibacterial and deodorizing textile fabric include long-staple cotton, zinc nitrate hexahydrate, 2-methylimidazole, naringenin, deionized water, methanol solution, polyvinyl pyrrolidone, β-cyclodextrin, polycaprolactone, quaternized chitosan, and polyester, and the ratio of the raw materials is preset and optimized by constructing an optimization model using the response surface method, and the reaction device adopts a double-layer glass reactor to achieve automatic heating and mixing and stirring;
[0009] Step 2, the zinc nitrate hexahydrate is dissolved in a methanol solution according to a preset ratio to obtain a zinc nitrate hexahydrate methanol solution, the zinc nitrate hexahydrate methanol solution and 2-methylimidazole are prepared into a mixed solution according to a preset ratio, and then added into a double-layer glass reactor, and stirred for 1 hour;
[0010] The chemical reaction equation of the zinc nitrate hexahydrate and 2-methylimidazole is:
[0011] C4H6N2+Zn(NO3)2﹒6H2O→C8H 12 N4﹒ Zn (1)
[0012] In formula (1), C4H6N2 is 2-methylimidazole, Zn(NO3)2﹒6H2O is zinc nitrate hexahydrate, and C8H 12 N4﹒ Zn is a ZIF-8 nanocarrier;
[0013] Step 3, the polyvinyl pyrrolidone, the deionized water and the naringenin are added to a double-layer glass reactor according to a preset ratio, and stirred at 30° C. for 4.5 hours to prepare a PVP-naringenin methanol solution. The PVP-naringenin methanol solution and the ZIF-8 nanocarrier are prepared into a mixed solution according to a preset ratio and added to a double-layer glass reactor, and stirred for 1 hour to prepare NAR@ZIF-8. The NAR@ZIF-8 represents a ZIF-8 nanomaterial doped with naringenin. The chemical reaction equation of the PVP-naringenin methanol solution and the ZIF-8 nanomaterial is:
[0014] PVP-C 15 O 12 O5+ZIF-8→NAR@ZIF-8 (2)
[0015] In formula (2), PVP-C 15 O 12 O5 represents PVP-naringenin methanol solution, and ZIF-8 represents ZIF-8 nanomaterials;
[0016] Step 4: The β-cyclodextrin is carbonized at high temperature in the reaction device to obtain GQDs, wherein the GQDs represent graphene quantum dots. The reaction time is 15 hours, the reaction temperature is 210° C., and the carbonization reaction equation of the β-cyclodextrin is:
[0017] C 42 H 70 O 35 →GQDs (3)
[0018] In formula (3), C 42 H 70 O 35 represents β-cyclodextrin;
[0019] Step 5: The polycaprolactone and quaternized chitosan are blended in a designated reaction device by melt blending to prepare a material QCTS-PCL with antibacterial effect, wherein QCTS-PCL represents a quaternized chitosan / polycaprolactone blend, the designated reaction device is an internal mixer, and the chemical equation for the reaction of polycaprolactone and quaternized chitosan is:
[0020] (C6H 10 O2)n+(C6H 11 NO4)m→QCTS-PCL (4)
[0021] In formula (4), (C6H 10 O2)n represents polycaprolactone, n represents the degree of polymerization of polycaprolactone, (C6H 11NO4) m represents quaternized chitosan, and m represents the degree of polymerization of quaternized chitosan;
[0022] Step 6: The QCTS-PCL and the GQDs are calcined at high temperature to produce quaternized chitosan-polycaprolactone loaded with graphene quantum dots, and the reaction temperature is 210 °C;
[0023] Step 7: The NAR@ZIF-8 and the quaternized chitosan / polycaprolactone loaded with graphene quantum dots in Step 6 are used to prepare composite nanofibers by electrospinning technology;
[0024] Step 8: The polyester, the composite nanomaterial, and the long-staple cotton are used to prepare an antibacterial and deodorant textile fabric by three-dimensional weaving technology.
[0025] As a further technical solution of the present invention, the response surface simulation optimization model uses the multiple regression analysis method to establish the correlation function between the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric and the performance indicators of the antibacterial and deodorant textile fabric. The proportion sample set of the raw materials for preparing the antibacterial and deodorant textile fabric is X = {x1,...,x i ,...,x n}, 1 ≤ i ≤ n, and the expression of the correlation function is:
[0026]
[0027] In formula (5), Y i is the performance indicator of the antibacterial and deodorant textile fabric corresponding to the proportion of the i-th raw material for preparing the antibacterial and deodorant textile fabric, x i is the proportion sample of the i-th raw material for preparing the antibacterial and deodorant textile fabric, b i is the independent variable coefficient corresponding to the proportion of the i-th raw material for preparing the antibacterial and deodorant textile fabric, n is the total number of proportion samples of the raw materials for preparing the antibacterial and deodorant textile fabric, i is the ordinal number of the proportion sample of the raw materials for preparing the antibacterial and deodorant textile fabric, b0 is the constant term coefficient, and ε is the random error term; Based on the correlation function, the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric is iteratively optimized, and the calculation formula is:
[0028]
[0029] In formula (6), x N is the updated proportion of the raw materials for preparing the antibacterial and deodorant textile fabric, x o is the current proportion of the raw materials for preparing the antibacterial and deodorant textile fabric, c1 and c2 are update acceleration coefficients used to control the global optimal solution, 0 < c1 ≠ c2 < 2, and α is the learning rate used to control the utilization degree of the optimization space, is the objective function for the current proportion of the raw materials for preparing the antibacterial and deodorant textile fabric xo The gradient of the antibacterial and deodorizing textile fabric is searched for the optimal ratio of the raw materials for preparing the antibacterial and deodorizing textile fabric through iterative calculation.
[0030] As a further technical solution of the present invention, the components of the raw materials for preparation include 65 parts by weight of the long-staple cotton, 12.5 parts by weight of the polyester, 5 parts by weight of the zinc nitrate hexahydrate, 5 parts by weight of the 2-methylimidazole, 2 parts by weight of the naringenin, 3 parts by weight of the deionized water, 4 parts by weight of the methanol solution, 1.5 parts by weight of the polyvinyl pyrrolidone, 1 part by weight of the β-cyclodextrin, 0.5 parts by weight of the polycaprolactone, and 0.5 parts by weight of the quaternized chitosan.
[0031] As a further technical solution of the present invention, the working method for preparing the composite nanofiber in step seven is: the NAR@ZIF-8 and the quaternized chitosan-polycaprolactone loaded with graphene quantum dots are mixed to prepare a spinning solution, and the spinning solution is subjected to 10KV high voltage static electricity, and the fiber diameter of the fiber deposited on the receiver is controlled by increasing the speed of the wire collection drum;
[0032] As a further technical solution of the present invention, the double-layer glass reactor includes a motor, a vacuum nozzle, a glass condenser, a reflux elbow, a thermometer, a glass reactor body, a PTFE stirring paddle, a discharge valve, a universal wheel with a brake, a constant pressure dropping funnel, a temperature display meter, a speed display adjustment meter, and a solid feeding port. The double-layer glass reactor includes a control part, a feeding part, a discharging part, a stirring part, and a display part. The motor constitutes the control part of the double-layer glass reactor. The motor is connected to the top of the double-layer glass reactor through an electric wire. The motor adopts A low-speed booster motor and a reducer are used to ensure that the equipment can perform long-term stirring work. The glass kettle body and the PTFE stirring paddle constitute the stirring part of the double-layer glass reactor. The PTFE stirring paddle is placed in the middle position inside the glass kettle body. The constant pressure dropping funnel, the glass condenser, the reflux elbow, and the solid feeding port together constitute the feeding part of the double-layer glass reactor. The constant pressure dropping funnel is placed on the left side of the motor. The constant pressure dropping funnel is equipped with a high vacuum PTFE hand valve to ensure that the internal pressure of the double-layer glass reactor remains unchanged. To prevent back suction, the glass condenser is placed on the right side of the motor, the glass condenser adopts a double-layer coiled design, so that the contact area between the glass condenser and the gaseous material is increased to improve the condensation efficiency, the vacuum nozzle is placed on the upper end of the glass condenser by connecting the vacuum pump, and the glass condenser is decompressed to accelerate the condensation speed of the glass condenser, the reflux elbow is connected to the glass condenser through a glass conduit, and is placed at the lower end of the glass condenser to separate the liquid, the thermometer is placed at the edge position inside the glass kettle body to measure the temperature of the reactant in real time, the solid feeding port is placed at the opening above the glass kettle body, the temperature display table and the speed display adjustment table together constitute the display part of the double-layer glass reactor, which is connected to the left side of the constant pressure dropping funnel through an internal communication method, the discharge valve constitutes the discharge part of the double-layer glass reactor, and is connected to the bottom of the glass kettle body through a detachable design to make the discharge work of the double-layer glass reactor thorough, and the universal wheel with brake is placed at the bottom of the stainless steel support frame to make the movement more convenient and flexible.
[0033] As a further technical solution of the present invention, the device structure adopted by the electrospinning technology includes a metering pump, a syringe, a high-voltage power supply, a capillary, a Taylor cone, and a receiver. The device structure adopted by the electrospinning technology includes a high-voltage power supply, an injection device, and a receiving device. The metering pump, the syringe, the capillary, and the Taylor cone are connected through a hollow spiral tube to form an injection device of the electrospinning machine, which is placed on the left side of the entire electrospinning machine. The Taylor cone is placed on the rightmost side of the capillary. The high-voltage power supply is connected to the lower end of the syringe through an electric wire. The receiver constitutes the receiving device of the electrospinning and is placed on the rightmost side of the electrospinning.
[0034] As a further technical solution of the present invention, the internal mixer reaction device in step five includes: a main motor, a coupling, an accelerator, a tooth section, a speed ratio gear, a cylinder, a stuffing box, a flap door, a rotor, an oil pressure system, a heating and cooling system, and an internal mixing chamber. The main motor, the coupling, the accelerator, the tooth section, and the speed ratio gear together constitute the power system of the internal mixer through a hollow connection, and are placed on the left side of the internal mixer. The cylinder, the stuffing box, the flap door, the rotor, the oil pressure system, the heating and cooling system, and the internal mixing chamber together constitute the reaction system of the internal mixer. The reaction system includes an upper part and a lower part. The upper part of the reaction system and the lower part of the reaction system are connected by a hollow connection. The flap door The plate door and the stuffing box constitute the upper part of the reaction system, the cylinder is embedded in the upper part of the reaction system, the rotor, the oil pressure system, the heating and cooling system, and the mixing chamber constitute the lower part of the reaction system. When the mixing mill is working, the rotor rotates relatively, clamps the material from the stuffing box and brings it into the roller gap to be squeezed and sheared by the rotor, and then enters the mixing chamber for mixing. The oil pressure system is placed on the outside of the rotor so that the upper structure of the reaction system can obtain sufficient hydraulic oil when working, and at the same time reduce the impact force generated by each component when working. The heating and cooling system is placed above the mixing chamber through a line connection to control the surface temperature of the rotor and the inner cavity wall of the mixing chamber.
[0035] The present invention discloses an antibacterial and deodorizing textile fabric and a preparation method thereof. The preparation process is simple, convenient and efficient, and a textile fabric with good antibacterial and deodorizing properties can be obtained, which has high commercialization and industrial production potential. The response surface simulation optimization model is used to preset and optimize the ratio, which can realize accurate control of the raw material ratio, improve the quality and production efficiency of the product, and make the preparation process more efficient and cost-saving. At the same time, a double-layer glass reactor is used for automatic heating and mixing and stirring, which greatly reduces the difficulty and labor intensity of manual operation, and also ensures the uniformity and efficiency of the reaction, making the reaction process more stable and uniform. In addition, long-staple cotton, zinc nitrate hexahydrate, 2-methylimidazole, naringenin, deionized water, methanol solution, polyvinyl pyrrolidone, β-cyclodextrin, polycaprolactone, quaternized chitosan, and polyester are added to improve the antibacterial and deodorizing properties of the textile fabric; high quality, high efficiency, and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a flow chart of a method for preparing an antibacterial and deodorizing textile fabric according to the present invention;
[0037] Figure 2 This is a schematic diagram of the proportion of raw materials in the preparation method of an antibacterial and deodorizing textile fabric of the present invention;
[0038] Figure 3 This is a structural diagram of an electrospinning machine in a method for preparing an antibacterial and deodorizing textile fabric according to the present invention;
[0039] Figure 4 It is a structural diagram of an internal mixer in a method for preparing an antibacterial and deodorizing textile fabric of the present invention;
[0040] Figure 5 The present invention is a structural diagram of a double-layer glass reactor in a method for preparing antibacterial and deodorizing textile fabrics. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] A method for preparing an antibacterial and deodorizing textile fabric, the method comprising:
[0044] Step 1, preparing the raw materials and reaction device for the preparation of the antibacterial and deodorizing textile fabric, wherein the raw materials for the preparation of the antibacterial and deodorizing textile fabric include long-staple cotton, zinc nitrate hexahydrate, 2-methylimidazole, naringenin, deionized water, methanol solution, polyvinyl pyrrolidone, β-cyclodextrin, polycaprolactone, quaternized chitosan, and polyester, and the ratio of the raw materials is preset and optimized by constructing an optimization model using the response surface method, and the reaction device adopts a double-layer glass reactor to achieve automatic heating and mixing and stirring;
[0045] Step 2, the zinc nitrate hexahydrate is dissolved in a methanol solution according to a preset ratio to obtain a zinc nitrate hexahydrate methanol solution, the zinc nitrate hexahydrate methanol solution and 2-methylimidazole are prepared into a mixed solution according to a preset ratio, and then added into a double-layer glass reactor, and stirred for 1 hour;
[0046] The chemical reaction equation of the zinc nitrate hexahydrate and 2-methylimidazole is:
[0047] C4H6N2+Zn(NO3)2﹒6H2O→C8H 12 N4﹒ Zn (1)
[0048] In formula (1), C4H6N2 is 2-methylimidazole, Zn(NO3)2﹒6H2O is zinc nitrate hexahydrate, and C8H 12 N4﹒ Zn is a ZIF-8 nanocarrier;
[0049] Step 3, the polyvinyl pyrrolidone, the deionized water and the naringenin are added to a double-layer glass reactor according to a preset ratio, and stirred at 30° C. for 4.5 hours to prepare a PVP-naringenin methanol solution. The PVP-naringenin methanol solution and the ZIF-8 nanocarrier are prepared into a mixed solution according to a preset ratio and added to a double-layer glass reactor, and stirred for 1 hour to prepare NAR@ZIF-8. The NAR@ZIF-8 represents a ZIF-8 nanomaterial doped with naringenin. The chemical reaction equation of the PVP-naringenin methanol solution and the ZIF-8 nanomaterial is:
[0050] PVP-C 15 O 12 O5+ZIF-8→NAR@ZIF-8 (2)
[0051] In formula (2), PVP-C 15 O 12 O5 represents PVP-naringenin methanol solution, and ZIF-8 represents ZIF-8 nanomaterials;
[0052] Step 4: The β-cyclodextrin is carbonized at high temperature in the reaction device to obtain GQDs, wherein the GQDs represent graphene quantum dots. The reaction time is 15 hours, the reaction temperature is 210° C., and the carbonization reaction equation of the β-cyclodextrin is:
[0053] C 42 H 70 O 35 →GQDs (3)
[0054] In formula (3), C 42 H 70 O 35 represents β-cyclodextrin;
[0055] Step 5: The polycaprolactone and quaternized chitosan are blended in a designated reaction device by melt blending to prepare a material QCTS-PCL with antibacterial effect, wherein QCTS-PCL represents a quaternized chitosan / polycaprolactone blend, the designated reaction device is an internal mixer, and the chemical equation for the reaction of polycaprolactone and quaternized chitosan is:
[0056] (C6H 10 O2)n+(C6H 11 NO4)m→QCTS-PCL (4)
[0057] In formula (4), (C6H 10 O2)n represents polycaprolactone, n represents the degree of polymerization of polycaprolactone, (C6H 11 NO4)m represents quaternary ammonium chitosan, and m represents the degree of polymerization of quaternary ammonium chitosan;
[0058] Step 6: The QCTS-PCL and the GQDs are calcined at high temperature to produce quaternized chitosan-polycaprolactone loaded with graphene quantum dots, and the reaction temperature is 210° C.
[0059] Step 7, the NAR@ZIF-8 and the quaternary ammonium chitosan / polycaprolactone loaded with graphene quantum dots described in step 6 are used to prepare composite nanofibers by electrospinning technology;
[0060] Step eight, the polyester, the composite nano material and the long-staple cotton are prepared into antibacterial and deodorizing textile fabrics by using three-dimensional textile technology.
[0061] In a specific embodiment, the above preparation process does not use any treatment agent, antibacterial nanomaterials are added to the fiber to make permanent antibacterial fiber, and microporous adsorption nanomaterials are added to the fiber to make fiber. The two kinds of fibers are mixed together to achieve antibacterial and deodorizing effects.
[0062] In this example, the antibacterial and deodorizing textile fabric group A prepared by the present method and the antibacterial and deodorizing textile fabric group B prepared by the traditional method were used as research objects. The two fabrics were smeared with equal amounts of E. coli solution, placed at room temperature for 12 hours, 24 hours, and 48 hours, and the two groups of samples were tested using an electron microscope. According to the content of E. coli under the electron microscope, the antibacterial rate of the two groups of antibacterial and deodorizing fabrics was calculated, and the data of each group was recorded in Table 1.
[0063] Table 1 Comparative statistics of bacterial content
[0064] Testing time Group A Escherichia coli (standard value ≥ 70) Group B Escherichia coli (standard value ≥ 70) 12 hours 94 90 24 hours 94.4 85 48 hours 93.5 84.5 average 94.0 86.5
[0065] Through the above antibacterial test, the antibacterial effects of group A and group B can be compared, and the effect of the antibacterial and deodorizing textile fabric prepared by this method on the hardness of the coating can be evaluated. From the test results, it can be seen that the antibacterial effect of the antibacterial and deodorizing textile fabric prepared by this method is much better than that of the traditional antibacterial and deodorizing textile fabric. This shows that the antibacterial and deodorizing textile fabric prepared by this method can enhance the antibacterial effect of the traditional antibacterial and deodorizing textile fabric and improve the antibacterial rate.
[0066] Example 2
[0067] A method for preparing an antibacterial and deodorizing textile fabric, the method comprising:
[0068] Step 1, preparing the raw materials and reaction device for the preparation of the antibacterial and deodorizing textile fabric, wherein the raw materials for the preparation of the antibacterial and deodorizing textile fabric include long-staple cotton, zinc nitrate hexahydrate, 2-methylimidazole, naringenin, deionized water, methanol solution, polyvinyl pyrrolidone, β-cyclodextrin, polycaprolactone, quaternized chitosan, and polyester, and the ratio of the raw materials is preset and optimized by constructing an optimization model using the response surface method, and the reaction device adopts a double-layer glass reactor to achieve automatic heating and mixing and stirring;
[0069] Step 2, the zinc nitrate hexahydrate is dissolved in a methanol solution according to a preset ratio to obtain a zinc nitrate hexahydrate methanol solution, the zinc nitrate hexahydrate methanol solution and 2-methylimidazole are prepared into a mixed solution according to a preset ratio, and then added into a double-layer glass reactor, and stirred for 1 hour;
[0070] The chemical reaction equation of the zinc nitrate hexahydrate and 2-methylimidazole is:
[0071] C4H6N2+Zn(NO3)2﹒6H2O→C8H 12 N4﹒ Zn (1)
[0072] In formula (1), C4H6N2 is 2-methylimidazole, Zn(NO3)2﹒6H2O is zinc nitrate hexahydrate, and C8H 12N4﹒ Zn is a ZIF-8 nanocarrier;
[0073] Step 3, the polyvinyl pyrrolidone, the deionized water and the naringenin are added to a double-layer glass reactor according to a preset ratio, and stirred at 30° C. for 4.5 hours to prepare a PVP-naringenin methanol solution. The PVP-naringenin methanol solution and the ZIF-8 nanocarrier are prepared into a mixed solution according to a preset ratio and added to a double-layer glass reactor, and stirred for 1 hour to prepare NAR@ZIF-8. The NAR@ZIF-8 represents a ZIF-8 nanomaterial doped with naringenin. The chemical reaction equation of the PVP-naringenin methanol solution and the ZIF-8 nanomaterial is:
[0074] PVP-C 15 O 12 O5+ZIF-8→NAR@ZIF-8 (2)
[0075] In formula (2), PVP-C 15 O 12 O5 represents PVP-naringenin methanol solution, and ZIF-8 represents ZIF-8 nanomaterials;
[0076] Step 4: The β-cyclodextrin is carbonized at high temperature in the reaction device to obtain GQDs, wherein the GQDs represent graphene quantum dots. The reaction time is 15 hours, the reaction temperature is 210° C., and the carbonization reaction equation of the β-cyclodextrin is:
[0077] C 42 H 70 O 35 →GQDs (3)
[0078] In formula (3), C 42 H 70 O 35 represents β-cyclodextrin;
[0079] Step 5: The polycaprolactone and quaternized chitosan are blended in a designated reaction device by melt blending to prepare a material QCTS-PCL with antibacterial effect, wherein QCTS-PCL represents a quaternized chitosan / polycaprolactone blend, the designated reaction device is an internal mixer, and the chemical equation for the reaction of polycaprolactone and quaternized chitosan is:
[0080] (C6H 10 O2)n+(C6H 11 NO4)m→QCTS-PCL (4)
[0081] In formula (4), (C6H 10O2)n represents polycaprolactone, n represents the degree of polymerization of polycaprolactone, (C6H 11 NO4)m represents quaternary ammonium chitosan, and m represents the degree of polymerization of quaternary ammonium chitosan;
[0082] Step 6: The QCTS-PCL and the GQDs are calcined at high temperature to produce quaternized chitosan-polycaprolactone loaded with graphene quantum dots, and the reaction temperature is 210° C.
[0083] Step 7, the NAR@ZIF-8 and the quaternary ammonium chitosan / polycaprolactone loaded with graphene quantum dots described in step 6 are used to prepare composite nanofibers by electrospinning technology;
[0084] Step eight, the polyester, the composite nano material and the long-staple cotton are prepared into antibacterial and deodorizing textile fabrics by using three-dimensional textile technology.
[0085] In a specific embodiment, this embodiment uses the antibacterial and deodorizing textile fabric group A prepared by the present method and the antibacterial and deodorizing textile fabric group B prepared by the traditional method as research objects, applies the same amount of E. coli solution to the two fabrics, and leaves them at room temperature for 12 hours, 24 hours, and 48 hours, and uses an electron microscope to test the two groups of samples. According to the content of E. coli under the electron microscope, the antibacterial rate of the two groups of antibacterial and deodorizing fabrics is calculated, and each group of data is recorded in Table 2.
[0086] Table 2 Comparative statistics of bacterial content
[0087] Testing time Group A Escherichia coli (standard value ≥ 70) Group B Escherichia coli (standard value ≥ 70) 12 hours 94 90 24 hours 94.4 85 48 hours 93.5 84.5 average 94.0 86.5
[0088] Through the above antibacterial test, the antibacterial effects of group A and group B can be compared, and the effect of the antibacterial and deodorizing textile fabric prepared by this method on the hardness of the coating can be evaluated. From the test results, it can be seen that the antibacterial effect of the antibacterial and deodorizing textile fabric prepared by this method is much better than that of the traditional antibacterial and deodorizing textile fabric. This shows that the antibacterial and deodorizing textile fabric prepared by this method can enhance the antibacterial effect of the traditional antibacterial and deodorizing textile fabric and improve the antibacterial rate.
[0089] Example 3
[0090] In the above embodiment, the response surface simulation optimization model uses a multivariate regression analysis method to establish a correlation function between the proportion of the raw materials for preparing the antibacterial and deodorizing textile fabrics and the performance index of the antibacterial and deodorizing textile fabrics, and the proportion sample set of the raw materials for preparing the antibacterial and deodorizing textile fabrics is X = {x1, ..., x i ,...,x n}, 1≤i≤n, the expression of the correlation function is:
[0091]
[0092] In formula (5), Y i is the performance index of the antibacterial and deodorant textile fabric corresponding to the proportion of the raw materials for preparing the i-th antibacterial and deodorant textile fabric, x i is the sample of the proportion of the raw materials for preparing the i-th antibacterial and deodorant textile fabric, b i is the independent variable coefficient corresponding to the proportion of the raw materials for preparing the i-th antibacterial and deodorant textile fabric, n is the total number of samples of the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric, i is the ordinal number of the sample of the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric, b0 is the constant term coefficient, and ε is the random error term; based on the correlation function, the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric is iteratively optimized, and the calculation formula is:
[0093]
[0094] In formula (6), x N is the updated proportion of the raw materials for preparing the antibacterial and deodorant textile fabric, x o is the current proportion of the raw materials for preparing the antibacterial and deodorant textile fabric, c1 and c2 are update acceleration coefficients used to control the global optimal solution, 0 < c1 ≠ c2 < 2, and α is the learning rate used to control the utilization degree of the optimization space, is the gradient of the objective function with respect to the current proportion x o of the raw materials for preparing the antibacterial and deodorant textile fabric, and the optimal ratio of the raw materials for preparing the antibacterial and deodorant textile fabric is searched through iterative calculation.
[0095] In a specific embodiment, in the response surface simulation optimization model, a multiple regression analysis method is used to establish the correlation function between the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric and the performance index of the antibacterial and deodorant textile fabric. This model can obtain the estimated values of each coefficient through the multiple regression analysis method, thereby constructing the mapping relationship between the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric and the performance index of the antibacterial and deodorant textile fabric. In actual production, the proportion of the raw materials for preparing the antibacterial and deodorant textile fabric can be optimized according to this correlation function to obtain a more excellent antibacterial and deodorant textile fabric. The response surface simulation optimization model should be established based on a certain amount of experimental data to ensure the accuracy and reliability of the model. In addition, when establishing the optimization model, it is necessary to fully consider the optimization objectives in the preparation process, such as improving the performance index of the product and reducing the raw material cost, etc., to ensure that the obtained optimization scheme can meet multiple optimization objectives at the same time.
[0096] The hardware working environment of the response surface simulation optimization model includes the following contents:
[0097] 1. Computer: Used to implement tasks such as the establishment, optimization calculation, and result analysis of the response surface simulation optimization model.
[0098] 2. Multiple regression analysis software: used to establish the correlation function between the proportion of raw materials for the preparation of antibacterial and deodorizing textile fabrics and the performance indicators of antibacterial and deodorizing textile fabrics, such as SPSS, Minitab and other software.
[0099] 3. Statistical analysis software: used for analysis and optimization calculation of model prediction results, such as Design-Expert, MATLAB and other software.
[0100] 4. Experimental equipment: used for experimental testing between the ratio of raw materials for the preparation of antibacterial and deodorizing textile fabrics and the performance indicators of antibacterial and deodorizing textile fabrics, such as reactors, rotary evaporators, laboratory balances and other equipment.
[0101] 5. Communication equipment: used for data transmission and information sharing between devices, such as computer networks, sensors and other equipment.
[0102] In a specific embodiment, this embodiment uses the antibacterial and deodorizing textile fabric group A prepared by the present method and the antibacterial and deodorizing textile fabric group B prepared by the traditional method as research objects, and the two fabrics are dry-cleaned and washed to the same extent to obtain samples. During the test, the bacterial solution is inoculated in an agar culture dish by drawing parallel lines, and the sample is attached to the agar surface. After culturing at room temperature for 12 hours, 24 hours, and 48 hours, the clean area along the drawn line on the agar surface due to the interruption of bacterial reproduction is checked, the antibacterial ability of the fabric is evaluated, and the antibacterial rate of the two groups of antibacterial and deodorizing fabrics is calculated, and each group of data is recorded in Table 3.
[0103] Table 3 Comparative statistics of bacterial content
[0104] Testing time Group A Escherichia coli (standard value ≥ 70) Group B Escherichia coli (standard value ≥ 70) 12 hours 94 89 24 hours 94.3 85.5 48 hours 93.3 83.2 average 93.9 85.9
[0105] The experimental results are shown in Table 3. It can be seen that the antibacterial and deodorizing textile fabric group A prepared by the present method has higher anti-dry cleaning and anti-water washing effects than the antibacterial and deodorizing textile fabric group B prepared by the traditional method, indicating that the antibacterial fiber in the antibacterial and deodorizing textile fabric prepared by the present method has a stronger antibacterial effect. This shows that the antibacterial and deodorizing textile fabric prepared by the present method improves the application performance of the antibacterial and deodorizing textile fabric in daily life.
[0106] Example 4
[0107] In the above embodiment, the components of the raw materials include 65 parts by weight of the long-staple cotton, 12.5 parts by weight of the polyester, 5 parts by weight of the zinc nitrate hexahydrate, 5 parts by weight of the 2-methylimidazole, 2 parts by weight of the naringenin, 3 parts by weight of the deionized water, 4 parts by weight of the methanol solution, 1.5 parts by weight of the polyvinyl pyrrolidone, 1 part by weight of the β-cyclodextrin, 0.5 parts by weight of the polycaprolactone, and 0.5 parts by weight of the quaternized chitosan.
[0108] In the above embodiment, the working method for preparing the composite nanofiber in step seven is: the NAR@ZIF-8 and the quaternized chitosan-polycaprolactone loaded with graphene quantum dots are mixed to prepare a spinning solution, and the spinning solution is subjected to 10KV high voltage static electricity, and the fiber diameter of the fiber deposited on the receiver is controlled by increasing the speed of the wire collection drum;
[0109] In a specific embodiment, this embodiment uses the antibacterial and deodorizing textile fabric group A prepared by this method and the antibacterial and deodorizing textile fabric group B prepared by the traditional method as research objects, cuts the two fabrics into 20*260px size, makes 3 of each fabric, places the two groups of fabrics in the center of 6 closed containers, uses a rubber dropper to drip 5 drops of alcohol into each of the 5 closed containers, tightens the lid to prevent air leakage, places in a 37°C thermostat, takes out the closed container at 1 hour, 2 hours, and 4 hours, opens the lid, and uses a concentration tester to test the alcohol concentration in the container to determine the deodorizing effect. The results are recorded in Table 4.
[0110] Table 4 Deodorization effect comparison statistics
[0111] Testing time Deodorizing effect of group A (mg / ml) B Deodorizing effect (mg / ml) 1 hour 20.3 50.6 2 hours 18.6 45.7 4 hours 16.4 44.6 average 18.4 47.0
[0112] The experimental results are shown in Table 4. It can be seen that the deodorizing effect of the antibacterial and deodorizing textile fabric group A prepared by the present method is better than that of the antibacterial and deodorizing textile fabric group B prepared by the traditional method, indicating that the antibacterial and deodorizing textile fabric group B prepared by the traditional method has a better deodorizing effect. This shows that the present method can effectively improve the deodorizing effect of textile fabrics and has better performance in practical applications.
[0113] Example 5
[0114] In the above embodiment, the components of the raw materials include 65 parts by weight of the long-staple cotton, 12.5 parts by weight of the polyester, 5 parts by weight of the zinc nitrate hexahydrate, 5 parts by weight of the 2-methylimidazole, 2 parts by weight of the naringenin, 3 parts by weight of the deionized water, 4 parts by weight of the methanol solution, 1.5 parts by weight of the polyvinyl pyrrolidone, 1 part by weight of the β-cyclodextrin, 0.5 parts by weight of the polycaprolactone, and 0.5 parts by weight of the quaternized chitosan.
[0115] In the above embodiment, the working method for preparing the composite nanofiber in step seven is: the NAR@ZIF-8 and the quaternized chitosan-polycaprolactone loaded with graphene quantum dots are mixed to prepare a spinning solution, and the spinning solution is subjected to 10KV high voltage static electricity, and the fiber diameter of the fiber deposited on the receiver is controlled by increasing the speed of the wire collection drum;
[0116] In a specific embodiment, this embodiment uses the antibacterial and deodorizing textile fabric group A prepared by the present method and the antibacterial and deodorizing textile fabric group B prepared by the traditional method as research objects, cuts the two fabrics into 20*260px size, makes 3 of each fabric, places the two groups of fabrics in the center of 6 closed containers, uses a rubber dropper to drip 5 drops of alcohol into each of the 5 closed containers, tightens the lid to prevent air leakage, places in a 37°C thermostat, takes out the closed container at 1 hour, 2 hours, and 4 hours, opens the lid, and uses a concentration tester to test the alcohol concentration in the container to determine the deodorizing effect. The results are recorded in Table 5.
[0117] Table 5 Deodorization effect comparison statistics
[0118] Testing time Deodorizing effect of group A (mg / ml) B Deodorizing effect (mg / ml) 1 hour 20.3 50.6 2 hours 18.6 45.7 4 hours 16.4 44.6 average 18.4 47.0
[0119] The experimental results are shown in Table 4. It can be seen that the deodorizing effect of the antibacterial and deodorizing textile fabric group A prepared by the present method is better than that of the antibacterial and deodorizing textile fabric group B prepared by the traditional method, indicating that the antibacterial and deodorizing textile fabric group B prepared by the traditional method has a better deodorizing effect. This shows that the present method can effectively improve the deodorizing effect of textile fabrics and has better performance in practical applications.
[0120] In the above embodiment, the reactor includes a motor 1, a vacuum nozzle 2, a glass condenser 3, a reflux elbow 4, a thermometer 5, a glass reactor body 6, a polytetrafluoroethylene stirring paddle 7, a discharge valve 8, a universal wheel with a brake 9, a constant pressure dropping funnel 10, a temperature display meter 11, a speed display adjustment meter 12, and a solid feeding port 13. The double-layer glass reactor includes a control part, a feeding part, a discharging part, a stirring part, and a display part. The motor 1 constitutes the control part of the double-layer glass reactor. The motor 1 is connected to the top of the double-layer glass reactor through an electric wire. The motor 1 adopts a low speed The power-enhancing motor and the reducer ensure that the equipment can perform long-term stirring work. The glass kettle body 6 and the PTFE stirring paddle 7 constitute the stirring part of the double-layer glass reactor. The PTFE stirring paddle 7 is placed in the middle position inside the glass kettle body 6. The constant pressure dropping funnel 10, the glass condenser 3, the reflux elbow 4, and the solid feeding port 13 together constitute the feeding part of the double-layer glass reactor. The constant pressure dropping funnel 10 is placed on the left side of the motor 1. The constant pressure dropping funnel 10 is equipped with a high vacuum PTFE hand valve to ensure that the internal pressure of the double-layer glass reactor remains unchanged. To prevent back suction, the glass condenser 3 is placed on the right side of the motor 1. The glass condenser 3 adopts a double-layer coiled design to increase the contact area between the glass condenser 3 and the gaseous material to improve the condensation efficiency. The vacuum nozzle 2 is placed at the upper end of the glass condenser 3 by connecting a vacuum pump to reduce the pressure of the glass condenser 3 to accelerate the condensation speed of the glass condenser 3. The reflux elbow 4 is connected to the glass condenser 3 through a glass conduit and is placed at the lower end of the glass condenser 3 to separate the liquid. The thermometer 5 is placed at the edge of the glass kettle 6 to To measure the temperature of the reactants in real time, the solid feeding port 13 is placed at the opening above the glass kettle body 6, the temperature display meter 11 and the speed display adjustment meter 12 together constitute the display part of the double-layer glass reactor, which is connected to the left side of the constant pressure dropping funnel 10 through an internal connection, the discharge valve 8 constitutes the discharge part of the double-layer glass reactor, and is connected to the bottom of the glass kettle body 6 through a detachable design to enable the discharge work of the double-layer glass reactor to be carried out thoroughly, and the universal wheel 9 with brake is placed at the bottom of the stainless steel support frame to make the movement more convenient and flexible.
[0121] The process of the double-layer glass reactor is illustrated below by a specific embodiment. When the present invention is working, the working method of the double-layer glass reactor is as follows: the raw materials to be reacted are placed in the raw material glass reactor body 6, according to the required proportion, and the PTFE stirring paddle 7 and the discharge valve 8 are opened. The heating temperature and time required for the reaction are set so that the reaction can proceed evenly. The temperature display table 11 detects the heating temperature in the raw material glass reactor body 6 in real time. Through the design of the present invention, the double-layer glass reactor can achieve rapid mixing of raw materials, reaction heating and cleaning of products, and has the advantages of high processing efficiency, energy and resource saving, etc.
[0122] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that these specific embodiments are only illustrative, and those skilled in the art may omit, replace, and change the details of the above methods and systems in various ways without departing from the principles and essence of the present invention. For example, merging the above method steps so as to perform substantially the same functions in substantially the same manner to achieve substantially the same results is within the scope of the present invention. Therefore, the scope of the present invention is limited only by the appended claims.
Claims
1. A method for preparing an antibacterial and deodorizing textile fabric, characterized in that: The preparation method comprises: Step 1, preparing raw materials and a reaction device for preparing antibacterial and deodorizing textile fabrics, wherein the raw materials for preparing the antibacterial and deodorizing textile fabrics include long-staple cotton, polyester, zinc nitrate hexahydrate, 2-methylimidazole, naringenin, deionized water, methanol solution, polyvinyl pyrrolidone, β-cyclodextrin, polycaprolactone, and quaternized chitosan; Step 2, the zinc nitrate hexahydrate is dissolved in the methanol solution according to a preset ratio to obtain a zinc nitrate hexahydrate methanol solution, the zinc nitrate hexahydrate methanol solution and the 2-methylimidazole are prepared into a mixed solution according to a preset ratio, and then added into a double-layer glass reactor, and stirred for 1 hour; The chemical reaction equation of the zinc nitrate hexahydrate and the 2-methylimidazole is: (1) In formula (1), is 2-methylimidazole, It is zinc nitrate hexahydrate. It is a ZIF-8 nanocarrier; Step 3, the polyvinyl pyrrolidone, the deionized water and the naringenin are added to the double-layer glass reactor according to a preset ratio, and stirred at 30° C. for 4.5 hours to prepare a PVP-naringenin methanol solution. The PVP-naringenin methanol solution and the ZIF-8 nanocarrier are prepared into a mixed solution according to a preset ratio and added to the double-layer glass reactor, and stirred for 1 hour to prepare NAR@ZIF-8. The NAR@ZIF-8 represents a ZIF-8 nanomaterial doped with naringenin. The chemical reaction equation of the PVP-naringenin methanol solution and the ZIF-8 nanomaterial is: PVP- + ZIF-8→NAR@ZIF-8 (2) In formula (2), PVP- represents PVP-naringenin methanol solution, ZIF-8 represents ZIF-8 nanomaterial; Step 4: The β-cyclodextrin is carbonized at high temperature in the reaction device to obtain GQDs, wherein the GQDs represent graphene quantum dots. The reaction time is 15 hours, the reaction temperature is 210° C., and the carbonization reaction equation of β-cyclodextrin is: →GQDs (3) In formula (3), represents β-cyclodextrin; Step 5: The polycaprolactone and the quaternized chitosan are blended in a designated reaction device by melt blending to prepare a material QCTS-PCL with antibacterial effect, wherein the QCTS-PCL represents a quaternized chitosan-polycaprolactone blend, the designated reaction device is an internal mixer, and the chemical equation for the reaction of the polycaprolactone and the quaternized chitosan is: QCTS-PCL (4) In formula (4), represents polycaprolactone, represents the degree of polymerization of polycaprolactone, represents quaternary ammonium chitosan, m represents the degree of polymerization of quaternary ammonium chitosan; Step 6: The QCTS-PCL and the GQDs are calcined at high temperature to produce quaternized chitosan-polycaprolactone loaded with graphene quantum dots, and the reaction temperature is 210° C. Step 7, the NAR@ZIF-8 and the quaternary ammonium chitosan-polycaprolactone loaded with graphene quantum dots described in step 6 are used to prepare composite nanofibers by electrospinning technology; Step 8: The polyester, the composite nanofiber, and the long-staple cotton are prepared into an antibacterial and deodorizing textile fabric by using three-dimensional textile technology; The components of the raw materials for preparation are 65 parts by weight of the long-staple cotton, 12.5 parts by weight of the polyester, 5 parts by weight of the zinc nitrate hexahydrate, 5 parts by weight of the 2-methylimidazole, 2 parts by weight of the naringenin, 3 parts by weight of the deionized water, 4 parts by weight of the methanol solution, 1.5 parts by weight of the polyvinyl pyrrolidone, 1 part by weight of the β-cyclodextrin, 0.5 parts by weight of the polycaprolactone, and 0.5 parts by weight of the quaternized chitosan.
2. The method for preparing an antibacterial and deodorizing textile fabric according to claim 1, characterized in that: The working method for preparing the composite nanofibers in step seven is: the NAR@ZIF-8 and the quaternized chitosan-polycaprolactone loaded with graphene quantum dots are mixed to prepare a spinning solution, and the spinning solution is subjected to 10KV high voltage static electricity and the fiber diameter of the fiber deposited on the receiver is controlled to be 3-30 microns by increasing the rotation speed of the wire collection drum.
3. The method for preparing an antibacterial and deodorizing textile fabric according to claim 1, characterized in that: The double-layer glass reactor comprises a motor (1), a vacuum nozzle (2), a glass condenser (3), a reflux elbow (4), a thermometer (5), a glass reactor body (6), a polytetrafluoroethylene stirring paddle (7), a discharge valve (8), a universal wheel with a brake (9), a constant pressure dropping funnel (10), a temperature display meter (11), a speed display adjustment meter (12), and a solid feeding port (13). The double-layer glass reactor comprises a control part, a feeding part, a discharging part, a stirring part, and a display part. The motor (1) constitutes the control part of the double-layer glass reactor. The motor (1) is connected to the top of the double-layer glass reactor through an electric wire. The electric wire The machine (1) adopts a low-speed booster motor and a reducer to ensure that the equipment can perform long-term stirring work. The glass kettle body (6) and the polytetrafluoroethylene stirring paddle (7) constitute the stirring part of the double-layer glass reactor. The polytetrafluoroethylene stirring paddle (7) is placed in the middle position inside the glass kettle body (6). The constant pressure dropping funnel (10), the glass condenser (3), the reflux elbow (4), and the solid feeding port (13) together constitute the feeding part of the double-layer glass reactor. The constant pressure dropping funnel (10) is placed on the left side of the motor (1). The constant pressure dropping funnel (10) is equipped with a high vacuum polytetrafluoroethylene hand valve to ensure the double-layer glass reactor. The internal pressure remains unchanged, which plays a role in preventing backflow. The glass condenser (3) is placed on the right side of the motor (1). The glass condenser (3) adopts a double-layer coiled design to increase the contact area between the glass condenser (3) and the gaseous material to improve the condensation efficiency. The vacuum nozzle (2) is placed at the upper end of the glass condenser (3) by connecting to a vacuum pump to reduce the pressure of the glass condenser (3) to accelerate the condensation speed of the glass condenser (3). The reflux elbow (4) is connected to the glass condenser (3) through a glass conduit and is placed at the lower end of the glass condenser (3) to separate the liquid. The thermometer (5) is placed at the upper end of the glass condenser (3). The edge position inside the glass kettle (6) is used to measure the temperature of the reactants in real time. The solid feeding port (13) is placed at the opening above the glass kettle (6). The temperature display meter (11) and the speed display adjustment meter (12) together constitute the display part of the double-layer glass reactor, which is connected to the left side of the constant pressure dropping funnel (10) through an internal connection. The discharge valve (8) constitutes the discharge part of the double-layer glass reactor, and is connected to the bottom of the glass kettle (6) through a detachable design to enable the discharge work of the double-layer glass reactor to be carried out thoroughly. The universal wheel with brake (9) is placed at the bottom of the stainless steel support frame.
4. The method for preparing an antibacterial and deodorizing textile fabric according to claim 1, characterized in that: The device structure used in the electrospinning technology includes a metering pump (14), a syringe (15), a high-voltage power supply (16), a capillary (17), a Taylor cone (18), and a receiver (19). The device structure used in the electrospinning technology includes a high-voltage power supply, an injection device, and a receiving device. The metering pump (14), the syringe (15), the capillary (17), and the Taylor cone (18) are connected through a hollow spiral tube to form an injection device of the electrospinning machine, which is placed on the left side of the entire electrospinning machine. The Taylor cone (18) is placed on the rightmost side of the capillary (17). The high-voltage power supply (16) is connected to the lower end of the syringe (15) through an electric wire. The receiver (19) constitutes the receiving device of the electrospinning and is placed on the rightmost side of the electrospinning machine.
5. The method for preparing an antibacterial and deodorizing textile fabric according to claim 1, characterized in that: The internal mixer reaction device in step 5 comprises: a main motor (20), a coupling (21), an accelerator (22), a tooth section (23), a speed ratio gear (24), a cylinder (25), a stuffing box (26), a flap door (27), a rotor (28), an oil pressure system (29), a heating and cooling system (30), and an internal mixer chamber (31). The main motor (20), the coupling (21), the accelerator (22), the tooth section (23), and the speed ratio gear (24) together constitute a power system of the internal mixer by means of a hollow connection and are placed on the left side of the internal mixer. The cylinder (25), the stuffing box (26), the flap door (27), the rotor (28), the oil pressure system (29), the heating and cooling system (30), and the internal mixer chamber (31) together constitute a reaction system of the internal mixer. The reaction system comprises an upper part and a lower part. The upper part of the reaction system and the lower part of the reaction system are connected by a hollow connection. The flap door (27) and the stuffing box (26) constitute the upper part of the reaction system, the cylinder (25) is embedded in the upper part of the reaction system, the rotor (28), the oil pressure system (29), the heating and cooling system (30), and the mixing chamber (31) constitute the lower part of the reaction system. When the mixing machine is working, the rotor (28) rotates relatively, clamps the material from the stuffing box (26) and brings it into the roller gap to be squeezed and sheared by the rotor (28), so that it enters the mixing chamber (31) for mixing. The oil pressure system (29) is placed outside the rotor (28) so that the upper structure of the reaction system can obtain sufficient hydraulic oil when working, and at the same time reduce the impact force generated by each component when working. The heating and cooling system (30) is placed above the mixing chamber (31) through a line connection to control the surface temperature of the inner cavity wall of the rotor (28) and the mixing chamber (31).
6. The method for preparing an antibacterial and deodorizing textile fabric according to claim 1, characterized in that: The ratio of the raw materials for preparation is preset and optimized by constructing an optimization model using the response surface method. The response surface simulation optimization model uses a multivariate regression analysis method to establish a correlation function between the ratio of the raw materials for preparing the antibacterial and deodorizing textile fabrics and the performance indicators of the antibacterial and deodorizing textile fabrics. The ratio sample set of the raw materials for preparing the antibacterial and deodorizing textile fabrics is , , the expression of the correlation function is: (5) In formula (5), is the performance index of the antibacterial and deodorizing textile fabric corresponding to the ratio of the raw materials for preparing the i-th antibacterial and deodorizing textile fabric, The proportion sample of the raw material for preparing the i-th antibacterial and deodorizing textile fabric, is the independent variable coefficient corresponding to the proportion of the raw materials for preparing the i-th antibacterial and deodorizing textile fabric, is the total number of proportion samples of the raw materials for preparing the antibacterial and deodorizing textile fabrics, i is the ordinal number of the proportion samples of the raw materials for preparing the antibacterial and deodorizing textile fabrics, is the constant term coefficient, is a random error term; based on the correlation function, the ratio of the raw materials for preparing the antibacterial and deodorizing textile fabric is iteratively optimized, and the calculation formula is: (6) In formula (6), The updated ratio of raw materials for preparing the antibacterial and deodorizing textile fabric is: The current raw material ratio for the preparation of antibacterial and deodorizing textile fabrics. and To update the acceleration coefficient, used to control the global optimal solution, , is the learning rate, which is used to control the utilization of the optimization space. The objective function is the ratio of raw materials for the current antibacterial and deodorizing textile fabrics. The gradient of the antibacterial and deodorizing textile fabric is searched for the optimal ratio of the raw materials for preparing the antibacterial and deodorizing textile fabric through iterative calculation.
7. An antibacterial and deodorizing textile fabric, characterized in that: The fabric is prepared by the method for preparing an antibacterial and deodorizing textile fabric according to any one of claims 1 to 6.
Citation Information
Patent Citations
ZIF-8 / polyvinylidene fluoride composite nanofiber membrane and preparation method and application thereof
CN108893863A
CS-ZIF-8 / PLA composite electrostatic spinning fiber membrane with rapid degradation in water, high antibacterial property and filtering efficiency
CN117306103A
Cited By
Preparation method and application of polyester staple fibers with deodorizing and antibacterial functions
CN122169234A