A thin gauge 1000MPa grade high strength steel quenching plate shape control method
By optimizing the steel smelting, heating, rolling and quenching processes, the problem of quenching plate shape control of 1000MPa grade high-strength steel quenching is solved, and the good straightness and deformation-free cutting of the steel plate are achieved, and the production needs of high-strength and high-value-added products are met. .
Patent Information
- Application Number
- CN202411118542.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The prior art is difficult to effectively control the shape of 1000MPa grade high-strength steel quenched plates with thickness specifications of 6 to 20 mm and width specifications of 2500 to 4000 mm, especially in reducing warping and bending deformation.
Adopted the optimized steel smelting, heating, rolling, heat treatment and quenching process, including controlling the continuous casting superheat, billet rate, electromagnetic stirring current intensity and secondary cooling water volume, through two-stage rolling and heat straightening processes, combined with High and low temperature quenching process, strictly control the furnace time and temperature at each stage.
It effectively reduces the warping and bending deformation of the steel plate after quenching, meets the plate shape control requirements (straightness is below 3mm/2m), and does not deform after cutting, and does not require subsequent offline tempering and straightening treatment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heat treatment of steel plates, and in particular to a method for controlling the shape of a quenched plate of 1000MPa grade high-strength steel with a thickness specification of 6-20mm and a width specification of 2500-4000mm. Background Art
[0002] Quenching of medium and thick plates is an important technical means to produce high-performance and high-value-added products. Some high-strength and high-grade medium and thick plate products (such as high-strength ship steel, engineering machinery steel, etc.) require quenching technology to ensure performance. However, the violent cooling process can easily produce serious residual stress in the steel plate, causing the steel plate to bend and warp after quenching, and also affecting the dynamic performance of subsequent materials (such as fracture toughness, etc.). At present, the quenching of high-strength grade steel plates mainly adopts roller continuous quenching, that is, after the steel plate is taken out of the furnace, it is cooled by a roller quenching equipment composed of multiple groups of upper and lower water cooling facilities. Roller quenching equipment generally achieves uniformity of steel plate quenching, cooling rate control and plate shape control by adjusting parameters such as the water volume of the water cooling system and the roller speed of the equipment. During roller continuous quenching, since water cooling can be seen on the upper and lower surfaces of the steel plate, there is no quenching soft spot, and its cooling uniformity, cooling rate control and other problems can be greatly improved.
[0003] However, a large number of studies have shown that: although on the roller quenching machine, by reasonably controlling the water volume, water ratio and roller speed of the upper and lower nozzles of the quenching machine, steel plates with a thickness greater than 20mm can basically obtain excellent performance and good quenched plate shape. However, there are still certain problems for thin-gauge steel plates with a thickness of no more than 20mm. This is because the factors affecting the plate shape after quenching of thin plates are more complicated. The fundamental reason for the warping and deformation of thin-gauge steel plates during the quenching process lies in the internal stress. There are two main types of internal stress, one is the thermal stress caused by uneven cooling, and the other is the organizational stress caused by phase change during quenching. The manifestation of the two stress forms in the quenched steel plate is related to many factors such as the chemical composition, size, hardenability of the steel, quenching medium and cooling method. Therefore, as the thickness of the steel plate is reduced to less than 20mm, the control of cooling uniformity and plate flatness becomes the key to quenching process control. How to solve the problem of quenched plate shape of 1000MPa high-strength steel with a thickness of 6 to 20mm and a width of 2500 to 4000mm is the key to the development of this thin-gauge and wide-width high-strength steel plate.
[0004] So far, there is little research on the control of quenched plate shape of 1000MPa high-strength steel with thin specifications (thickness 6-20mm) and width greater than 2500mm at home and abroad. The Chinese patent application with publication number CN 115011764A discloses "a segmented quenching control process for ultra-thin high-hardness steel plates". The steel plate quenching process is segmented and cooled. The steel plate is divided into a high-temperature section and a low-temperature section with a segmentation point of 50 to +150℃ above the Ms point. Different cooling methods are used for quenching. A combination of high restraint stress and different cooling rates is used to ensure that the plate shape is straight when the phase transformation stress of the steel plate is large, and the organization control of the steel plate is achieved simultaneously. Compared with the existing roller quenching process, the segmented quenching control process has higher requirements on equipment and cooling manifold accuracy and response time, and it is aimed at steel plates with a thickness of less than 15mm. The requirements for the width of the steel plate and the straightness after quenching are not clear.
[0005] The journal article "Control of Plate Shape during Quenching of Thin-Gauge Steel Plates" (Journal of Iron and Steel Research, 2011.9) mainly stabilizes the unevenness of the plate shape of thin-gauge steel plates after quenching within a controllable range through the adjustment and calibration of the quenching machine equipment, combined with reasonable quenching process parameters, but it does not clarify the plate width and thickness group range suitable for production. Summary of the invention
[0006] The present invention provides a thin-gauge 1000MPa-grade high-strength steel quenching plate shape control method, which is suitable for 1000MPa-grade high-strength steel with a thickness specification of 6-20mm and a width specification of 2500-4000mm. The method adopts the method of optimizing the ingot smelting, heating, rolling, steel plate heat treatment and quenching process to solve the problem of plate warping and bending deformation of 1000MPa-grade high-strength steel after quenching. The plate shape control requirements (straightness is below 3mm / 2m) can be met without subsequent offline tempering and straightening treatment, and the steel plate will not be deformed after cutting.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for controlling the shape of thin-gauge 1000MPa grade high-strength steel quenched, wherein the chemical composition of the steel plate includes, by weight percentage: C 0.14% to 0.19%, Si 0.2% to 0.45%, Mn 1.3% to 1.5%, P ≤ 0.02%, S ≤ 0.005%, Ti 0.015% to 0.03%, B 0.0003% to 0.0016%, Als 0.015% to 0.045%, Ceq 0.39%~0.46%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15; the balance is Fe and unavoidable impurities, O≤0.0050% among the impurities, and the total amount of other impurity elements is less than 0.05%; the steel plate production process includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, ingot reheating, controlled rolling, hot straightening and quenching.
[0009] Furthermore, the steel plate production process is specifically as follows:
[0010] 1) Molten steel smelting to continuous casting;
[0011] During the pretreatment of molten iron, the S content is controlled to be ≤0.005%, the P content is controlled to be ≤0.02% during converter smelting, the C content is controlled to be 0.14% to 0.19% at the end of converter smelting, and argon is blown for 21 to 25 minutes during converter tapping; RH vacuum degassing is maintained for more than 15 minutes; then Al is added, Ti-Fe is added for micro-titanium treatment, and then B-Fe alloy is added for B alloying treatment;
[0012] During continuous casting of slabs, the superheat is controlled at 15-25°C, the billet drawing rate is 1.5-1.8 m / min, the electromagnetic stirring current intensity in the secondary cooling zone is 200-250 A, and the secondary cooling water volume is 1.8-2.5 L / kg; under the heavy pressure at the horizontal sector section, i.e. the end of solidification, the continuous casting billet is pressed down by 25-35 mm;
[0013] Reheating of the ingot;
[0014] The temperature of the preheating section is 950-1150℃, the heating temperatures of the soaking section and the heating section are both 1235-1250℃, the total heating time of the soaking section and the heating section is 4.5-6.5h, and the total furnace time is 6-8h; the air-fuel ratio is controlled to be 1:1.8-1:2.5, and the temperature difference between the upper and lower surfaces of the ingot is controlled within 30℃;
[0015] Controlled rolling;
[0016] Rolling is carried out in two stages; the starting rolling temperature of rough rolling is ≥1100℃, the final rolling temperature of rough rolling is 985~1025℃, the rough rolling is not more than 8 passes, and the reduction rate of at least the first 2 passes is more than 20%; the starting rolling temperature of finishing rolling is 920~960℃, the final rolling temperature of finishing rolling is 830~880℃, the finishing rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 20%;
[0017] Heat straightening;
[0018] The straightening temperature is 700-750℃, the straightening force is 2000-2500kN, the bending roller is set to 1-1.8mm, and the tilting value is set to 3-5.5mm;
[0019] Quenching;
[0020] The heat treatment furnace adjusts the furnace temperature in different zones. The temperature of the front high-temperature section is 880-920°C, and the temperature of the rear cooling section is 770-800°C. The steel plate slowly cools down to 770-800°C during its movement to the heat treatment furnace exit. The steel plate stays in the furnace for 1.5-2.0 min / mm in the high-temperature section, and for 2.1-2.5 min / mm in the cooling section. During the quenching of the steel plate, the water ratio of the upper and lower headers is 1.6-2.1, the cooling rate is 10-60°C / s, the roller speed is 1.2-2.1 m / s, and the acceleration is 0.003-0.005 m / s. 2 The final quenching temperature is 150-250℃.
[0021] Furthermore, the finished steel plate has a thickness of 6 to 20 mm and a width of 2500 to 4000 mm.
[0022] Furthermore, the thickness of the cast billet is less than 250 mm, and the thickness of the intermediate billet is 3 to 4.5 times the thickness of the finished steel plate.
[0023] Furthermore, the straightness of the finished steel plate is ≤3mm / 2m.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1) By controlling the continuous casting superheat, billet drawing rate, electromagnetic stirring current intensity in the secondary cooling zone and the secondary cooling water volume, the surface and corner quality defects of the billet can be effectively reduced, the average carbon segregation index can be reduced, and segregation can be inhibited; at the end of solidification, the billet is put under heavy pressure to effectively reduce the central porosity level and segregation of the billet, refine the austenite grains, and reduce internal structural defects.
[0026] 2) By controlling the preheating temperature, it is ensured that the carbide of Ti is quickly and fully dissolved in the matrix and fully diffused; by using a high heating temperature, while ensuring the furnace time of the soaking section and the heating section, controlling the air-fuel ratio, shortening the temperature difference between the surface and the core of the continuous casting billet, improving the uniformity of the lateral and longitudinal metal flow on the surface of the steel plate, and ensuring the uniformity of the upper and lower surface temperatures of the billet during the subsequent rolling process; by controlling the total furnace time, it is effectively promoted to fully and uniformly diffuse the C and Mn elements, ensuring the good plate shape of the rolled steel plate.
[0027] 3) A two-stage controlled rolling process is adopted. By controlling the final rolling temperature in the rough rolling stage, the intermediate billet is kept in the austenite recrystallization temperature range during the temperature waiting process to ensure the uniformity of the structure. By limiting the two-stage rolling reduction rate and the thickness of the intermediate billet, the uniformity of the structure in the thickness direction of the rolled steel plate is ensured. A reasonable hot straightening process is adopted to promote the full release of internal stress. By setting appropriate roll gaps, roll bending amounts and tilting values, the straightness of the straightened plate is ensured to be good.
[0028] 4) High and low temperature quenching process is adopted, and the furnace time of each stage is strictly controlled to ensure that the steel plate is quickly heated to the austenitizing temperature, so as to provide organizational guarantee for the subsequent quenching of the steel plate to obtain martensite; at the same time, the temperature is controlled not to be too high to avoid coarse austenite grains and reduce the low-temperature toughness of the steel plate; the temperature of the 15-meter temperature zone at the tail of the heat treatment furnace is cooled, the purpose is to reduce the austenite to below the Ar3 temperature in the cooling section. In this temperature range, due to the short-term phase transformation incubation period of the steel plate with slow cooling, most of the austenite structure is basically maintained and only a very small amount of ferrite structure is formed. Based on this, it is quenched to 150-250℃, which ensures that the quenched steel plate is fully hardened while reducing the stress level of the steel plate during the quenching process; by controlling the upper and lower header water ratio, cooling rate, roller speed and acceleration during the quenching process of the steel plate, the upper and lower surface temperature uniformity of the steel plate during the quenching process is ensured; after quenching, the steel plate can meet the plate shape control requirements (straightness is below 3mm / 2m) without subsequent offline tempering and straightening treatment, and the steel plate will not deform after cutting. DETAILED DESCRIPTION
[0029] The invention discloses a thin-gauge 1000MPa-grade high-strength steel quenching plate shape control method, which is applicable to 1000MPa-grade high-strength steel plates with a thickness of 6-20mm and a width of 2500-4000mm; the chemical composition of the steel plates comprises, by weight percentage, C 0.14%-0.19%, Si 0.2%-0.45%, Mn 1.3%-1.5%, P≤0.02%, S≤0.005%, Ti0.015%-0.03%, B 0.0003%-0.0016%, Als 0.015%-0.045%, Ceq 0.39%-0.46%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, the remainder is Fe and unavoidable impurities, O in the impurities is ≤0.0050%, and the total amount of other impurity elements is less than 0.05%.
[0030] The production process of a thin-gauge 1000MPa high-strength steel plate described in the present invention includes molten steel smelting → refining outside the furnace + RH vacuum degassing → micro-Ti treatment → B alloying → continuous casting → ingot reheating → controlled rolling → hot straightening → quenching and other processes. The specific control process is as follows:
[0031] Molten steel smelting and continuous casting:
[0032] The raw materials are pre-treated by KR hot metal to control the S content below 0.005%, and then enter the converter after slag removal; the double slag method is used to remove P in the converter to control the P content ≤ 0.02%, and the C content is controlled at 0.14% to 0.19% at the end of converter smelting. Argon is blown for 21 to 25 minutes when the converter is tapped. Argon blowing before continuous casting can promote the removal of inclusions in the molten steel and improve the uniformity of the molten steel composition.
[0033] Then LF refining and RH vacuum degassing are carried out, and the RH vacuum degassing is maintained for more than 15 minutes. After the degassing treatment is completed, sufficient Al is added according to the Als requirement. Then Ti-Fe is added for micro-titanium treatment, and B-Fe alloy is added for B alloying treatment. When adding materials, ensure that they are added into the molten steel to avoid floating on the slag layer.
[0034] During continuous casting of slabs, the continuous casting superheat is controlled at 15-25℃, and the billet drawing rate is 1.5-1.8m / min; by controlling the pouring superheat and the continuous casting billet drawing speed, the surface and corner quality defects of the billet are effectively reduced. The electromagnetic stirring current intensity of the secondary cooling zone in the continuous casting stage is controlled to be 200-250A, and the secondary cooling water volume is 1.8-2.5L / kg, in order to reduce the average carbon segregation index and inhibit segregation; by limiting the secondary cooling intensity, the tendency of the central crack of the billet to worsen is inhibited. When the horizontal fan-shaped section, i.e., the end of solidification, is put under heavy pressure, the continuous casting billet is pressed down by 25-35mm; putting under heavy pressure helps to reduce billet segregation, refine austenite grains, and reduce internal structural defects.
[0035] Reheating of the ingot;
[0036] The ingot (thickness less than 250mm) is sent into a walking beam heating furnace for heating. The temperature range of the preheating section is 950-1150℃, which makes the carbide of Ti quickly and fully dissolved in the matrix and fully diffused. The heating temperature of the soaking section and the heating section are both 1235-1250℃. The total heating time of the soaking section and the heating section is 4.5-6.5 hours. The total time in the furnace is controlled at 6-8 hours. The opening of the upper and lower burners of the heating furnace is adjusted, and the air-fuel ratio is controlled to be 1:1.8-1:2.5. The temperature difference between the upper and lower surfaces of the ingot is controlled within 30℃.
[0037] The high heating temperature is adopted, while the soaking section and the heating section are kept in the furnace for a certain time, in order to shorten the temperature difference between the surface and the core of the continuous casting billet, improve the uniformity of the metal flow in the transverse and longitudinal directions on the surface of the steel plate, and ensure the shape of the rolled steel plate; the total time in the furnace is increased to effectively promote the full diffusion of C and Mn elements and ensure the uniformity of the hot-rolled structure.
[0038] Controlled rolling;
[0039] Rolling is divided into two stages; the first stage is recrystallization rolling (rough rolling), the rough rolling start temperature is ≥1100℃, the rough rolling final rolling temperature range is 985~1025℃, the rough rolling is not more than 8 passes, and the pass reduction system is that at least the first 2 passes ensure the reduction rate is above 20%. The thickness of the intermediate billet is 3 to 4.5 times the thickness of the finished steel plate. The second stage is non-recrystallization rolling (finishing rolling), the finishing rolling start temperature range is 920~960℃, the finishing rolling final rolling temperature range is 830~880℃, the finishing rolling is not more than 6 passes, and the pass reduction system is that at least the first 2 passes ensure the reduction rate is above 20%.
[0040] By controlling the final rolling temperature in the rough rolling stage, the intermediate billet is kept in the austenite recrystallization temperature range during the temperature waiting process to ensure the uniformity of the structure; by limiting the reduction rate of the two-stage rolling, the uniformity of the structure of the steel plate in the thickness direction after rolling is ensured.
[0041] Heat straightening;
[0042] The straightening temperature of hot straightening is 700-750℃, the straightening force is between 2000-2500kN, the bending roller is set to 1-1.8mm, and the tilting value is set to 3-5.5mm. Hot straightening promotes the full release of internal stress, and by setting the appropriate roll gap, bending roller and tilting value, the straightness of the plate after straightening is guaranteed to be good.
[0043] Quenching;
[0044] The steel plate quenching and heating process is divided into a high temperature section and a cooling section. During the quenching and heating process of thin-gauge high-strength steel with a thickness of less than 20 mm, the heat treatment furnace is used to adjust the furnace temperature by zoning. The temperature of the high temperature section at the front (preferably within 75 meters from the heat treatment furnace entrance) is 880-920°C, and the temperature of the cooling zone at the rear (preferably within 15 meters from the heat treatment furnace exit) is 770-800°C. The steel plate is slowly cooled to 770-800°C when moving toward the heat treatment furnace exit. The steel plate in the high temperature section is 1.5-2.0 min / mm in the furnace, and the steel plate in the low temperature section is 2.1-2.5 min / mm in the furnace. During the steel plate quenching process, the upper and lower header water ratio is 1.6-2.1, the cooling rate is 10-60°C / s, the roller speed is 1.2-2.1 m / s, and the acceleration is 0.003-0.005 m / s 2 The final quenching temperature is 150-250℃.
[0045] The temperature of the high temperature section is controlled at 880-920℃, and the time in the high temperature section is controlled at 1.5-2.0 min / mm. The purpose is to quickly heat the steel plate to the austenitizing temperature and provide organizational guarantee for the subsequent quenching of the steel plate to obtain martensite. Since excessive temperature will cause the austenite grains to increase and reduce the low-temperature toughness of the steel plate, the holding time should not exceed 2.0min / mm. The temperature of the cooling section is controlled at 770-800℃, and the time in the cooling section is controlled at 2.1-2.5min / mm. The purpose is to reduce the austenite to below the Ar3 temperature in the cooling section. In this temperature range, due to the slow cooling and short phase transformation incubation period of the steel plate, most of the austenite structure is basically maintained and only a very small amount of ferrite structure is formed. Based on this, it is quenched to 150-250℃. While ensuring that the quenched steel plate is fully hardened, it also reduces the stress level of the steel plate during the quenching process.
[0046] The 1000MPa high-strength steel plates with a thickness of 6 to 20mm and a width of 2500 to 4000mm prepared by the above-mentioned composition and process have effectively solved the problems of plate warping and bending deformation after quenching. No subsequent offline tempering and straightening treatment is required to meet the plate shape control requirements (straightness is below 3mm / 2m), and the steel plates will not be deformed after cutting.
[0047] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention.
[0048] Example
[0049] Table 1 shows the chemical composition of the steel in each embodiment, Table 2 shows the smelting process parameters of the steel in each embodiment, Table 3 shows the heating process parameters of the ingot in each embodiment, Table 4 shows the rolling process parameters of the steel plate in each embodiment, Table 5 shows the straightening and heat treatment process parameters of the steel plate in each embodiment, and Table 6 shows the quenching process parameters of the steel plate and the finished plate shape indicators in each embodiment.
[0050] Table 1 Chemical composition of steel (wt, %)
[0051] Example C Si Mn Als B Ti Ceq 1 0.16 0.33 1.45 0.016 0.0003 0.018 0.402 2 0.18 0.22 1.38 0.043 0.0008 0.017 0.410 3 0.14 0.44 1.49 0.029 0.0015 0.025 0.390 4 0.19 0.29 1.32 0.037 0.0011 0.030 0.410 5 0.17 0.38 1.48 0.028 0.0006 0.024 0.416 6 0.16 0.35 1.43 0.019 0.0009 0.017 0.398
[0052] Note: Impurity elements in steel: P≤0.02%, S≤0.005%, O≤0.0050%.
[0053] Table 2 Steel smelting process parameters
[0054] Example Argon blowing time / min RH vacuum degassing time / min Superheat / ℃ <![CDATA[Drawing speed / m·min -1 > Electromagnetic stirring current intensity / A Continuous casting billet reduction / mm Secondary cooling water / L / kg 1 22 16 16 1.6 220 25 1.8 2 21 17 23 1.7 250 32 2.2 3 25 20 22 1.8 230 33 2.4 4 23 18 25 1.5 250 28 2.5 5 22 16 15 1.6 235 30 2.2 6 24 19 19 1.7 240 29 2.0
[0055] Table 3 Heating process parameters of ingot
[0056]
[0057] Table 4 Rolling process parameters of steel plates
[0058] Example Rough rolling start temperature / ℃ Rough rolling and final rolling temperature / ℃ Roughing pass times Intermediate billet thickness / mm Rough rolling first pass reduction rate / % Rough rolling second pass reduction rate / % Finish rolling first pass reduction rate / % Finishing rolling second pass reduction rate / % Finish rolling start temperature / ℃ Finish rolling temperature / ℃ Finishing pass times 1 1130 1020 6 80 20 25 23 20 960 870 5 2 1125 995 5 63 22 20 23 21 945 855 6 3 1120 985 4 44 25 22 22 23 958 835 6 4 1108 1005 8 24 23 21 22 20 935 830 5 5 1115 1015 6 50 23 24 20 22 950 860 4 6 1112 1025 7 48 22 25 23 21 953 850 4
[0059] Table 5 Steel plate straightening and heat treatment process parameters
[0060] Example Heat correction temperature / ℃ Straightening force / kN Roll bending amount / mm Tilt value / mm Heat treatment high temperature section temperature / ℃ High temperature section in furnace time / min / mm Heat treatment low temperature section temperature / ℃ Low temperature section in furnace time / min / mm 1 730 2200 1.2 3.2 910 1.8 780 2.2 2 745 2380 1.5 4.5 880 1.9 775 2.5 3 728 2225 1.7 4.8 890 1.6 790 2.1 4 702 2415 1.4 5.3 920 2.0 800 2.3 5 725 2306 1.1 5.5 900 1.7 785 2.2 6 735 2300 1.7 3.8 885 1.5 790 2.4
[0061] Table 6 Quenching process parameters and plate shape indicators of steel plates
[0062] Example <![CDATA[Rollerway acceleration / m / s 2 > Roller speed / m / s Water ratio Cooling speed / ℃ / s Quenching end temperature / ℃ Steel plate thickness / mm Straightness / 2m 1 0.004 1.5 1.7 55 230 20 2 2 0.005 2.1 2.0 35 180 14 3 3 0.005 1.7 1.8 20 150 10 1 4 0.004 1.5 1.7 12 200 6 2 5 0.003 1.3 2.1 20 170 12 2 6 0.003 2.0 1.6 35 180 15 1
[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for controlling the shape of thin-gauge 1000MPa grade high-strength steel quenched, characterized in that: The chemical composition of the steel plate includes by weight percentage: C 0.14%-0.19%, Si 0.2%-0.45%, Mn 1.3%-1.5%, P≤0.02%, S≤0.005%, Ti 0.015%-0.03%, B 0.0003%-0.0016%, Als 0.015%-0.045%, Ceq 0.39%-0.46%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15; the balance is Fe and unavoidable impurities, O in the impurities is ≤0.0050%, and the total amount of other impurity elements is less than 0.05%; the production process of the steel plate includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, ingot reheating, controlled rolling, hot straightening and quenching; the thickness of the finished steel plate is 6-20mm; The steel plate production process is specifically as follows: 1) Molten steel smelting to continuous casting: During the pretreatment of molten iron, the S content is controlled to be ≤0.005%, the P content is controlled to be ≤0.02% during converter smelting, the C content is controlled to be 0.14% to 0.19% at the end of converter smelting, and argon is blown for 21 to 25 minutes during converter tapping; RH vacuum degassing is maintained for more than 15 minutes; then Al is added, Ti-Fe is added for micro-titanium treatment, and then B-Fe alloy is added for B alloying treatment; During continuous casting of slabs, the superheat is controlled at 15-25°C, the billet drawing rate is 1.5-1.8 m / min, the electromagnetic stirring current intensity in the secondary cooling zone is 200-250 A, and the secondary cooling water volume is 1.8-2.5 L / kg; the billet is pressed down by 25-35 mm under heavy pressure at the horizontal sector section, i.e., at the end of solidification; 2) Reheating of ingot: The temperature of the preheating section is 950-1150℃, the heating temperatures of the soaking section and the heating section are both 1235-1250℃, the total heating time of the soaking section and the heating section is 4.5-6.5h, and the total furnace time is 6-8h; the air-fuel ratio is controlled to be 1:1.8-1:2.5, and the temperature difference between the upper and lower surfaces of the ingot is controlled within 30℃; 3) Controlled rolling: Rolling is carried out in two stages; the starting rolling temperature of rough rolling is ≥1100℃, the final rolling temperature of rough rolling is 985~1025℃, the rough rolling is not more than 8 passes, and the reduction rate of at least the first 2 passes is more than 20%; the starting rolling temperature of finishing rolling is 920~960℃, the final rolling temperature of finishing rolling is 830~880℃, the finishing rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 20%; 4) Heat straightening: The straightening temperature is 700-750℃, the straightening force is 2000-2500kN, the bending roller is set to 1-1.8mm, and the tilting value is set to 3-5.5mm; 5) Quenching: The heat treatment furnace adjusts the furnace temperature in different zones. The temperature of the front high-temperature section is 880-920°C, and the temperature of the rear cooling section is 770-800°C. The steel plate slowly cools down to 770-800°C during its movement to the heat treatment furnace exit. The steel plate stays in the furnace for 1.5-2.0 min / mm in the high-temperature section, and for 2.1-2.5 min / mm in the cooling section. During the quenching of the steel plate, the water ratio of the upper and lower headers is 1.6-2.1, the cooling rate is 10-60°C / s, the roller speed is 1.2-2.1 m / s, and the acceleration is 0.003-0.005 m / s. 2 The final quenching temperature is 150-250℃.
2. A thin gauge 1000MPa grade high strength steel quenching plate shape control method according to claim 1, characterized in that: The width of the finished steel plate is 2500~4000mm.
3. A thin gauge 1000MPa grade high strength steel quenching plate shape control method according to claim 1, characterized in that: The thickness of the cast billet is less than 250 mm, and the thickness of the intermediate billet is 3 to 4.5 times the thickness of the finished steel plate.
4. A thin gauge 1000MPa grade high strength steel quenching plate shape control method according to claim 1, characterized in that: The straightness of the finished steel plate is ≤3mm / 2m.
Citation Information
Patent Citations
Subsection quenching control process for ultra-thin high-hardness steel plate
CN115011764A
Steel for hot forming
CN109023136A
Short-process produced quenched distribution-partitioning steel with tensile strength greater than or equal to 980MPa and method
CN111440987A