A method for preparing corrosion-resistant aluminum alloy profile for ships
Through surface treatment and multi-layer coating preparation technology, the anti-corrosion coating stability and physical properties of aluminum alloy profiles for ships are improved, the failure problem of existing coatings in complex environments is solved, and the corrosion resistance is achieved and self-cleaning effect.
Patent Information
- Application Number
- CN202411017147.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The overall stability of the surface anticorrosion coating of existing aluminum alloy profiles for ships is not ideal, the compatibility is poor, and it is prone to uneven coating thickness, voids, and bubble defects, and under seawater erosion, ultraviolet radiation, low temperature environment and mechanical friction Failure, physical performance and self-cleaning performance are insufficient.
After surface treatment, a modified alumina base material and functional ceramic powder are prepared, and the first coating is formed by laser cladding, and then the suspension and composite modification are prepared, and the film-forming treatment is carried out to form the second coating to improve the coating. The stability, hardness and wear resistance of the layer, and enhance corrosion resistance through the self-cleaning of the hydrophobic surface.
Form a dense and firm coating structure, improve the corrosion resistance, low temperature stability and hardness of aluminum alloy profiles, avoid coating defects, enhance resistance to seawater, ultraviolet rays and mechanical friction, and achieve overall coating stability and improve self-cleaning performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum alloy profiles, and in particular to a method for preparing a corrosion-resistant aluminum alloy profile for ships. Background Art
[0002] Aluminum alloy profiles have the characteristics of low specific gravity, good elastic modulus, good weldability, easy processing, no magnetic interference, and good low-temperature characteristics. Compared with traditional metal materials, the application of aluminum alloy profiles in shipbuilding has the following main advantages: 1) Due to the low specific gravity of aluminum alloy profiles, the weight of the hull can be reduced, the power of the power equipment can be reduced, and the navigation speed can be ensured to be stable; fuel consumption can be reduced, the economy and environmental protection of navigation can be improved; the length-to-width ratio of the ship can be improved, the stability of the ship can be increased, and the ship can be easier to operate. 2) The substrate and welded joints of aluminum alloy profiles for ships have low tendency to stress corrosion, exfoliation corrosion and intergranular corrosion in seawater or marine environments, which can save maintenance costs and extend the service life of ships. 3) Aluminum alloy profiles have good processing performance and are easy to perform cutting, punching, cold bending, rolling and other processing operations; they are conducive to the manufacture of thin-walled profiles and prefabricated parts of ships, thereby reducing the amount of welding, improving the assembly production efficiency, and reducing labor costs. 4) Aluminum alloy profiles have good welding performance and simple welding processing. The automatic argon arc welding method is used, and the welding formation is good, the cracks are few, and it is easy to correct. 5) Aluminum alloy profiles have a higher elastic modulus, a greater ability to absorb pulse voltage, and higher safety. 6) During the processing of aluminum alloy profiles, aluminum scraps are easy to recycle and can be reused, with a high material utilization rate.
[0003] However, the complex marine environment is still highly corrosive to aluminum alloy profiles for ships. Long-term exposure to corrosive environments such as seawater will easily cause erosion and damage to aluminum alloy hulls. The corrosion effects of the marine environment on aluminum alloy profiles for ships mainly include the following aspects: 1) Seawater contains a large amount of chloride ions, which can penetrate the oxide film on the surface of the aluminum alloy and enter the grain boundary of the aluminum alloy to cause local corrosion, namely pitting corrosion; pitting corrosion will cause scattered pits on the surface of aluminum alloy for ships, and gradually expand, eventually affecting the overall strength of the ship. At the same time, chloride ions will also react with the oxide film on the surface of aluminum alloy for ships to form unstable compounds, further accelerating the corrosion process. 2) There are abundant microorganisms in the marine environment, and some microorganisms can form biofilms on the surface of aluminum alloys. These biofilms can not only adsorb and aggregate other corrosive substances (such as iron oxide, sulfate, etc.), but also produce acidic metabolites by decomposing organic matter, thereby accelerating the corrosion of aluminum alloys. 3) Changes in seawater temperature have a certain effect on the mechanical properties of aluminum alloys for ships. Low-temperature or high-temperature seawater environments will reduce their overall stability and accelerate the corrosion of aluminum alloys. 4) The high salinity, high humidity and long-term sunlight exposure of the marine environment will further accelerate the corrosion of aluminum alloys by the aforementioned chloride ions, sulfur ions, etc.
[0004] In order to improve the corrosion resistance of aluminum alloys for ships in the marine environment, anti-corrosion coatings are usually prepared on the surface of aluminum alloy profiles for ships in the prior art. The anti-corrosion coatings protect and isolate the aluminum alloy profiles for ships, thereby reducing the corrosion effect of the complex marine environment on the aluminum alloys for ships.
[0005] However, the overall stability of the existing anti-corrosion coating prepared on the surface of aluminum alloy profiles for ships is not ideal, and the compatibility with the aluminum alloy profile substrate is poor. During the preparation process, defects such as uneven coating thickness, coating gaps, and bubbling are prone to occur. The weak points, gaps, or bubbles in the thickness are prone to become the starting point of corrosion, which in turn leads to the failure of the entire anti-corrosion coating. At the same time, in the actual application of aluminum alloy for ships, the anti-corrosion coating is affected by factors such as seawater scouring, ultraviolet radiation, long-term low temperature environment, and mechanical friction, and is prone to aging or damage problems, which in turn leads to the loss of the original anti-corrosion performance of the anti-corrosion coating.
[0006] Furthermore, the overall physical properties and self-cleaning performance of the existing anti-corrosion coating on the surface of aluminum alloy profiles for ships need to be further improved. Summary of the invention
[0007] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing a corrosion-resistant aluminum alloy profile for ships, which can improve the overall stability of the anti-corrosion coating on the surface of the aluminum alloy profile for ships, improve the compatibility of the anti-corrosion coating with the aluminum alloy profile substrate, and avoid the occurrence of uneven coating thickness, coating voids, and coating bubbling defects during the preparation process; improve the resistance of aluminum alloy for ships to adverse factors such as seawater scouring, ultraviolet radiation, long-term low temperature environment, mechanical friction, etc., and further improve the overall physical properties and self-cleaning performance of the anti-corrosion coating on the surface of the aluminum alloy profile for ships.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0009] A method for preparing a corrosion-resistant aluminum alloy profile for ships comprises the following steps: surface treatment, preparation of a first coating, and preparation of a second coating.
[0010] The surface treatment method comprises the following steps: using a sodium hydroxide solution with a concentration of 5-6wt% to remove the aluminum oxide film on the surface of a 5086 aluminum alloy profile; polishing with 800# sandpaper, 1000# sandpaper and 1200# sandpaper in sequence; completely immersing the aluminum alloy profile in acetone; and ultrasonically cleaning the aluminum alloy profile for 10-20min; then completely immersing the aluminum alloy profile in a sodium hydroxide solution with a concentration of 5-6wt%, heating the aluminum alloy profile to 55-65°C, taking the aluminum alloy profile out after heat preservation for 240-300s, and washing the aluminum alloy profile to neutrality with deionized water; then completely immersing the aluminum alloy profile in a nitric acid solution with a concentration of 25-28wt%, taking the aluminum alloy profile out after room temperature treatment for 20-40s, washing the aluminum alloy profile to neutrality with deionized water, and drying the aluminum alloy profile; and sandblasting the aluminum alloy profile until the surface roughness Ra of the aluminum alloy profile is 1-1.2μm to obtain the aluminum alloy profile after surface treatment.
[0011] The preparation of the first coating comprises the following steps: preparing a modified alumina base material, preparing functional ceramics, and laser cladding.
[0012] The method for preparing the modified alumina base material comprises: adding α-alumina to a nitric acid solution with a concentration of 0.3-0.35 mol / L, stirring and heating to 70-75° C., keeping the temperature and stirring for 2-3 hours, centrifuging to separate solids, washing the solids with deionized water until neutral, transferring the solids to a constant temperature drying oven, and drying at 100-110° C. to constant weight to obtain pre-modified α-alumina; then adding acrylamide and ammonium persulfate to a nitric acid solution with a concentration of 14-15wt%. In the acid aluminum solution, ultrasonically disperse for 10-15 minutes, then continue to add urea and stir for 20-30 minutes; then add pre-modified α-alumina, stir and heat to 60-65°C, keep stirring for 2-3 hours, let it stand for 30-40 minutes, centrifuge to separate the solid and transfer it to a constant temperature drying oven, dry it at 80-85°C for 40-42 hours, transfer it to a calcining furnace, keep it at 520-530°C for 3-4 hours, cool it naturally, and obtain the modified alumina base material.
[0013] In the preparation of the modified alumina base material, the particle size of α-alumina is 80-100 nm, and the specific surface area is 3-3.2 m 2 / g, pore volume is 0.7-0.8mL / g;
[0014] The weight ratio of α-alumina to nitric acid solution is 1:7-8;
[0015] The weight ratio of acrylamide, ammonium persulfate, aluminum nitrate solution, urea and pre-modified alpha-alumina is 4-4.3:1-1.2:100-105:5.5-5.8:22-24.
[0016] The method for preparing functional ceramics comprises the following steps: adding a modified alumina base material, nano-calcium fluoride, chromium oxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution into a ball mill, controlling the ball-to-material ratio to be 2-2.5:1, the ball milling speed to be 140-160 rpm, ball milling for 8-10 hours, drying and obtaining ball milled material; after uniformly mixing the ball milled material with boric acid, transferring the mixture into a calcining furnace, heating the mixture to 1400-1500° C. at a heating rate of 8-10° C. / min, calcining the mixture at the temperature for 2.5-3 hours, cooling the mixture naturally, and crushing the mixture to 12-17 μm to obtain functional ceramic powder.
[0017] In the preparation of the functional ceramic, the weight ratio of the modified alumina base material, nano-calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose, and ethanol solution is 70-73:7-8:10-11:3-3.5:0.8-1:44-46;
[0018] The volume concentration of the ethanol solution is 60-65%;
[0019] The weight ratio of the ball-milled material to the boric acid is 100:1.8-2.2.
[0020] The laser cladding method comprises the following steps: uniformly mixing aluminum silicon alloy powder and functional ceramic powder at a weight ratio of 1:2.2-2.5 to obtain coating powder; pre-placing the coating powder on the outer surface of the aluminum alloy profile after surface treatment, and controlling the thickness of the coating powder to be 1.2-1.6 mm; and performing laser cladding treatment using a cross-flow continuous CO2 laser under argon protection conditions, controlling the laser output power to be 2000-2200 W, the scanning speed to be 9-11 mm / s, and the spot diameter to be 4-5 mm; and cooling after the laser cladding treatment is completed to complete the preparation of the first coating and obtain the aluminum alloy profile with the first coating.
[0021] The preparation of the second coating comprises the following steps: preparation of a suspension, modification treatment, and film-forming treatment.
[0022] The method for preparing the suspension comprises the following steps: adding an ethanol solution with a volume concentration of 70-75%, nano silicon dioxide, nano zirconium dioxide and nano yttrium oxide into a ball mill, controlling the ball-to-material ratio to be 4.2-4.7:1, and the ball milling speed to be 80-110 rpm; after ball milling for 10-12 minutes, spraying silane coupling agent KH-602 and silane coupling agent KH-560 during the ball milling process, controlling the adding time of silane coupling agent KH-602 and silane coupling agent KH-560 to be 20-30 seconds, and after the addition of silane coupling agent KH-602 and silane coupling agent KH-560, continuing ball milling for 70-90 minutes, taking out the ball milled mixed material, drying it, and obtaining a ball milled product; adding the ball milled product and sodium dodecyl sulfate into deionized water, ultrasonically treating it for 10-20 minutes, and stirring it for 30-40 minutes to obtain a suspension.
[0023] In the preparation of the suspension, the weight ratio of the ethanol solution, nano silicon dioxide, nano zirconium dioxide, nano yttrium oxide, silane coupling agent KH-602, and silane coupling agent KH-560 is 5-5.8:6-7:3-3.5:1-1.2:0.9-1.1:0.4-0.5;
[0024] The weight ratio of the ball-milled product, sodium dodecyl sulfate and deionized water is 5-6:0.6-0.7:110-120.
[0025] The modification method comprises the following steps: adding carboxymethyl chitosan into a suspension, ultrasonically treating the suspension for 40-50 minutes, adding hexadecyltrimethylammonium bromide under stirring, stirring the suspension at room temperature for 30-40 minutes, and then standing the suspension for 2-3 hours; adding L-ascorbic acid, stirring the suspension and heating the suspension to 40-45° C., keeping the temperature for 22-24 hours, separating and obtaining a solid, washing the solid with 4-5 times the volume of deionized water, and drying the solid at 65-70° C. for 10-12 hours in a vacuum environment of 0.07-0.08 MPa to obtain a composite modified product.
[0026] In the modification treatment, the weight ratio of carboxymethyl chitosan, suspension, hexadecyltrimethylammonium bromide and L-ascorbic acid is 1-1.1:110-120:0.2-0.3:0.55-0.65.
[0027] The film-forming treatment method comprises the following steps: putting silane coupling agent Si-69, silane coupling agent A-163 and a composite modifier into an ethanol solution with a volume concentration of 50-60%, ultrasonically dispersing for 15-20 minutes, adding acetic acid dropwise under stirring to adjust the pH value to 4-5, stirring and heating to 40-42° C., and keeping the temperature and stirring for 7-8 hours to obtain a film-forming solution; completely immersing the aluminum alloy profile with the first coating into 1.5-2 times the volume of the film-forming solution, immersing for 30-40 minutes, pulling out the aluminum alloy profile, heating to 80-85° C. at a heating rate of 1-1.5° C. / min, and keeping the temperature for heat treatment for 40-60 minutes; heating to 125-135° C. at a heating rate of 3.5-4° C. / min, and keeping the temperature for heat treatment for 1-1.5 hours to complete the self-assembly preparation of the second coating, and obtain a corrosion-resistant aluminum alloy profile for ships.
[0028] In the film forming process, the weight ratio of silane coupling agent Si-69, silane coupling agent A-163, composite modified substance and ethanol solution is 2.5-3:1.5-1.7:2.2-2.5:100.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The method for preparing a corrosion-resistant aluminum alloy profile for ships of the present invention comprises the following steps: after surface treatment of the aluminum alloy profile, in the preparation of a modified alumina base material for preparing a first coating, α-alumina is first treated with nitric acid to improve its bonding performance with subsequent reinforcing components (acrylamide, aluminum nitrate, etc.) while maintaining the physical properties of α-alumina. Then, macroporous alumina is in-situ grown on the surface of the pre-modified α-alumina to obtain a modified alumina base material. The porous structure and large surface area of the modified alumina base material are used to improve its bonding performance with functional ceramics. The bonding performance of the enhanced phase components (nano-calcium fluoride, chromium trioxide, lanthanum oxide, etc.) is enhanced to produce functional ceramic powder; the functional ceramic powder is clad with aluminum silicon alloy powder, and the modified alumina base material is used as the hard phase. The functional ceramic powder produced by combining with nano-calcium fluoride, chromium trioxide, lanthanum oxide, etc. can reduce coating defects and porosity, enhance the bonding performance between the first coating and the aluminum alloy profile substrate, improve the stability of the coating, form a denser and firmer coating structure, improve the hardness and wear resistance of the coating, and improve the low-temperature stability of the coating. In the step of preparing the suspension of the second coating, a bisaminosilane coupling agent and an epoxysilane coupling agent are firstly used to carry out surface synergistic modification and composite treatment on nano silicon dioxide, nano zirconium dioxide and nano yttrium oxide, so as to improve the composite performance of the effective components in the suspension and their reactivity with chitosan; then carboxymethyl chitosan and hexadecyltrimethylammonium bromide are used for modification treatment to obtain a composite modified product; the composite modified product is combined with silane coupling agent Si-69 and silane coupling agent A-163 on the surface of the first coating of the aluminum alloy profile for coating. The second coating is self-assembled, and the composite modifier is evenly distributed in the self-assembled coating (i.e., the second coating) to form a dense protective film layer, which effectively blocks the penetration of water and corrosive media in seawater, and improves the hydrophobicity, corrosion resistance, low-temperature stability, hardness and wear resistance of the aluminum alloy profile; through the barrier effect of the air film on the hydrophobic surface of the surface film layer, the contact between the aluminum alloy profile and the seawater environment is reduced. When the corrosive medium is attached to the outer surface of the aluminum alloy profile, the corrosive medium is removed under the condition of water flow scouring through the hydrophobic self-cleaning effect of the film layer. Through the synergistic effect of the above-mentioned technical means, the overall stability of the anti-corrosion coating on the surface of the aluminum alloy profile for ships can be improved, the compatibility of the anti-corrosion coating with the aluminum alloy profile substrate can be improved, and the uneven coating thickness, coating gaps, and coating bubbling defects in the preparation process can be avoided; the resistance of aluminum alloy for ships to adverse factors such as seawater scouring, ultraviolet radiation, long-term low temperature environment, mechanical friction, etc. can be improved, and the overall physical properties and self-cleaning properties of the anti-corrosion coating on the surface of aluminum alloy profiles for ships can be further improved.
[0031] (2) The method for preparing the corrosion-resistant aluminum alloy profile for ships of the present invention has a coating free of voids and blister defects, a coating thickness deviation rate of 0.94-0.97%, a coating hardness of 1006-1017 HV, a coating adhesion grade of 0, a water droplet contact angle on the coating of 99-101°, and a water droplet complete freezing time of 36.9-37.2 min.
[0032] (3) The method for preparing the corrosion-resistant aluminum alloy profile for ships of the present invention has a corrosion potential of -0.491V to -0.483V and a corrosion current density of (0.391-0.401)×10 -8 A.cm 2 ; After the cross-cut test of the coating adhesion level, the corrosion potential degradation rate was 0.04-0.05%.
[0033] (4) The method for preparing the corrosion-resistant aluminum alloy profile for ships of the present invention, after the friction treatment, the corrosion-resistant aluminum alloy profile for ships has no delamination, separation, crack defects under the conditions of 60 consecutive cycles of low-temperature salt water immersion, direct ultraviolet irradiation and xenon lamp simulated sunlight, and the corrosion potential is -0.511V to -0.501V, and the corrosion current density is (0.405-0.419)×10 -8 A.cm 2 , the coating adhesion grade is 0, and the contact angle of water droplets on the coating is 94-96°. DETAILED DESCRIPTION
[0034] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0035] Example 1
[0036] A method for preparing a corrosion-resistant aluminum alloy profile for ships, specifically comprising:
[0037] 1. Surface treatment
[0038] A 5wt% sodium hydroxide solution was used to remove the aluminum oxide film on the surface of the 5086 aluminum alloy profile. After being polished with 800# sandpaper, 1000# sandpaper and 1200# sandpaper in sequence, the profile was completely immersed in acetone and ultrasonically cleaned for 10 minutes. The aluminum alloy profile was then completely immersed in a 5wt% sodium hydroxide solution, heated to 55°C, and taken out after heat preservation for 240s. It was washed with deionized water until neutral, and then completely immersed in a 25wt% nitric acid solution. After treatment at room temperature for 20s, it was taken out, washed with deionized water until neutral, and dried. The aluminum alloy profile was sandblasted until the surface roughness Ra of the aluminum alloy profile was 1μm, and the surface-treated aluminum alloy profile was obtained.
[0039] 2. Preparation of the first coating
[0040] 1) Preparation of modified alumina base material
[0041] α-alumina was put into a nitric acid solution with a concentration of 0.3 mol / L, stirred and heated to 70°C, kept warm and stirred for 2 hours, and then the solid was separated by centrifugation. The solid was washed with deionized water until neutral, and then transferred to a constant temperature drying oven, and dried at 100°C to constant weight to obtain pre-modified α-alumina; then acrylamide and ammonium persulfate were put into an aluminum nitrate solution with a concentration of 14wt%, and after ultrasonic dispersion for 10 minutes, urea was continued to be added and stirred for 20 minutes; then the pre-modified α-alumina was added, stirred and heated to 60°C, kept warm and stirred for 2 hours, and then allowed to stand for 30 minutes, the solid was separated by centrifugation and transferred to a constant temperature drying oven, dried at 80°C for 40 hours, and then transferred to a roasting furnace, kept warm and roasted at 520°C for 3 hours, and naturally cooled to obtain a modified alumina base material.
[0042] Among them, the particle size of α-alumina is 80nm and the specific surface area is 3.1m 2 / g, and the pore volume is 0.73mL / g.
[0043] The weight ratio of α-alumina to the nitric acid solution is 1:7.
[0044] The weight ratio of acrylamide, ammonium persulfate, aluminum nitrate solution, urea, and pre-modified α-alumina is 4:1:100:5.5:22.
[0045] 2) Preparation of functional ceramics
[0046] Put modified alumina base material, nano-calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution into a ball mill, control the ball-to-material ratio to 2:1, the ball mill speed to 140rpm, ball milling for 8 hours, dry to obtain ball-milled material; after mixing the ball-milled material with boric acid evenly, transfer it into a calcining furnace, heat it to 1400℃ at a heating rate of 8℃ / min, calcine it for 2.5 hours, cool it naturally, and grind it to 12μm to obtain functional ceramic powder.
[0047] Among them, the weight ratio of modified alumina base material, nano calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution is 70:7:10:3:0.8:44.
[0048] The volume concentration of the ethanol solution is 60%.
[0049] The weight ratio of the ball-milled material to the boric acid was 100:1.8.
[0050] 3) Laser cladding
[0051] Aluminum silicon alloy powder and functional ceramic powder are uniformly mixed in a weight ratio of 1:2.2 to obtain coating powder; the coating powder is pre-placed on the outer surface of the aluminum alloy profile after surface treatment, and the thickness of the coating powder is controlled to be 1.2mm, and under argon protection conditions, a cross-flow continuous CO2 laser is used for laser cladding treatment, and the laser output power is controlled to be 2000W, the scanning speed is 9mm / s, and the spot diameter is 4mm; after the laser cladding treatment is completed, it is cooled to complete the preparation of the first coating, and the aluminum alloy profile with the first coating is obtained.
[0052] 3. Preparation of the second coating
[0053] 1) Preparation of suspension
[0054] Put 70% volume concentration of ethanol solution, nano silicon dioxide, nano zirconium dioxide, nano yttrium oxide into a ball mill, control the ball-to-material ratio to 4.2:1, the ball milling speed to 80rpm, after ball milling for 10min, spray silane coupling agent KH-602 and silane coupling agent KH-560 during the ball milling process, control the addition time of silane coupling agent KH-602 and silane coupling agent KH-560 to 20s, after the addition of silane coupling agent KH-602 and silane coupling agent KH-560, continue ball milling for 70min, take out the ball milled mixed material, dry it, and obtain the ball milled material; put the ball milled material and sodium dodecyl sulfate into deionized water, ultrasonically treat for 10min, and stir for 30min to obtain a suspension.
[0055] Among them, the weight ratio of ethanol solution, nano silicon dioxide, nano zirconium dioxide, nano yttrium oxide, silane coupling agent KH-602 and silane coupling agent KH-560 is 5:6:3:1:0.9:0.4.
[0056] The weight ratio of the ball-milled product, sodium dodecyl sulfate, and deionized water is 5:0.6:110.
[0057] 2) Modification treatment
[0058] Carboxymethyl chitosan was added to the suspension, and after ultrasonic treatment for 40 minutes, hexadecyltrimethylammonium bromide was continuously added under stirring conditions, and the mixture was stirred at room temperature for 30 minutes and allowed to stand for 2 hours; L-ascorbic acid was continuously added, and the mixture was stirred and heated to 40°C, and kept warm for 22 hours to separate and obtain a solid. The solid was washed with 4 times the volume of deionized water, and dried at 65°C for 10 hours in a vacuum environment of 0.07 MPa to obtain a composite modified product.
[0059] Wherein, the weight ratio of carboxymethyl chitosan, suspension, hexadecyltrimethylammonium bromide and L-ascorbic acid is 1:110:0.2:0.55.
[0060] 3) Film forming treatment
[0061] Silane coupling agent Si-69, silane coupling agent A-163 and composite modifier were put into 50% volume concentration ethanol solution, ultrasonically dispersed for 15 minutes, and then acetic acid was added dropwise under stirring to adjust the pH to 4, and then the solution was heated to 40°C with stirring and kept stirring for 7 hours to obtain a film-forming solution; the aluminum alloy profile with the first coating was completely immersed in 1.5 times the volume of the film-forming solution, and after immersion for 30 minutes, the aluminum alloy profile was pulled out, and the temperature was increased to 80°C at a heating rate of 1°C / min, and the solution was kept warm for 40 minutes; the temperature was increased to 125°C at a heating rate of 3.5°C / min, and the solution was kept warm for 1 hour to complete the self-assembly preparation of the second coating, and a corrosion-resistant aluminum alloy profile for ships was obtained.
[0062] Wherein, the weight ratio of silane coupling agent Si-69, silane coupling agent A-163, composite modified product and ethanol solution is 2.5:1.5:2.2:100.
[0063] Example 2
[0064] A method for preparing a corrosion-resistant aluminum alloy profile for ships, specifically comprising:
[0065] 1. Surface treatment
[0066] A 5.5wt% sodium hydroxide solution was used to remove the aluminum oxide film on the surface of the 5086 aluminum alloy profile. After being polished with 800# sandpaper, 1000# sandpaper, and 1200# sandpaper in sequence, the profile was completely immersed in acetone and ultrasonically cleaned for 15 minutes. The aluminum alloy profile was then completely immersed in a 5.5wt% sodium hydroxide solution, heated to 60°C, and taken out after heat preservation for 270s. It was washed with deionized water until neutral, and then completely immersed in a 26.5wt% nitric acid solution. After treatment at room temperature for 30s, it was taken out, washed with deionized water until neutral, and dried. The aluminum alloy profile was sandblasted until the surface roughness Ra of the aluminum alloy profile was 1.1μm, and the surface-treated aluminum alloy profile was obtained.
[0067] 2. Preparation of the first coating
[0068] 1) Preparation of modified alumina base material
[0069] α-alumina was put into a nitric acid solution with a concentration of 0.32 mol / L, stirred and heated to 72°C, kept warm and stirred for 2.5 hours, and then the solid was separated by centrifugation. The solid was washed with deionized water until neutral, and then transferred to a constant temperature drying oven, and dried to constant weight at 105°C to obtain pre-modified α-alumina; then acrylamide and ammonium persulfate were put into an aluminum nitrate solution with a concentration of 14.5wt%, and after ultrasonic dispersion for 12 minutes, urea was continued to be added and stirred for 25 minutes; then the pre-modified α-alumina was added, stirred and heated to 62°C, kept warm and stirred for 2.5 hours, and then allowed to stand for 35 minutes, the solid was separated by centrifugation and transferred to a constant temperature drying oven, dried at 82°C for 41 hours, and then transferred to a roasting furnace, kept warm and roasted at 525°C for 3.5 hours, and naturally cooled to obtain a modified alumina base material.
[0070] Among them, the particle size of α-alumina is 80nm and the specific surface area is 3.1m 2 / g, and the pore volume is 0.73mL / g.
[0071] The weight ratio of α-alumina to nitric acid solution is 1:7.5.
[0072] The weight ratio of acrylamide, ammonium persulfate, aluminum nitrate solution, urea, and pre-modified α-alumina is 4.2:1.1:102:5.7:23.
[0073] 2) Preparation of functional ceramics
[0074] Put modified alumina base material, nano-calcium fluoride, chromium oxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution into a ball mill, control the ball-to-material ratio to 2.3:1, the ball mill speed to 150rpm, ball milling for 9 hours, dry to obtain ball-milled material; after mixing the ball-milled material with boric acid evenly, transfer it to a calcining furnace, heat it to 1450℃ at a heating rate of 9.2℃ / min, calcine it at this temperature for 2.8 hours, cool it naturally, and grind it to 15μm to obtain functional ceramic powder.
[0075] Among them, the weight ratio of modified alumina base material, nano calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution is 72:7.5:10.5:3.2:0.9:45.
[0076] The volume concentration of the ethanol solution is 62%.
[0077] The weight ratio of the ball-milled material to the boric acid was 100:1.9.
[0078] 3) Laser cladding
[0079] Aluminum silicon alloy powder and functional ceramic powder are uniformly mixed in a weight ratio of 1:2.3 to obtain coating powder; the coating powder is pre-placed on the outer surface of the aluminum alloy profile after surface treatment, and the thickness of the coating powder is controlled to be 1.4mm, and under argon protection conditions, a cross-flow continuous CO2 laser is used for laser cladding treatment, and the laser output power is controlled to be 2100W, the scanning speed is 9.5mm / s, and the spot diameter is 4.5mm; after the laser cladding treatment is completed, it is cooled to complete the preparation of the first coating, and the aluminum alloy profile with the first coating is obtained.
[0080] 3. Preparation of the second coating
[0081] 1) Preparation of suspension
[0082] Put an ethanol solution with a volume concentration of 72%, nano silicon dioxide, nano zirconium dioxide, and nano yttrium oxide into a ball mill, control the ball-to-material ratio to 4.5:1, and the ball milling speed to 100 rpm. After ball milling for 11 minutes, spray silane coupling agent KH-602 and silane coupling agent KH-560 during the ball milling process, and control the addition time of silane coupling agent KH-602 and silane coupling agent KH-560 to be 25 seconds. After the addition of silane coupling agent KH-602 and silane coupling agent KH-560, continue ball milling for 80 minutes, take out the ball-milled mixed material, dry it, and obtain a ball-milled product; put the ball-milled product and sodium dodecyl sulfate into deionized water, ultrasonically treat it for 15 minutes, and stir it for 35 minutes to obtain a suspension.
[0083] Among them, the weight ratio of ethanol solution, nano silicon dioxide, nano zirconium dioxide, nano yttrium oxide, silane coupling agent KH-602 and silane coupling agent KH-560 is 5.6:6.5:3.3:1.1:1:0.48.
[0084] The weight ratio of the ball-milled product, sodium dodecyl sulfate, and deionized water is 5.7:0.65:115.
[0085] 2) Modification treatment
[0086] Carboxymethyl chitosan was added to the suspension, and after ultrasonic treatment for 45 minutes, hexadecyltrimethylammonium bromide was continued to be added under stirring conditions. After stirring at room temperature for 35 minutes, it was allowed to stand for 2.5 hours; L-ascorbic acid was continued to be added, and the temperature was raised to 42°C with stirring, and kept warm for 23 hours. The solid was separated and washed with 4.5 times the volume of deionized water, and dried at 68°C for 11 hours in a vacuum environment with a degree of vacuum of 0.075 MPa to obtain a composite modified product.
[0087] Wherein, the weight ratio of carboxymethyl chitosan, suspension, hexadecyltrimethylammonium bromide and L-ascorbic acid is 1.06:115:0.25:0.6.
[0088] 3) Film forming treatment
[0089] Silane coupling agent Si-69, silane coupling agent A-163 and composite modifier were put into ethanol solution with volume concentration of 55%, and ultrasonically dispersed for 18 minutes. Then, acetic acid was added dropwise under stirring to adjust the pH to 4.5, and the mixture was heated to 41°C with stirring and kept stirring for 7.5 hours to obtain a film-forming solution. The aluminum alloy profile with the first coating was completely immersed in 1.8 times the volume of the film-forming solution. After immersion for 35 minutes, the aluminum alloy profile was pulled out and heated to 82°C at a heating rate of 1.2°C / min, and kept heat-treated for 50 minutes; the temperature was increased to 130°C at a heating rate of 3.7°C / min, and kept heat-treated for 1.3 hours to complete the self-assembly preparation of the second coating, and a corrosion-resistant aluminum alloy profile for ships was obtained.
[0090] Wherein, the weight ratio of silane coupling agent Si-69, silane coupling agent A-163, composite modified product and ethanol solution is 2.8:1.6:2.3:100.
[0091] Example 3
[0092] A method for preparing a corrosion-resistant aluminum alloy profile for ships, specifically comprising:
[0093] 1. Surface treatment
[0094] A 6wt% sodium hydroxide solution was used to remove the aluminum oxide film on the surface of the 5086 aluminum alloy profile. After being polished with 800# sandpaper, 1000# sandpaper and 1200# sandpaper in sequence, the profile was completely immersed in acetone and ultrasonically cleaned for 20 minutes. The aluminum alloy profile was then completely immersed in a 6wt% sodium hydroxide solution, heated to 65°C, and taken out after heat treatment for 300s. It was washed with deionized water until neutral, and then completely immersed in a 28wt% nitric acid solution. After treatment at room temperature for 40s, it was taken out, washed with deionized water until neutral, and dried. The aluminum alloy profile was sandblasted until the surface roughness Ra of the aluminum alloy profile was 1.2μm, and the surface-treated aluminum alloy profile was obtained.
[0095] 2. Preparation of the first coating
[0096] 1) Preparation of modified alumina base material
[0097] α-alumina was put into a nitric acid solution with a concentration of 0.35 mol / L, stirred and heated to 75°C, kept warm and stirred for 3 hours, and then the solid was separated by centrifugation. The solid was washed with deionized water until neutral, and then transferred to a constant temperature drying oven, and dried at 110°C to constant weight to obtain pre-modified α-alumina; then acrylamide and ammonium persulfate were put into an aluminum nitrate solution with a concentration of 15wt%, and after ultrasonic dispersion for 15 minutes, urea was continued to be added and stirred for 30 minutes; then the pre-modified α-alumina was added, stirred and heated to 65°C, kept warm and stirred for 3 hours, and then allowed to stand for 40 minutes, the solid was separated by centrifugation and transferred to a constant temperature drying oven, dried at 85°C for 42 hours, and then transferred to a roasting furnace, kept warm and roasted at 530°C for 4 hours, and naturally cooled to obtain a modified alumina base material.
[0098] Among them, the particle size of α-alumina is 80nm and the specific surface area is 3.1m 2 / g, and the pore volume is 0.73mL / g.
[0099] The weight ratio of α-alumina to the nitric acid solution is 1:8.
[0100] The weight ratio of acrylamide, ammonium persulfate, aluminum nitrate solution, urea, and pre-modified α-alumina is 4.3:1.2:105:5.8:24.
[0101] 2) Preparation of functional ceramics
[0102] Put modified alumina base material, nano-calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution into a ball mill, control the ball-to-material ratio to 2.5:1, the ball milling speed to 160rpm, ball milling for 10 hours, and drying to obtain ball-milled material; after mixing the ball-milled material with boric acid evenly, transfer it into a calcining furnace, heat it to 1500℃ at a heating rate of 10℃ / min, calcine it for 3 hours, cool it naturally, and grind it to 17μm to obtain functional ceramic powder.
[0103] Among them, the weight ratio of modified alumina base material, nano calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution is 73:8:11:3.5:1:46.
[0104] The volume concentration of the ethanol solution is 65%.
[0105] The weight ratio of the ball-milled material to the boric acid was 100:2.2.
[0106] 3) Laser cladding
[0107] Aluminum silicon alloy powder and functional ceramic powder are uniformly mixed in a weight ratio of 1:2.5 to obtain coating powder; the coating powder is pre-placed on the outer surface of the aluminum alloy profile after surface treatment, and the thickness of the coating powder is controlled to be 1.6mm, and under argon protection conditions, a cross-flow continuous CO2 laser is used for laser cladding treatment, and the laser output power is controlled to be 2200W, the scanning speed is 11mm / s, and the spot diameter is 5mm; after the laser cladding treatment is completed, it is cooled to complete the preparation of the first coating, and the aluminum alloy profile with the first coating is obtained.
[0108] 3. Preparation of the second coating
[0109] 1) Preparation of suspension
[0110] Put an ethanol solution with a volume concentration of 75%, nano-silicon dioxide, nano-zirconium dioxide, and nano-yttrium oxide into a ball mill, control the ball-to-material ratio to 4.7:1, and the ball milling speed to 110rpm. After ball milling for 12 minutes, spray silane coupling agent KH-602 and silane coupling agent KH-560 during the ball milling process, and control the addition time of silane coupling agent KH-602 and silane coupling agent KH-560 to be 30s. After the addition of silane coupling agent KH-602 and silane coupling agent KH-560, continue ball milling for 90 minutes, take out the ball-milled mixed material, dry it, and obtain a ball-milled product; put the ball-milled product and sodium dodecyl sulfate into deionized water, ultrasonically treat it for 20 minutes, and stir it for 40 minutes to obtain a suspension.
[0111] Among them, the weight ratio of ethanol solution, nano silicon dioxide, nano zirconium dioxide, nano yttrium oxide, silane coupling agent KH-602 and silane coupling agent KH-560 is 5.8:7:3.5:1.2:1.1:0.5.
[0112] The weight ratio of the ball-milled product, sodium dodecyl sulfate, and deionized water is 6:0.7:120.
[0113] 2) Modification treatment
[0114] Carboxymethyl chitosan was added to the suspension, and after ultrasonic treatment for 50 minutes, hexadecyltrimethylammonium bromide was added under stirring, and the mixture was stirred at room temperature for 40 minutes and allowed to stand for 3 hours; L-ascorbic acid was added, and the mixture was heated to 45°C with stirring and kept warm for 24 hours to separate the solid. The solid was washed with 5 times the volume of deionized water and dried at 70°C for 12 hours in a vacuum environment of 0.08 MPa to obtain a composite modified product.
[0115] Wherein, the weight ratio of carboxymethyl chitosan, suspension, hexadecyltrimethylammonium bromide and L-ascorbic acid is 1.1:120:0.3:0.65.
[0116] 3) Film forming treatment
[0117] Silane coupling agent Si-69, silane coupling agent A-163 and composite modifier were put into 60% ethanol solution by volume, and ultrasonically dispersed for 20 minutes. Then, acetic acid was added dropwise under stirring to adjust the pH to 5, and the mixture was heated to 42°C with stirring and kept stirred for 8 hours to obtain a film-forming solution. The aluminum alloy profile with the first coating was completely immersed in 2 times the volume of the film-forming solution. After immersion for 40 minutes, the aluminum alloy profile was pulled out, heated to 85°C at a heating rate of 1.5°C / min, and kept heat treated for 60 minutes; then heated to 135°C at a heating rate of 4°C / min, and kept heat treated for 1.5 hours to complete the self-assembly preparation of the second coating, and a corrosion-resistant aluminum alloy profile for ships was obtained.
[0118] Wherein, the weight ratio of silane coupling agent Si-69, silane coupling agent A-163, composite modified product and ethanol solution is 3:1.7:2.5:100.
[0119] Comparative Example 1
[0120] The technical solution of Example 2 is adopted, but the differences are as follows: 1) in the preparation of the first coating, the step of preparing the modified alumina base material is omitted, and α-alumina is used directly in the subsequent step of preparing functional ceramics instead of the modified alumina base material; 2) in the step of preparing functional ceramics in the preparation of the first coating, the addition of nano-calcium fluoride and chromium oxide is omitted.
[0121] Comparative Example 2
[0122] The technical solution of Example 2 is adopted, but the differences are: 1) in the preparation of the second coating, the suspension preparation step and the modification treatment step are omitted, and nano-silicon dioxide is used instead of the composite modifier for the subsequent film-forming treatment step; 2) in the film-forming treatment step of preparing the second coating, the silane coupling agent A-163 is omitted.
[0123] The preparation methods of the corrosion-resistant aluminum alloy profiles for ships of Examples 1-3 and Comparative Examples 1-2 were used to prepare the corrosion-resistant aluminum alloy profiles for ships, and the coatings of the obtained aluminum alloy profiles were observed and recorded to see whether there were voids and blister defects; and a thickness gauge was used to randomly select 10 points within the coating range of the corrosion-resistant aluminum alloy profiles for ships of 30 cm × 30 cm to detect the coating thickness, and after calculating the average coating thickness, the coating thickness deviation rate of each point compared to the average coating thickness was calculated, and the maximum value was taken. The coating thickness deviation rate was calculated as [(|coating thickness at a certain point - average coating thickness|) / average coating thickness] × 100%.
[0124] Furthermore, an electrochemical workstation was used to detect the corrosion potential and corrosion current density of each aluminum alloy profile in a 3.5wt% sodium chloride solution through a three-electrode system consisting of a working electrode, an auxiliary electrode, and a reference electrode. Among them, each aluminum alloy profile was used as a working electrode, a platinum electrode was used as an auxiliary electrode, and a saturated calomel electrode was used as a reference electrode.
[0125] Furthermore, a Vickers hardness tester was used to test the coating thickness of each aluminum alloy profile. The specific test method refers to GB / T7997-2014.
[0126] Furthermore, the adhesion level of the surface coating of the aluminum alloy profile specimen is tested by the cross-cut method, and the specific test method refers to ISO 2409-2020; at the same time, before and after the cross-cut test, the corrosion potential of the aluminum alloy profile specimen is detected by the aforementioned method, and the corrosion potential degradation rate is calculated. Specifically, the calculation method of the corrosion potential degradation rate is: [(corrosion potential after cross-cutting - corrosion potential before cross-cutting) / corrosion potential before cross-cutting] × 100%, taking the absolute value.
[0127] Furthermore, a contact angle meter was used to measure the contact angle of a drop of water (volume 5 μL) on the outer surface of each aluminum alloy profile. At the same time, at a temperature of -5°C, the complete freezing time of the water drop on the outer surface of each aluminum alloy profile was observed and recorded.
[0128] The specific results are shown in the following table:
[0129]
[0130] Furthermore, in order to test the overall stability of the coating of the corrosion-resistant aluminum alloy profile for ships, as well as the resistance to adverse factors such as seawater scouring, ultraviolet radiation, low temperature environment, and mechanical friction, the aluminum alloy profiles of Examples 1-3 and Comparative Examples 1-2 were subjected to friction treatment using a friction loss tester, respectively. The friction environment temperature was 25°C, the relative humidity was 60%, and quenched 45# steel was used as the dry friction material. The friction speed was controlled to be 100rpm, the normal load was 200N, and the friction treatment time was 15min. After the friction was completed, half of the volume of each aluminum alloy profile was immersed in a sodium chloride solution (concentration of 4.5wt%) at a temperature of -1°C, and half of the coating on the surface of the aluminum alloy profile was kept immersed in the sodium chloride solution. Half of the coating was exposed to the air, and sodium chloride solution was continuously sprayed on the half of the coating exposed to the air. At the same time, a 1200W ultraviolet lamp was used to continuously irradiate the surface coating of the corrosion-resistant aluminum alloy profile for ships. After immersion-ultraviolet irradiation for 14 hours, the aluminum alloy profile was taken out and placed in a -30℃ environment. A 1000W xenon lamp was used to continuously irradiate the surface coating of the corrosion-resistant aluminum alloy profile for ships for 10 hours; the aforementioned immersion-ultraviolet irradiation and low-temperature xenon lamp irradiation operation was regarded as one treatment (a total of 24 hours). After 60 times of treatment, the surface coating of the aluminum alloy profile was observed and recorded for delamination, detachment, and crack defects, and the aforementioned method was used to detect the corrosion potential, corrosion current density, coating adhesion grade, and contact angle of the aluminum alloy profile. The specific results are shown in the following table:
[0131]
[0132] It can be seen that the method for preparing the corrosion-resistant aluminum alloy profile for ships of the present invention is to treat the aluminum alloy profile on the surface, and then in the preparation of the modified alumina base material for preparing the first coating, firstly treat the α-alumina with nitric acid, while maintaining the physical properties of the α-alumina, improve its bonding performance with subsequent reinforcing components (acrylamide, aluminum nitrate, etc.), and then in-situ grow macroporous alumina on the surface of the pre-modified α-alumina to prepare the modified alumina base material, and improve its bonding performance with the functional ceramics through the porous structure and large surface area of the modified alumina base material. The functional ceramic powder is prepared by combining the ceramic reinforcing phase components (nano-calcium fluoride, chromium trioxide, lanthanum oxide, etc.); the functional ceramic powder is clad with aluminum silicon alloy powder, and the modified alumina base material is used as the hard phase. The functional ceramic powder prepared by combining with nano-calcium fluoride, chromium trioxide, lanthanum oxide, etc. can reduce coating defects and porosity, enhance the bonding performance between the first coating and the aluminum alloy profile substrate, improve the stability of the coating, form a denser and firmer coating structure, improve the hardness and wear resistance of the coating, and improve the low-temperature stability of the coating. In the step of preparing the suspension of the second coating, a bisaminosilane coupling agent and an epoxysilane coupling agent are firstly used to carry out surface synergistic modification and composite treatment on nano silicon dioxide, nano zirconium dioxide and nano yttrium oxide, so as to improve the composite performance of the effective components in the suspension and their reactivity with chitosan; then carboxymethyl chitosan and hexadecyltrimethylammonium bromide are used for modification treatment to obtain a composite modified product; the composite modified product is combined with silane coupling agent Si-69 and silane coupling agent A-163 on the surface of the first coating of the aluminum alloy profile for coating. The second coating is self-assembled, and the composite modifier is evenly distributed in the self-assembled coating (i.e., the second coating) to form a dense protective film layer, which effectively blocks the penetration of water and corrosive media in seawater, and improves the hydrophobicity, corrosion resistance, low-temperature stability, hardness and wear resistance of the aluminum alloy profile; through the barrier effect of the air film on the hydrophobic surface of the surface film layer, the contact between the aluminum alloy profile and the seawater environment is reduced. When the corrosive medium is attached to the outer surface of the aluminum alloy profile, the corrosive medium is removed under the condition of water flow scouring through the hydrophobic self-cleaning effect of the film layer. Through the synergistic effect of the above-mentioned technical means, the overall stability of the anti-corrosion coating on the surface of the aluminum alloy profile for ships can be improved, the compatibility of the anti-corrosion coating with the aluminum alloy profile substrate can be improved, and the uneven coating thickness, coating gaps, and coating bubbling defects in the preparation process can be avoided; the resistance of aluminum alloy for ships to adverse factors such as seawater scouring, ultraviolet radiation, long-term low temperature environment, mechanical friction, etc. can be improved, and the overall physical properties and self-cleaning properties of the anti-corrosion coating on the surface of aluminum alloy profiles for ships can be further improved.
[0133] It can be seen from Comparative Example 1 that the step of preparing the modified alumina base material is omitted in the preparation of the first coating, and the addition of nano-calcium fluoride and chromium trioxide is omitted in the step of preparing the functional ceramics. The synergistic effect of the modified alumina base material and the functional ceramic reinforcing phase components (nano-calcium fluoride, chromium trioxide, lanthanum oxide, etc.) cannot be used to reduce coating defects and pores, and the bonding performance between the coating and the aluminum alloy profile substrate cannot be further enhanced. The overall stability of the coating is reduced, and the hardness, wear resistance and low-temperature stability of the coating cannot be effectively improved. Specifically, the coating has voids and blister defects, the uniformity of the coating thickness is reduced, and its corrosion resistance, hardness, and coating adhesion grade are all significantly deteriorated. At the same time, after the aluminum alloy is subjected to friction treatment, under the conditions of continuous circulation of low-temperature salt water immersion, direct ultraviolet radiation and simulated direct sunlight, the film layer of the aluminum alloy profile has delamination, detachment, and crack defects, and the corrosion potential and corrosion current density are significantly deteriorated.
[0134] It can be seen from Comparative Example 2 that the steps of preparing the suspension and the modification treatment are omitted in the preparation of the second coating, and the addition of the silane coupling agent A-163 in the film-forming treatment is omitted. The distribution of the effective components in the composite modifier in the self-assembled coating and the synergistic enhancement effect cannot block the penetration of water and corrosive media in seawater, and the hydrophobicity, corrosion resistance, low-temperature stability, hardness and wear resistance of the aluminum alloy profile cannot be further improved, and the hydrophobic self-cleaning of the aluminum alloy profile cannot be effectively achieved. Specifically, the corrosion potential, corrosion current density and hardness of the film layer deteriorate to a certain extent, and the contact angle and the time for the water droplet to completely freeze deteriorate significantly.
[0135] Unless otherwise specified, all percentages used in the present invention are by mass.
[0136] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a corrosion-resistant aluminum alloy profile for ships, characterized in that: The method comprises the following steps: surface treatment, preparation of a first coating, and preparation of a second coating; The preparation of the first coating comprises the following steps: preparing a modified alumina base material, preparing functional ceramics, and laser cladding; The method for preparing the modified alumina base material is as follows: immersing α-alumina in a nitric acid solution, heating it to 70-75°C, stirring it at the temperature, separating out solids, washing and drying the solids to obtain pre-modified α-alumina; then adding acrylamide and ammonium persulfate to the aluminum nitrate solution, dispersing them uniformly, and then adding urea and stirring; adding the pre-modified α-alumina, heating it to 60-65°C, stirring it at the temperature, standing it, separating out solids, drying the solids, and then roasting them at 520-530°C to obtain the modified alumina base material; The method for preparing functional ceramics comprises the following steps: uniformly ball-milling a modified alumina base material, nano-calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose and an ethanol solution, and drying the mixture to obtain a ball-milled material; uniformly mixing the ball-milled material with boric acid, heating the mixture to 1400-1500° C., calcining the mixture at the same temperature, cooling the mixture naturally, and crushing the mixture to 12-17 μm to obtain a functional ceramic powder; The laser cladding method comprises: mixing aluminum-silicon alloy powder and functional ceramic powder evenly to obtain coating powder; pre-placing the coating powder on the outer surface of the aluminum alloy profile after surface treatment, and performing laser cladding treatment under argon protection conditions to obtain the aluminum alloy profile with the first coating; The preparation of the second coating comprises the following steps: preparation of a suspension, modification treatment, and film formation treatment; The method for preparing the suspension comprises: evenly ball-milling an ethanol solution, nano-silicon dioxide, nano-zirconium dioxide and nano-yttrium oxide, spraying silane coupling agent KH-602 and silane coupling agent KH-560 during the ball-milling process, continuing ball-milling, drying and obtaining a ball-milled product; adding the ball-milled product and sodium dodecyl sulfate into deionized water, dispersing them evenly and obtaining a suspension; The modification method comprises the following steps: adding carboxymethyl chitosan to a suspension and dispersing the mixture uniformly; adding hexadecyl trimethyl ammonium bromide with stirring, stirring the mixture uniformly at room temperature, and then standing the mixture; continuously adding L-ascorbic acid, stirring the mixture and heating the mixture to 40-45° C., keeping the temperature for 22-24 hours, separating the solid matter, washing the solid matter, and vacuum drying the solid matter to obtain a composite modified product; The film-forming treatment method comprises the following steps: putting silane coupling agent Si-69, silane coupling agent A-163 and a composite modifier into an ethanol solution, dispersing them uniformly, adjusting the pH value to 4-5 with acetic acid, stirring and heating to 40-42° C., and stirring while keeping the temperature, so as to obtain a film-forming liquid; completely immersing an aluminum alloy profile having a first coating into the film-forming liquid, pulling out the aluminum alloy profile after immersion, heating the profile to 80-85° C., and performing heat treatment at the temperature; heating the profile to 125-135° C., and performing heat treatment at the temperature, so as to obtain a corrosion-resistant aluminum alloy profile for ships.
2. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: In the preparation of the modified alumina base material, the concentration of the nitric acid solution is 0.3-0.35 mol / L; The concentration of the aluminum nitrate solution is 14-15wt%; The temperature is raised to 60-65°C and the stirring time is 2-3h; The calcination time at 520-530℃ is 3-4h.
3. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: In the preparation of the modified alumina base material, the particle size of α-alumina is 80-100 nm, and the specific surface area is 3-3.2 m 2 / g, pore volume is 0.7-0.8mL / g; The weight ratio of α-alumina to nitric acid solution is 1:7-8; The weight ratio of acrylamide, ammonium persulfate, aluminum nitrate solution, urea and pre-modified alpha-alumina is 4-4.3:1-1.2:100-105:5.5-5.8:22-24.
4. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: In the preparation of the functional ceramic, the heating rate to 1400-1500°C is 8-10°C / min; The calcination time at 1400-1500℃ is 2.5-3h; The weight ratio of modified alumina base material, nano calcium fluoride, chromium trioxide, lanthanum oxide, carboxymethyl cellulose and ethanol solution is 70-73:7-8:10-11:3-3.5:0.8-1:44-46; The volume concentration of the ethanol solution is 60-65%; The weight ratio of the ball-milled material to the boric acid is 100:1.8-2.
2.
5. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: In the laser cladding, the weight ratio of aluminum silicon alloy powder to functional ceramic powder is 1:2.2-2.5; The coating powder is pre-placed on the outer surface of the surface-treated aluminum alloy profile with a thickness of 1.2-1.6 mm; The laser output power of laser cladding is 2000-2200W, the scanning speed is 9-11mm / s, and the spot diameter is 4-5mm.
6. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: In the prepared suspension, the volume concentration of the ethanol solution is 70-75%; Control the addition time of silane coupling agent KH-602 and silane coupling agent KH-560 to 20-30s; The weight ratio of ethanol solution, nano silicon dioxide, nano zirconium dioxide, nano yttrium oxide, silane coupling agent KH-602 and silane coupling agent KH-560 is 5-5.8:6-7:3-3.5:1-1.2:0.9-1.1:0.4-0.5; The weight ratio of the ball-milled product, sodium dodecyl sulfate and deionized water is 5-6:0.6-0.7:110-120.
7. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: In the modification treatment, the weight ratio of carboxymethyl chitosan, suspension, hexadecyltrimethylammonium bromide and L-ascorbic acid is 1-1.1:110-120:0.2-0.3:0.55-0.
65.
8. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: In the film forming process, the volume concentration of the ethanol solution is 50-60%; The heating rate to 80-85°C is 1-1.5°C / min; The heating rate to 125-135°C is 3.5-4°C / min; The weight ratio of silane coupling agent Si-69, silane coupling agent A-163, composite modified product and ethanol solution is 2.5-3:1.5-1.7:2.2-2.5:
100.
9. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 1, characterized in that: The surface treatment method comprises the following steps: removing the aluminum oxide film on the surface of the aluminum alloy profile, grinding and polishing, and then completely immersing the aluminum alloy profile in acetone for ultrasonic cleaning; then completely immersing the aluminum alloy profile in a sodium hydroxide solution, heating the aluminum alloy profile to 55-65° C., taking the aluminum alloy profile out after heat preservation treatment, cleaning the aluminum alloy profile to neutrality, and then completely immersing the aluminum alloy profile in a nitric acid solution, taking the aluminum alloy profile out after room temperature treatment, cleaning the aluminum alloy profile to neutrality, and drying the aluminum alloy profile; and sandblasting the aluminum alloy profile until the surface roughness Ra is 1-1.2 μm to obtain the aluminum alloy profile after surface treatment.
10. The method for preparing the corrosion-resistant aluminum alloy profile for ships according to claim 9, characterized in that: In the surface treatment, the concentration of the sodium hydroxide solution is 5-6wt%; The heat preservation time at 55-65℃ is 240-300s; The concentration of nitric acid solution is 25-28wt%; The treatment time at room temperature is 20-40s.