Preparation method of high-molecular rubber sealing product with high-pressure hydrogen permeation resistance

By mixing EPDM rubber with natural rubber and introducing nanocomposites, a dense network structure is formed, which solves the problem of hydrogen penetration of rubber sealing products in a high-pressure hydrogen environment and significantly improves its resistance to high-pressure hydrogen penetration and air tightness. .

CN118725469AActive Publication Date: 2024-10-01ANHUI TONGFENG RUBBER & PLASTIC IND
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410970270.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing rubber sealing products are difficult to effectively block hydrogen penetration in high-pressure hydrogen environments, affecting the safety and reliability of the system.

Method used

EPDM rubber and natural rubber are mixed and refined, and a special nanocomposite is introduced. The nanocomposite strongly interacts with the rubber molecules to form a dense network structure, which increases air tightness and blocks hydrogen penetration. .

Benefits of technology

Significantly improves the high-pressure hydrogen permeability resistance and air tightness of rubber sealing products, ensuring stable performance in high-temperature and high-pressure environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a polymer rubber sealing product with high-pressure hydrogen permeation resistance, and relates to the technical field of rubber sealing, and the preparation method comprises the following steps: S1, obtaining plasticated rubber; s2, obtaining a rubber compound; and S3, putting the rubber compound obtained in the step S2 on a vulcanizing machine for pre-vulcanization, and performing thin passing for three times and secondary vulcanization to obtain the rubber material, the polymer rubber sealing product with high-pressure hydrogen permeation resistance can be applied to various industrial fields, and particularly plays an important role in high-temperature and high-pressure occasions. In the field of hydrogen energy, hydrogen is extremely small in molecule, high in activity and easy to permeate into a plurality of materials, so that preparation raw materials of the rubber sealing product are greatly improved and the dosage is optimized, and the prepared rubber sealing product not only has excellent chemical resistance and high-temperature resistance, but also has excellent mechanical property and high-temperature resistance. And in a high-pressure hydrogen medium environment, the composite material also has good airtight performance and high-pressure hydrogen permeation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber sealing, in particular to a method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance. Background Art

[0002] In modern industry and life, there are many places where sealing is needed. Therefore, rubber sealing products are everywhere. With their unique properties and wide range of applications, they have become an indispensable part of our daily life and industrial development.

[0003] Rubber sealing products are mainly made of natural rubber or synthetic rubber, with excellent elasticity, flexibility and electrical insulation properties. Rubber sealing products can maintain good sealing effects in a wide temperature range and have good tolerance to various chemical media.

[0004] Rubber sealing products include: rotating shaft rubber seals, multi-lip reciprocating rubber seals, Y / M special-section rubber seals, rubber gaskets, V-shaped rubber seals and many other products.

[0005] In order to cope with global climate change, the demand for energy conservation and environmental protection is constantly increasing. With the rapid development of the new energy vehicle industry, hydrogen energy vehicles have emerged. The hydrogen storage containers in their devices require an ultra-high pressure sealing system of 90MPa. The rubber sealing products used in this sealing system need to be resistant to hydrogen penetration.

[0006] With the rapid development of hydrogen energy technology, hydrogen, as a clean and efficient energy source, is gradually attracting global attention. However, in the process of hydrogen storage and transportation, how to ensure the safety and reliability of the system has become an urgent problem to be solved. Among them, rubber sealing products are an indispensable component of the hydrogen system, and their resistance to high-pressure hydrogen permeation is particularly important. This article will conduct an in-depth study on the resistance to high-pressure hydrogen permeation of rubber sealing products.

[0007] Based on this, a method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance is provided to solve the existing technical problems. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance to solve the deficiencies in the prior art.

[0009] The technical solution adopted by the present invention is as follows:

[0010] A method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance comprises the following steps:

[0011] S1: adding EPDM rubber and natural rubber to an internal mixer, heating the mixture to 92-95°C at a heating rate of 3°C / min, and plasticizing for 40 minutes to obtain plasticized rubber;

[0012] S2: adding the plasticized rubber, nanocomposite, stearic acid, antioxidant, vulcanizing agent and accelerator in step S1 to a mixer, heating the mixture to 98°C at a heating rate of 5°C / min, and mixing for 30-40 minutes to obtain a mixed rubber;

[0013] S3: placing the rubber compound obtained in step S2 on a vulcanizer for pre-vulcanization at 120-128° C. for 12-16 minutes, thin-passing for 3 times, and secondary vulcanization at 155-160° C. for 6-8 minutes to obtain the product.

[0014] As a further technical solution: the preparation method of the nanocomposite material in S2 is:

[0015] Add zinc acetate and lanthanum chloride to ethylene glycol monomethyl ether, adjust the temperature to 60°C, and stir for 30 minutes;

[0016] Then, ethanolamine was added dropwise, and the mixture was stirred and mixed for 2 hours under heat preservation, and allowed to stand for 20 hours to obtain a first reaction solution;

[0017] uniformly dispersing carbon nanotubes in ethylene glycol monomethyl ether to obtain a carbon nanotube dispersion;

[0018] The first reaction liquid is added to the carbon nanotube dispersion liquid, and then ultrasonically dispersed for 10 minutes to obtain a composite dispersion liquid;

[0019] Drying the composite dispersion to a constant weight to obtain a composite material;

[0020] The composite material is subjected to a primary calcination treatment in a furnace, and cooled to room temperature to obtain a calcined material;

[0021] Mix the silicate with anhydrous ethanol, then add deionized water, continue stirring and dispersing for 30 minutes, then add the calcined material, after ultrasonic dispersion, let it stand for 2 hours, then dry to constant weight, finally calcine it twice in a furnace, cool it to room temperature, and obtain a nanocomposite material.

[0022] As a further technical solution: the molar ratio of zinc acetate to lanthanum chloride is 2:1;

[0023] The mass ratio of zinc acetate to ethylene glycol monomethyl ether and ethanolamine is 1:20:3;

[0024] The mass fraction of the carbon nanotube dispersion is 10%;

[0025] The mixing volume ratio of the first reaction liquid to the carbon nanotube dispersion liquid is 3:1-1.5.

[0026] As a further technical solution: the primary calcination temperature is 500° C. and the time is 40 minutes.

[0027] As a further technical solution: the mass ratio of the silicate to anhydrous ethanol and deionized water is 1:6:4;

[0028] The mass ratio of the silicate to the calcined material is 1:3;

[0029] The secondary calcination temperature is 550°C and the time is 45 minutes.

[0030] As a further technical solution: the stirring speed during the plasticating is 150r / min;

[0031] The stirring speed during the mixing is 300 r / min.

[0032] As a further technical solution: the polymer rubber sealing product with high-pressure hydrogen permeation resistance includes, by weight: 50-60 parts of EPDM rubber, 25-28 parts of natural rubber, 12-15 parts of nano-composite materials, 1-2 parts of stearic acid, 1-3 parts of antioxidant, 1-1.5 parts of vulcanizing agent, and 0.5-0.8 parts of accelerator.

[0033] As a further technical solution: the antioxidant is antioxidant MB.

[0034] As a further technical solution: the vulcanizing agent is sulfur.

[0035] As a further technical solution, the accelerator is DTDM.

[0036] Beneficial effects:

[0037] The polymer rubber sealing product with high-pressure hydrogen permeation resistance prepared by the present invention can be applied to various industrial fields, and plays an important role in high-temperature and high-pressure occasions. In the field of hydrogen energy, since hydrogen molecules are extremely small and highly active, they can easily penetrate into many materials. Therefore, the present invention significantly improves the raw materials for preparing rubber sealing products and optimizes the dosage, so that the prepared rubber sealing products not only have excellent chemical resistance and high-temperature resistance, but also have good airtightness and high-pressure hydrogen permeation resistance in a high-pressure hydrogen medium environment.

[0038] Improve gas barrier properties: Nanoparticles have extremely small size and high specific surface area, and can form a dense network structure in the rubber matrix. The present invention introduces a special nanocomposite material, which can produce a strong interaction with the rubber molecules. This effect not only enhances the binding force between rubber molecules, but also enables the nanocomposite particles to be evenly dispersed in the rubber to form a stable network structure, greatly improving the air tightness of the rubber sealing product, thereby improving the performance of high-pressure hydrogen penetration resistance.

[0039] Since in traditional rubber sealing products, the penetration of gas molecules is mainly carried out through the gaps between rubber molecular chains, the present invention optimizes the raw material components of rubber sealing products and introduces a special nano-composite material to prevent this process from occurring. Through the introduction of the nano-composite material, a "barrier" can be formed in the rubber sealing product, thereby greatly blocking the penetration of hydrogen molecules. In addition, since the nano-composite material prepared by the present invention is not a single nano-particle, its structure is more complex, which can increase the tortuosity of the diffusion path of hydrogen molecules and further reduce the permeability of hydrogen. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] A method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance comprises the following steps:

[0043] S1: adding EPDM rubber and natural rubber to an internal mixer, heating the mixture to 92°C at a heating rate of 3°C / min, and plasticizing for 40 minutes to obtain plasticized rubber;

[0044] S2: adding the plasticized rubber, nanocomposite, stearic acid, antioxidant, vulcanizing agent and accelerator in step S1 to a mixer, heating the mixture to 98°C at a heating rate of 5°C / min, and mixing for 30 minutes to obtain a mixed rubber;

[0045] S3: placing the rubber compound obtained in step S2 on a vulcanizer for pre-vulcanization at 120° C. for 12 minutes, performing thin-pass vulcanization three times, and performing secondary vulcanization at 155° C. for 6 minutes to obtain the obtained product.

[0046] The preparation method of nanocomposite material is as follows:

[0047] Add zinc acetate and lanthanum chloride to ethylene glycol monomethyl ether, adjust the temperature to 60°C, and stir for 30 minutes;

[0048] Then, ethanolamine was added dropwise, and the mixture was stirred and mixed for 2 hours under heat preservation, and allowed to stand for 20 hours to obtain a first reaction solution;

[0049] uniformly dispersing carbon nanotubes in ethylene glycol monomethyl ether to obtain a carbon nanotube dispersion;

[0050] The first reaction liquid is added to the carbon nanotube dispersion liquid, and then ultrasonically dispersed for 10 minutes to obtain a composite dispersion liquid;

[0051] Drying the composite dispersion to a constant weight to obtain a composite material;

[0052] The composite material is subjected to a primary calcination treatment in a furnace, and cooled to room temperature to obtain a calcined material;

[0053] Mix the silicate with anhydrous ethanol, then add deionized water, continue stirring and dispersing for 30 minutes, then add the calcined material, after ultrasonic dispersion, let it stand for 2 hours, then dry to constant weight, finally calcine it twice in a furnace, cool it to room temperature, and obtain a nanocomposite material.

[0054] The molar ratio of zinc acetate to lanthanum chloride is 2:1;

[0055] The mass ratio of zinc acetate to ethylene glycol monomethyl ether and ethanolamine is 1:20:3;

[0056] The mass fraction of the carbon nanotube dispersion is 10%;

[0057] The mixing volume ratio of the first reaction liquid to the carbon nanotube dispersion liquid is 3:1.

[0058] The primary calcination temperature is 500°C and the time is 40 minutes.

[0059] The mass ratio of silicate to anhydrous ethanol and deionized water is 1:6:4;

[0060] The mass ratio of the silicate to the calcined material is 1:3;

[0061] The secondary calcination temperature is 550°C and the time is 45 minutes.

[0062] The stirring speed during plastication is 150r / min;

[0063] The stirring speed during the mixing is 300 r / min.

[0064] The polymer rubber sealing product with high-pressure hydrogen permeation resistance includes, by weight: 50 parts of EPDM rubber, 25 parts of natural rubber, 12 parts of nano-composite materials, 1 part of stearic acid, 1 part of antioxidant MB, 1 part of sulfur, and 0.5 part of accelerator DTDM.

[0065] Example 2

[0066] A method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance comprises the following steps:

[0067] S1: adding EPDM rubber and natural rubber to an internal mixer, heating the mixture to 93°C at a heating rate of 3°C / min, and plasticizing for 40 minutes to obtain plasticized rubber;

[0068] S2: adding the plasticized rubber, nanocomposite, stearic acid, antioxidant, vulcanizing agent and accelerator in step S1 to a mixer, heating the mixture to 98°C at a heating rate of 5°C / min, and mixing for 30 minutes to obtain a mixed rubber;

[0069] S3: placing the rubber compound obtained in step S2 on a vulcanizer for pre-vulcanization at 125° C. for 15 minutes, performing thin-pass vulcanization three times, and performing secondary vulcanization at 158° C. for 7 minutes to obtain the obtained product.

[0070] The preparation method of nanocomposite material is as follows:

[0071] Add zinc acetate and lanthanum chloride to ethylene glycol monomethyl ether, adjust the temperature to 60°C, and stir for 30 minutes;

[0072] Then, ethanolamine was added dropwise, and the mixture was stirred and mixed for 2 hours under heat preservation, and allowed to stand for 20 hours to obtain a first reaction solution;

[0073] uniformly dispersing carbon nanotubes in ethylene glycol monomethyl ether to obtain a carbon nanotube dispersion;

[0074] The first reaction liquid is added to the carbon nanotube dispersion liquid, and then ultrasonically dispersed for 10 minutes to obtain a composite dispersion liquid;

[0075] Drying the composite dispersion to a constant weight to obtain a composite material;

[0076] The composite material is subjected to a primary calcination treatment in a furnace, and cooled to room temperature to obtain a calcined material;

[0077] Mix the silicate with anhydrous ethanol, then add deionized water, continue stirring and dispersing for 30 minutes, then add the calcined material, after ultrasonic dispersion, let it stand for 2 hours, then dry to constant weight, finally calcine it twice in a furnace, cool it to room temperature, and obtain a nanocomposite material.

[0078] The molar ratio of zinc acetate to lanthanum chloride is 2:1;

[0079] The mass ratio of zinc acetate to ethylene glycol monomethyl ether and ethanolamine is 1:20:3;

[0080] The mass fraction of the carbon nanotube dispersion is 10%;

[0081] The mixing volume ratio of the first reaction liquid to the carbon nanotube dispersion liquid is 3:1.2.

[0082] The primary calcination temperature is 500°C and the time is 40 minutes.

[0083] The mass ratio of silicate to anhydrous ethanol and deionized water is 1:6:4;

[0084] The mass ratio of the silicate to the calcined material is 1:3;

[0085] The secondary calcination temperature is 550°C and the time is 45 minutes.

[0086] The stirring speed during plastication is 150r / min;

[0087] The stirring speed during the mixing is 300 r / min.

[0088] The polymer rubber sealing product with high-pressure hydrogen permeation resistance includes, by weight: 52 parts of EPDM rubber, 26 parts of natural rubber, 13 parts of nano-composite materials, 1.5 parts of stearic acid, 2 parts of antioxidant MB, 1.2 parts of sulfur, and 0.6 parts of accelerator DTDM.

[0089] Example 3

[0090] A method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance comprises the following steps:

[0091] S1: adding EPDM rubber and natural rubber to an internal mixer, heating the mixture to 94°C at a heating rate of 3°C / min, and plasticizing for 40 minutes to obtain plasticized rubber;

[0092] S2: adding the plasticized rubber, nanocomposite, stearic acid, antioxidant, vulcanizing agent and accelerator in step S1 to a mixer, heating the mixture to 98°C at a heating rate of 5°C / min, and mixing for 35 minutes to obtain a mixed rubber;

[0093] S3: placing the rubber compound obtained in step S2 on a vulcanizer for pre-vulcanization at 124° C. for 15 minutes, performing thin-pass vulcanization three times, and performing secondary vulcanization at 158° C. for 7 minutes to obtain the obtained product.

[0094] The preparation method of nanocomposite material is as follows:

[0095] Add zinc acetate and lanthanum chloride to ethylene glycol monomethyl ether, adjust the temperature to 60°C, and stir for 30 minutes;

[0096] Then, ethanolamine was added dropwise, and the mixture was stirred and mixed for 2 hours under heat preservation, and allowed to stand for 20 hours to obtain a first reaction solution;

[0097] uniformly dispersing carbon nanotubes in ethylene glycol monomethyl ether to obtain a carbon nanotube dispersion;

[0098] The first reaction liquid is added to the carbon nanotube dispersion liquid, and then ultrasonically dispersed for 10 minutes to obtain a composite dispersion liquid;

[0099] Drying the composite dispersion to a constant weight to obtain a composite material;

[0100] The composite material is subjected to a primary calcination treatment in a furnace, and cooled to room temperature to obtain a calcined material;

[0101] Mix the silicate with anhydrous ethanol, then add deionized water, continue stirring and dispersing for 30 minutes, then add the calcined material, after ultrasonic dispersion, let it stand for 2 hours, then dry to constant weight, finally calcine it twice in a furnace, cool it to room temperature, and obtain a nanocomposite material.

[0102] The molar ratio of zinc acetate to lanthanum chloride is 2:1;

[0103] The mass ratio of zinc acetate to ethylene glycol monomethyl ether and ethanolamine is 1:20:3;

[0104] The mass fraction of the carbon nanotube dispersion is 10%;

[0105] The mixing volume ratio of the first reaction liquid to the carbon nanotube dispersion liquid is 3:1.2.

[0106] The primary calcination temperature is 500°C and the time is 40 minutes.

[0107] The mass ratio of silicate to anhydrous ethanol and deionized water is 1:6:4;

[0108] The mass ratio of the silicate to the calcined material is 1:3;

[0109] The secondary calcination temperature is 550°C and the time is 45 minutes.

[0110] The stirring speed during plastication is 150r / min;

[0111] The stirring speed during the mixing is 300 r / min.

[0112] The polymer rubber sealing product with high-pressure hydrogen permeation resistance includes, by weight: 55 parts of EPDM rubber, 27 parts of natural rubber, 14 parts of nano-composite materials, 1.8 parts of stearic acid, 2 parts of antioxidant MB, 1.3 parts of sulfur, and 0.7 parts of accelerator DTDM.

[0113] Example 4

[0114] A method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance comprises the following steps:

[0115] S1: adding EPDM rubber and natural rubber to an internal mixer, heating the mixture to 93°C at a heating rate of 3°C / min, and plasticizing for 40 minutes to obtain plasticized rubber;

[0116] S2: adding the plasticized rubber, nanocomposite, stearic acid, antioxidant, vulcanizing agent and accelerator in step S1 to a mixer, heating the mixture to 98°C at a heating rate of 5°C / min, and mixing for 35 minutes to obtain a mixed rubber;

[0117] S3: placing the rubber compound obtained in step S2 on a vulcanizer for pre-vulcanization at 124° C. for 13 minutes, and then performing thin-pass vulcanization three times and performing secondary vulcanization at 157° C. for 7 minutes to obtain the obtained product.

[0118] The preparation method of nanocomposite material is as follows:

[0119] Add zinc acetate and lanthanum chloride to ethylene glycol monomethyl ether, adjust the temperature to 60°C, and stir for 30 minutes;

[0120] Then, ethanolamine was added dropwise, and the mixture was stirred and mixed for 2 hours under heat preservation, and allowed to stand for 20 hours to obtain a first reaction solution;

[0121] uniformly dispersing carbon nanotubes in ethylene glycol monomethyl ether to obtain a carbon nanotube dispersion;

[0122] The first reaction liquid is added to the carbon nanotube dispersion liquid, and then ultrasonically dispersed for 10 minutes to obtain a composite dispersion liquid;

[0123] Drying the composite dispersion to a constant weight to obtain a composite material;

[0124] The composite material is subjected to a primary calcination treatment in a furnace, and cooled to room temperature to obtain a calcined material;

[0125] Mix the silicate with anhydrous ethanol, then add deionized water, continue stirring and dispersing for 30 minutes, then add the calcined material, after ultrasonic dispersion, let it stand for 2 hours, then dry to constant weight, finally calcine it twice in a furnace, cool it to room temperature, and obtain a nanocomposite material.

[0126] The molar ratio of zinc acetate to lanthanum chloride is 2:1;

[0127] The mass ratio of zinc acetate to ethylene glycol monomethyl ether and ethanolamine is 1:20:3;

[0128] The mass fraction of the carbon nanotube dispersion is 10%;

[0129] The mixing volume ratio of the first reaction liquid to the carbon nanotube dispersion liquid is 3:1.2.

[0130] The primary calcination temperature is 500°C and the time is 40 minutes.

[0131] The mass ratio of silicate to anhydrous ethanol and deionized water is 1:6:4;

[0132] The mass ratio of the silicate to the calcined material is 1:3;

[0133] The secondary calcination temperature is 550°C and the time is 45 minutes.

[0134] The stirring speed during plastication is 150r / min;

[0135] The stirring speed during the mixing is 300 r / min.

[0136] The polymer rubber sealing product with high-pressure hydrogen permeation resistance includes, by weight: 54 parts of EPDM rubber, 26 parts of natural rubber, 14 parts of nano-composite materials, 1.5 parts of stearic acid, 2 parts of antioxidant MB, 1.2 parts of sulfur, and 0.6 parts of accelerator DTDM.

[0137] Example 5

[0138] A method for preparing a polymer rubber sealing product with high-pressure hydrogen permeation resistance comprises the following steps:

[0139] S1: adding EPDM rubber and natural rubber to an internal mixer, heating the mixture to 95°C at a heating rate of 3°C / min, and plasticizing for 40 minutes to obtain plasticized rubber;

[0140] S2: adding the plasticized rubber, nanocomposite, stearic acid, antioxidant, vulcanizing agent and accelerator in step S1 to a mixer, heating the mixture to 98°C at a heating rate of 5°C / min, and mixing for 40 minutes to obtain a mixed rubber;

[0141] S3: placing the rubber compound obtained in step S2 on a vulcanizer for pre-vulcanization at 128° C. for 16 minutes, performing thin-pass vulcanization three times, and performing secondary vulcanization at 160° C. for 8 minutes to obtain the obtained product.

[0142] The preparation method of nanocomposite material is as follows:

[0143] Add zinc acetate and lanthanum chloride to ethylene glycol monomethyl ether, adjust the temperature to 60°C, and stir for 30 minutes;

[0144] Then, ethanolamine was added dropwise, and the mixture was stirred and mixed for 2 hours under heat preservation, and allowed to stand for 20 hours to obtain a first reaction solution;

[0145] uniformly dispersing carbon nanotubes in ethylene glycol monomethyl ether to obtain a carbon nanotube dispersion;

[0146] The first reaction liquid is added to the carbon nanotube dispersion liquid, and then ultrasonically dispersed for 10 minutes to obtain a composite dispersion liquid;

[0147] Drying the composite dispersion to a constant weight to obtain a composite material;

[0148] The composite material is subjected to a primary calcination treatment in a furnace, and cooled to room temperature to obtain a calcined material;

[0149] Mix the silicate with anhydrous ethanol, then add deionized water, continue stirring and dispersing for 30 minutes, then add the calcined material, after ultrasonic dispersion, let it stand for 2 hours, then dry to constant weight, finally calcine it twice in a furnace, cool it to room temperature, and obtain a nanocomposite material.

[0150] The molar ratio of zinc acetate to lanthanum chloride is 2:1;

[0151] The mass ratio of zinc acetate to ethylene glycol monomethyl ether and ethanolamine is 1:20:3;

[0152] The mass fraction of the carbon nanotube dispersion is 10%;

[0153] The mixing volume ratio of the first reaction liquid to the carbon nanotube dispersion liquid is 3:1.5.

[0154] The primary calcination temperature is 500°C and the time is 40 minutes.

[0155] The mass ratio of silicate to anhydrous ethanol and deionized water is 1:6:4;

[0156] The mass ratio of the silicate to the calcined material is 1:3;

[0157] The secondary calcination temperature is 550°C and the time is 45 minutes.

[0158] The stirring speed during plastication is 150r / min;

[0159] The stirring speed during the mixing is 300 r / min.

[0160] The polymer rubber sealing product with high-pressure hydrogen permeation resistance includes, by weight: 60 parts of EPDM rubber, 28 parts of natural rubber, 15 parts of nano-composite materials, 2 parts of stearic acid, 3 parts of antioxidant MB, 1.5 parts of sulfur, and 0.8 parts of accelerator DTDM.

[0161] Comparative Example 1:

[0162] Based on the technical solution of Example 1, no nanocomposite material is added, and the rest of the technical solutions remain unchanged.

[0163] Comparative Example 2

[0164] On the basis of the technical solution of Example 1, the nanocomposite material is replaced with an equal amount of nano zinc oxide, and the rest of the technical solutions remain unchanged.

[0165] test:

[0166] The examples and comparative samples of the same specifications were tested:

[0167] Hardness test: refer to GB / T531.1-2008 standard;

[0168] Table 1

[0169] Shore Hardness A Example 1 90 Example 2 92 Example 3 91 Example 4 90 Example 5 92 Comparative Example 1 78 Comparative Example 2 86

[0170] It can be seen from Table 1 that the polymer rubber sealing product with high-pressure hydrogen permeation resistance prepared by the present invention has a relatively high hardness.

[0171] High-pressure hydrogen permeation resistance test (hydrogen medium, pressure 75MPa, 88℃, 72 hours):

[0172] Table 2 Hardness change

[0173] Hardness change rate % Example 1 -1.88 Example 2 -1.94 Example 3 -1.85 Example 4 -1.90 Example 5 -1.93 Comparative Example 1 -6.67 Comparative Example 2 -4.02

[0174] It can be seen from Table 2 that the hardness of the polymer rubber sealing product prepared by the present invention changes little under high-pressure hydrogen medium, indicating that it has good performance in resisting the influence of high-pressure hydrogen.

[0175] Table 3 Volume changes

[0176] Volume change rate % Example 1 +0.83 Example 2 +0.92 Example 3 +0.78 Example 4 +0.85 Example 5 +0.87 Comparative Example 1 +2.33 Comparative Example 2 +1.54

[0177] It can be seen from Table 3 that the hardness of the polymer rubber sealing product prepared by the present invention changes little under high-pressure hydrogen medium, indicating that it has good resistance to high-pressure hydrogen penetration. The above is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made according to the concept of the present invention, or modified to equivalent embodiments of equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. A method for preparing a polymer rubber sealing product with high pressure hydrogen permeation resistance, It is characterized in that The following steps are involved: S1: adding EPDM rubber and natural rubber to an internal mixer, heating the mixture to 92-95°C at a heating rate of 3°C / min, and plasticizing for 40 minutes to obtain plasticized rubber; S2: adding the plasticized rubber, nanocomposite, stearic acid, antioxidant, vulcanizing agent and accelerator in step S1 to a mixer, heating the mixture to 98°C at a heating rate of 5°C / min, and mixing for 30-40 minutes to obtain a mixed rubber; S3: placing the rubber compound obtained in step S2 on a vulcanizer for pre-vulcanization at 120-128° C. for 12-16 minutes, thin-passing for 3 times, and secondary vulcanization at 155-160° C. for 6-8 minutes to obtain the product.

2. A method for preparing a polymer rubber sealing product with high pressure hydrogen permeation resistance according to claim 1, Features: The preparation method of the nanocomposite material in S2 is: Add zinc acetate and lanthanum chloride to ethylene glycol monomethyl ether, adjust the temperature to 60°C, and stir for 30 minutes; Then, ethanolamine was added dropwise, and the mixture was stirred and mixed for 2 hours under heat preservation, and allowed to stand for 20 hours to obtain a first reaction solution; uniformly dispersing carbon nanotubes in ethylene glycol monomethyl ether to obtain a carbon nanotube dispersion; The first reaction liquid is added to the carbon nanotube dispersion liquid, and then ultrasonically dispersed for 10 minutes to obtain a composite dispersion liquid; Drying the composite dispersion to a constant weight to obtain a composite material; The composite material is subjected to a primary calcination treatment in a furnace, and cooled to room temperature to obtain a calcined material; Mix the silicate with anhydrous ethanol, then add deionized water, continue stirring and dispersing for 30 minutes, then add the calcined material, after ultrasonic dispersion, let it stand for 2 hours, then dry to constant weight, finally calcine it twice in a furnace, cool it to room temperature, and obtain a nanocomposite material.

3. A method for preparing a high-molecular rubber sealing product with high-pressure hydrogen permeation resistance according to claim 2, Features: The molar ratio of zinc acetate to lanthanum chloride is 2:1; The mass ratio of zinc acetate to ethylene glycol monomethyl ether and ethanolamine is 1:20:3; The mass fraction of the carbon nanotube dispersion is 10%; The mixing volume ratio of the first reaction liquid to the carbon nanotube dispersion liquid is 3:1-1.

5.

4. The method for preparing a high molecular rubber sealing product with high pressure hydrogen permeation resistance according to claim 2, Features: The primary calcination temperature is 500° C. and the time is 40 minutes.

5. The method for preparing a high molecular rubber sealing product with high pressure hydrogen permeation resistance according to claim 2, Features: The mass ratio of the silicate to anhydrous ethanol and deionized water is 1:6:4; The mass ratio of the silicate to the calcined material is 1:3; The secondary calcination temperature is 550°C and the time is 45 minutes.

6. The method for preparing a high molecular rubber sealing product with high pressure hydrogen permeation resistance according to claim 1, Features: The stirring speed during the plasticizing is 150r / min; The stirring speed during the mixing is 300 r / min.

7. The method for preparing a high molecular rubber sealing product with high pressure hydrogen permeation resistance according to claim 1, Features: The polymer rubber sealing product with high-pressure hydrogen permeation resistance comprises, by weight: 50-60 parts of EPDM rubber, 25-28 parts of natural rubber, 12-15 parts of nano-composite material, 1-2 parts of stearic acid, 1-3 parts of antioxidant, 1-1.5 parts of vulcanizing agent, and 0.5-0.8 parts of accelerator.

8. The method for preparing a high-molecular rubber sealing product with high-pressure hydrogen permeation resistance according to claim 7, Features: The antioxidant is antioxidant MB.

9. The method for preparing a high molecular rubber sealing product with high pressure hydrogen permeation resistance according to claim 1, Features: The vulcanizing agent is sulfur.

10. The method for preparing a high molecular rubber sealing product with high pressure hydrogen permeation resistance according to claim 1, It is characterized in that The accelerator is DTDM.

Citation Information

Patent Citations

  • Cyclopentadiene-modified carbon nanotube / rubber composite material and preparation method thereof

    CN104650400A

  • Oxide nanosheet as well as preparation method and composite catalyst thereof

    CN108355632A

  • Preparation method for wear-resistant damping ethylene propylene rubber seal ring

    CN109401079A

  • High-pressure-hydrogen-permeation-resistant rubber material and preparation method thereof

    CN113861571A

  • Gas sealing member for high-pressure hydrogen plant and high-pressure hydrogen plant

    CN115151752A