Preparation and application of reinforced composite polyolefin material with corrosion resistance and high stability

Through modified polyolefin materials and fiber reinforcement, the temperature limitation and mechanical strength problems of polyolefin in the gas meter movement are solved, and the high temperature resistance, corrosion resistance and mechanical properties are improved, making it suitable for harsh application scenarios.

CN118725495AInactive Publication Date: 2024-10-01HANGZHOU YICAI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105426.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyolefin materials have problems such as temperature restrictions, poor solvent resistance and low mechanical strength in gas meter movement applications, which affect their performance stability in extreme environments.

Method used

Modified polyolefin material is used, and the chemical resistance, thermal stability and mechanical properties of the material are improved by surface treatment of a blend of polytetrafluoroethylene and hexafluoropropylene, adding glass fiber and carbon fiber, and optimizing the formula and process.

Benefits of technology

It significantly improves the high temperature resistance, corrosion resistance and mechanical strength of the composite material, is suitable for high temperature and high pressure environments, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses preparation and application of a corrosion-resistant high-stability reinforced composite polyolefin material, and belongs to the technical field of polyolefin materials. The composite polyolefin material comprises modified polyolefin, modified carbon fibers, glass fibers, a filler, an antioxidant, a coupling agent, a lubricant and a weather-resistant agent, the modified polyolefin is obtained by reacting polyolefin, polytetrafluoroethylene subjected to surface treatment and hexafluoropropylene, and the mass ratio of the polyolefin to the polytetrafluoroethylene subjected to surface treatment to the hexafluoropropylene is (5-8): (2-4): 1; the modified carbon fiber is carbon fiber modified by nano silicon dioxide. By adopting the preparation and application of the corrosion-resistant high-stability reinforced composite polyolefin material, the composite polyolefin material realizes comprehensive improvement of corrosion resistance, high temperature resistance, solvent resistance and excellent mechanical properties by optimizing a formula and a process; and the material is very suitable for application scenarios with strict requirements on material performance, such as gas meter movement components and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyolefin materials, and in particular relates to the preparation and application of a corrosion-resistant and highly stable reinforced composite polyolefin material. Background Art

[0002] A gas meter is an instrument used to measure and record the volume or mass of gas transported through a pipeline. It is mainly used for civil and industrial purposes to measure the consumption of gas. Gas meters are widely used, mainly including family homes, commercial places, chemical plants, food processing plants, etc. The gas meter movement is the core component of the gas meter, which is responsible for accurately measuring the volume of gas passing through the gas meter. The gas meter movement includes key components such as diaphragms, distribution valves, metering chambers, transmission mechanisms, counters, filters, pressure regulators and impellers.

[0003] At present, polymers that can be used in gas meter cores need to have good mechanical properties, chemical stability and durability in order to maintain stable functions in long-term gas environments. The polymers used in the core of gas meters are mainly polyoxymethylene, polybutylene terephthalate, etc. Compared with metal materials, polyolefins have a lower density, which helps to reduce the overall weight of the gas meter and facilitates installation and transportation. Polyolefins are easy to process into complex shapes through injection molding, extrusion and other processes, which is convenient for manufacturing precise core parts. For smart gas meters, the electrical insulation of polyolefins can prevent short circuits and electrical interference, ensuring the normal operation of electronic components.

[0004] Although polyolefins have many advantages in gas meter movement applications, they also have some potential disadvantages that limit their applicability under certain conditions. The specific disadvantages are as follows: (1) Temperature limitation: Polyolefins have limited thermal stability. Although they can maintain their performance within a certain temperature range, extreme high or low temperatures will affect their mechanical properties and dimensional stability.

[0005] (2) Solvent resistance: Although polyolefins have good resistance to many chemicals, they may still be damaged by certain organic solvents or strong acids and alkalis, especially in the case of long-term contact.

[0006] (3) Mechanical strength and hardness: Compared with metals, polyolefins have lower mechanical strength and hardness, which means that polyolefin parts are more likely to deform or be damaged under high pressure or high stress environments. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing and applying a corrosion-resistant and highly stable reinforced composite polyolefin material, so as to solve the problem of poor temperature resistance, solvent resistance and mechanical strength of the above-mentioned polyolefin material after being applied to the core components of a gas meter.

[0008] To achieve the above object, the first aspect of the present invention provides a corrosion-resistant and highly stable reinforced composite polyolefin material, which comprises the following raw materials in parts by mass: Modified polyolefin 100~150 parts Modified carbon fiber 10~20 parts Glass fiber 20~30 parts Filler 10~15 parts Antioxidant 1~10 parts Coupling agent 1~10 parts Lubricant 1~10 parts Weathering agent 1~10 parts The modified polyolefin is obtained by reacting polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene, and the mass ratio of polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene is (5-8): (2-4): 1; The modified carbon fiber is carbon fiber modified by nano-silicon dioxide.

[0009] Preferably, the polyolefin comprises high-density polyethylene and polypropylene, and the mass ratio of high-density polyethylene to polypropylene is (2-4):1; The preparation method of modified polyolefin is: The polytetrafluoroethylene is placed in a plasma device, evacuated to a vacuum degree of less than 3 Pa, and a mixed gas of argon and oxygen is introduced, wherein the volume ratio of argon and oxygen is 1:1, and then a current and a voltage are applied to plasmaize the mixed gas to treat the polytetrafluoroethylene, wherein the treatment power is 100-150 W and the treatment time is 1-5 minutes, thereby obtaining the polytetrafluoroethylene after surface treatment; The polyolefin, the surface treated polytetrafluoroethylene and hexafluoropropylene are blended, melt-extruded at 250-300°C, cooled and pelletized to obtain the modified polyolefin.

[0010] Polyolefin materials have a wide range of performance advantages, such as low density and light weight of polyolefins. Polyolefin materials are easy to process and can be processed by various molding methods such as injection molding, blow molding, and extrusion. They are suitable for large-scale production, have short molding cycles, high production efficiency, and low costs. Polyolefin materials can also be recycled, which helps reduce waste. Although polyolefin materials have the above advantages, due to the singleness of the material, their comprehensive performance is reduced. In actual application, different application scenarios usually have different requirements for various properties of the material. In order to improve the comprehensive performance of the material such as high temperature resistance and corrosion resistance, the present invention modifies the polyolefin material, mixes the polyolefin material with polytetrafluoroethylene and hexafluoropropylene, and the addition of polytetrafluoroethylene and hexafluoropropylene significantly improves the chemical resistance and high temperature resistance of the composite material, which is convenient for adapting to environmental changes.

[0011] The present invention has been further developed and found that polytetrafluoroethylene has stable physical and chemical properties and is not easy to participate in chemical reactions, resulting in poor compatibility and reactivity with polyolefins and hexafluoropropylene. To address this problem, polytetrafluoroethylene is subjected to plasma surface treatment to destroy some CF bonds on its surface and form active points such as C=C double bonds or C≡C triple bonds. Free radical polymerization can be carried out using these active points, thereby increasing the reactivity with polyolefins and hexafluoropropylene.

[0012] Preferably, the outer diameter of the glass fiber is 5 μm-8 μm, and the aspect ratio is 80-100, the outer diameter of the carbon fiber is 0.5 μm-2 μm, and the aspect ratio is 500-800, and the ratio of the aspect ratio of the glass fiber to the aspect ratio of the carbon fiber is 1:(8-10).

[0013] The present invention adds glass fiber and carbon fiber as reinforcing materials to polyolefin materials, which can significantly improve the performance of the composite material, especially the mechanical stability and durability. The aspect ratio of the glass fiber is 80-100, which can effectively transfer the load, enhance the rigidity and bending strength of the composite material, and the glass fiber with an outer diameter of 5μm-8μm can be evenly dispersed in the matrix, reduce stress concentration, and improve the overall strength. The aspect ratio of the carbon fiber is as high as 500-800, and the outer diameter is 0.5μm-2μm, which can provide extremely high tensile strength and elastic modulus, significantly enhance the tensile performance of the composite material, and the outer diameter of the carbon fiber helps to form a denser network in the matrix, further enhancing the mechanical properties of the material. The aspect ratio of the glass fiber and the carbon fiber of the present invention is 1: (8-10), and this ratio can ensure the synergistic effect of the two, not only utilizing the high rigidity and dimensional stability of the glass fiber, but also giving play to the high strength and light weight characteristics of the carbon fiber, thereby forming a balanced mechanical performance system in the composite material. The present invention can further optimize the anisotropic properties of the composite material by finely controlling the distribution and orientation of the fibers to meet the requirements of specific applications.

[0014] Preferably, the preparation method of the modified carbon fiber is: 200-250 g of ethyl orthosilicate, 30-40 g of water and 5-15 g of glycerol were mixed, hydrochloric acid was added to adjust the pH value to 3, and after stirring for 1-3 hours, 30-40 g of a 5-8% polyvinyl alcohol aqueous solution was added, and stirring was continued for 1-3 hours, and then a silica precursor solution was obtained by filtration; The carbon fiber was soaked in acetone for 1 to 5 minutes, washed with deionized water, dried, and then soaked in a silica precursor solution for 5 to 20 minutes. Ultrasonic vibration of 30 to 50 kHz was used during the soaking process. After the soaking was completed, the carbon fiber was taken out and dried at room temperature for 10 to 30 minutes to obtain a pretreated carbon fiber. The pretreated carbon fiber is heated to 180-220°C at a rate of 4°C / min and kept at a constant temperature for 20-40 minutes, then heated to 450-550°C at a rate of 4°C / min and kept at a constant temperature for 60-90 minutes before being naturally cooled. The whole process is carried out under argon protection to obtain silica-modified carbon fiber.

[0015] Preferably, the inorganic filler includes one or more of calcium carbonate, talc, kaolin, barium sulfate, and glass microspheres; The antioxidant includes one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tris(2,4-di-tert-butylphenyl) phosphite or di-octadecyl thiodipropionate.

[0016] Preferably, the coupling agent includes one or more of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, and a borate coupling agent.

[0017] Preferably, the lubricant includes one or both of calcium stearate and N,N'-ethylene bisstearamide.

[0018] Preferably, the weathering agent includes one or more of hydroxybenzophenone light stabilizers, hydroxybenzotriazole light stabilizers, and hindered amine light stabilizers.

[0019] The second aspect of the present invention provides a method for preparing a corrosion-resistant and highly stable reinforced composite polyolefin material, comprising the following steps: (1) Put modified polyolefin, modified carbon fiber, glass fiber, filler, antioxidant, coupling agent, lubricant and weathering agent into a mixer according to proportion and mix them evenly to obtain a mixture; (2) The mixed material is fed into a twin-screw extruder through a feeder, sheared and mixed by the twin-screw extruder, extruded from a die, drawn into strips, air-cooled, pelletized, and dried to obtain a composite polyolefin material. The temperature of the twin-screw extruder is 260-300°C.

[0020] The third aspect of the present invention provides an application of a corrosion-resistant and highly stable reinforced composite polyolefin material, and an application of the composite polyolefin material in a core component of a gas meter.

[0021] Therefore, the present invention adopts the above-mentioned structure to prepare and apply a corrosion-resistant, highly stable reinforced composite polyolefin material, which has the following beneficial effects: (1) The modified polyolefin of the present invention comprises a polyolefin matrix, surface-treated polytetrafluoroethylene and hexafluoropropylene, which enhance the chemical corrosion resistance of the material and enable the material to resist corrosion from a variety of chemical media. The addition of polytetrafluoroethylene and hexafluoropropylene can also improve the thermal stability of the composite material, enabling the material to maintain its physical and chemical properties at higher temperatures, making the material suitable for high-temperature environments, such as the temperature changes that may be encountered inside a gas meter.

[0022] (2) The present invention contains two substances, glass fiber and modified carbon fiber. The addition of these reinforcing fibers significantly improves the mechanical strength, rigidity and wear resistance of the composite material. The high strength and high modulus of carbon fiber and the high rigidity and low moisture absorption of glass fiber work together to enable the composite material to have excellent impact resistance, flexural strength and dimensional stability.

[0023] (3) The composite polyolefin material of the present invention achieves comprehensive improvement in corrosion resistance, high temperature resistance, solvent resistance and excellent mechanical properties by optimizing the formula and process, and is very suitable for application scenarios with strict requirements on material properties, such as gas meter core components.

[0024] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0025] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment. Example

[0026] This embodiment provides a corrosion-resistant and highly stable reinforced composite polyolefin material, which includes the following raw materials in parts by mass: Modified polyolefin 120 parts Modified carbon fiber 12 parts Glass fiber 20 parts Filling 10 parts 2 parts antioxidant 5 parts of coupling agent 3 parts lubricant 2 parts of weathering agent The modified polyolefin is obtained by reacting polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene, and the mass ratio of polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene is 6:2:1; Polytetrafluoroethylene was purchased from 3M China Co., Ltd., model 1610.

[0027] The modified carbon fiber is carbon fiber modified by nano-silicon dioxide.

[0028] The outer diameter of the glass fiber is 6 μm, and the aspect ratio is 80; the outer diameter of the carbon fiber is 1 μm, and the aspect ratio is 640; the ratio of the aspect ratio of the glass fiber to the aspect ratio of the carbon fiber is 1:8.

[0029] The inorganic filler is calcium carbonate and talcum powder, wherein the mass ratio of calcium carbonate to talcum powder is 1:1.

[0030] The antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0031] The coupling agent is silane coupling agent KH550.

[0032] The lubricant is calcium stearate.

[0033] The weathering agent is a hydroxybenzophenone light stabilizer, and the hydroxybenzophenone light stabilizer is specifically 2,4-dihydroxybenzophenone.

[0034] The polyolefin includes high-density polyethylene and polypropylene, and the mass ratio of high-density polyethylene to polypropylene is 3:1; the high-density polyethylene is purchased from Sinopec Qilu Petrochemical Company, model DGDA6098, and the polypropylene is purchased from Dongguan Hongshao New Materials Co., Ltd., model BJ356MO.

[0035] The preparation method of modified polyolefin is: The polytetrafluoroethylene is placed in a plasma device, evacuated to a vacuum degree of less than 3 Pa, and a mixed gas of argon and oxygen is introduced, wherein the volume ratio of argon and oxygen is 1:1, and then a current and a voltage are applied to plasma-form the mixed gas to treat the polytetrafluoroethylene, wherein the treatment power is 120 W and the treatment time is 2 minutes, thereby obtaining the polytetrafluoroethylene after surface treatment; The polyolefin, the surface treated polytetrafluoroethylene and hexafluoropropylene are blended, melt-extruded at 270°C, cooled and pelletized to obtain the modified polyolefin.

[0036] The preparation method of modified carbon fiber is: 210 g of tetraethyl orthosilicate, 35 g of water and 10 g of glycerol were mixed, hydrochloric acid was added to adjust the pH value to 3, and after stirring for 1 hour, 32 g of a 5% polyvinyl alcohol aqueous solution was added, and stirring was continued for 2 hours, and then a silica precursor solution was obtained by filtration; The carbon fiber was soaked in acetone for 2 minutes, washed with deionized water, dried, and then soaked in a silica precursor solution for 15 minutes. 40kHz ultrasonic vibration was used during the soaking process. After the soaking was completed, the carbon fiber was taken out and dried at room temperature for 20 minutes to obtain a pretreated carbon fiber. The pretreated carbon fiber was heated to 200°C at a rate of 4°C / min and kept at a constant temperature for 30 minutes, then heated to 500°C at a rate of 4°C / min and kept at a constant temperature for 80 minutes before being naturally cooled. The entire process was carried out under argon protection to obtain silica-modified carbon fiber.

[0037] This embodiment also provides a method for preparing a corrosion-resistant and highly stable reinforced composite polyolefin material, comprising the following steps: (1) Put modified polyolefin, modified carbon fiber, glass fiber, filler, antioxidant, coupling agent, lubricant and weathering agent into a mixer according to proportion and mix them evenly to obtain a mixture; (2) The mixed material is fed into a twin-screw extruder through a feeder, sheared and mixed by the twin-screw extruder, extruded from a die, drawn into strips, air-cooled, pelletized, and dried to obtain a composite polyolefin material. The temperature of the twin-screw extruder is 300°C. Example

[0038] The difference from Example 1 is that the formula composition of the composite polyolefin material is different.

[0039] The composite polyolefin material of this embodiment includes the following raw materials in parts by mass: Modified polyolefin 135 parts Modified carbon fiber 15 parts Glass fiber 20 parts 14 parts of filler 5 parts antioxidant 3 parts of coupling agent 5 parts of lubricant 4 parts of weathering agent.

[0040] Comparative Example 1 The difference from Example 1 is that the surface-treated polytetrafluoroethylene in the modified polyolefin is replaced by pure polytetrafluoroethylene.

[0041] Comparative Example 2 The difference from Example 1 is that the high-density polyethylene in the polyolefin is replaced by low-density polyethylene, and the low-density polyethylene is purchased from PetroChina Dushanzi Petrochemical Company, with a model number of LL0209AA.

[0042] Comparative Example 3 The difference from Example 1 is that the mass ratio of high-density polyethylene to polypropylene is 3:2.

[0043] Comparative Example 4 The difference from Example 1 is that hexafluoropropylene is not added to the modified polyolefin, and the hexafluoropropylene is replaced by a polyolefin of equal mass.

[0044] Comparative Example 5 The difference from Example 1 is that the mass ratio of the polyolefin, the surface-treated polytetrafluoroethylene and the hexafluoropropylene in the modified polyolefin is 12:2:1.

[0045] Comparative Example 6 The difference from Example 1 is that the polyolefin in the modified polyolefin, the surface-treated polytetrafluoroethylene and hexafluoropropylene are directly put into the preparation process of the composite polyolefin material according to proportion, and the preparation process of the modified polyolefin is not carried out.

[0046] Comparative Example 7 The difference from Example 1 is that the modified carbon fiber is not modified with silica, and the carbon fiber is directly put into the preparation process of the composite polyolefin material according to proportion.

[0047] Comparative Example 8 The difference from Example 1 is that the aspect ratio of the carbon fiber is 1000, and the ratio of the aspect ratio of the glass fiber to the aspect ratio of the carbon fiber is 1:12.5.

[0048] Comparative Example 9 The difference from Example 1 is that: glass fiber is not added to the composite polyolefin material, and the glass fiber is replaced by modified carbon fiber of the same mass.

[0049] Test example (1) The composite olefin material particles obtained in Examples 1-2 and Comparative Examples 1-9 were dried, made into test specimens in an injection molding machine, and subjected to mechanical property tests. The test results are shown in Table 1.

[0050] in: Tensile strength: Tested in accordance with GB-T 1447-2005 Test method for tensile properties of fiber reinforced plastics.

[0051] Bending strength: Tested in accordance with GBT 1449-2005-Test method for bending properties of fiber reinforced plastics.

[0052] Impact strength: Tested in accordance with GB / T 1451-2005 Test method for simply supported beam impact toughness of fiber reinforced plastics.

[0053] Table 1 Mechanical properties test results Group Tensile strength / MPa Bending strength / MPa <![CDATA[Notched impact strength of simply supported beam / kJ / m 2 > Example 1 138 175 9.5 Example 2 122 173 8.9 Comparative Example 1 80 99 5.5 Comparative Example 2 70 95 4.8 Comparative Example 3 101 115 6.0 Comparative Example 4 68 97 6.5 Comparative Example 5 92 100 6.3 Comparative Example 6 62 93 4.6 Comparative Example 7 69 90 5.0 Comparative Example 8 75 98 5.4 Comparative Example 9 63 94 4.6 It can be seen from Table 1 that the composite polyolefin materials prepared in Examples 1 to 2 have high tensile strength, flexural strength and impact strength, and excellent mechanical properties, among which Example 1 has the best mechanical properties. This is because the modified polyolefin is used in the present invention, which contains three raw materials, and the raw materials have a synergistic effect, which can improve the mechanical properties of the composite polyolefin material.

[0054] The comparative examples did not adopt the technical solution of the present invention. In comparative example 1, polytetrafluoroethylene was used, and the polytetrafluoroethylene was not surface modified. Due to the high chemical stability of polytetrafluoroethylene, its reactivity with other raw materials polyolefin and hexafluoropropylene deteriorated, resulting in a decrease in the mechanical properties of the composite polyolefin material finally prepared. In comparative example 2, high-density polyethylene was replaced with low-density polyethylene. Most low-density polyethylenes have a linear structure and poor tensile strength. Its application in composite polyolefin materials leads to a decrease in its mechanical properties. In comparative example 3, the addition ratio of polyethylene and polypropylene in polyolefin was changed, resulting in a decrease in mechanical properties. This shows that the polyethylene and polypropylene in the present invention can only be mixed with other raw materials in a specific ratio, thereby fully improving the performance of the composite material. In comparative example 4, hexafluoropropylene was removed from the modified polyolefin, and polyolefin was used instead of hexafluoropropylene. The mechanical properties of the prepared composite material decreased, indicating that the polyolefin in the modified polyolefin of the present invention, the surface-modified polytetrafluoroethylene and hexafluoropropylene have a synergistic effect, and can be used together to improve the mechanical properties of the composite material. In Comparative Example 5, the ratio of raw materials in the modified polyolefin is changed, and the amount of polyolefin added is increased, which leads to a decrease in the mechanical properties of the composite material, further illustrating the synergistic effect of polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene in the modified polyolefin of the present invention. In Comparative Example 6, the raw materials in the modified polyolefin are directly added to the preparation process of the composite material, and the preparation of the modified polyolefin is not performed, which also leads to the deterioration of the mechanical properties of the composite polyolefin material. This shows that in the preparation process of the modified polyolefin, the polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene form a whole, interact with each other, and play a role in improving the mechanical properties in the composite material. In Comparative Example 7, the carbon fiber is not modified with silicon dioxide, the interface bonding between the carbon fiber and the polyolefin matrix is ​​deteriorated, and the mechanical properties of the composite material are reduced. Comparative Example 8 changes the aspect ratio of the carbon fiber, which leads to a change in the ratio of the aspect ratio of the glass fiber and the aspect ratio of the carbon fiber, destroys the balance between the glass fiber and the carbon fiber, and leads to the deterioration of the mechanical properties of the composite polyolefin material. In Comparative Example 9, no glass fiber was added, which also resulted in poor mechanical properties of the composite polyolefin material, indicating that the carbon fiber and glass fiber in the present invention have a synergistic effect and can increase the mechanical properties of the composite material.

[0055] (2) The composite olefin material particles obtained in Examples 1-2 and Comparative Examples 1-9 were dried and made into test specimens in an injection molding machine. The test specimens were placed in a heat aging box for artificial accelerated hot air aging at 85° C. for 96 hours. The aging resistance was measured by the mechanical property retention rate after aging. The larger the retention rate value, the better the aging resistance. The test results are shown in Table 2.

[0056] Tensile strength retention rate after aging = tensile strength after aging / tensile strength before aging × 100%. The calculation method of the flexural strength retention rate after aging and the impact strength retention rate after aging is the same as the calculation method of the tensile strength retention rate after aging.

[0057] Table 2 Aging resistance test results Group Tensile strength retention rate / % Bending strength retention rate / % Impact strength retention rate / % Example 1 96 95 93 Example 2 93 91 90 Comparative Example 1 80 79 78 Comparative Example 2 75 73 70 Comparative Example 3 85 80 82 Comparative Example 4 71 68 73 Comparative Example 5 82 83 80 Comparative Example 6 68 65 71 Comparative Example 7 72 75 69 Comparative Example 8 69 65 70 Comparative Example 9 78 75 71 It can be seen from Table 2 that after the aging resistance test, the composite polyolefin materials prepared in Examples 1 to 2 can maintain their mechanical properties, indicating that they have high temperature resistance, while the composite materials prepared in Comparative Examples 1 to 9 have different degrees of decline in mechanical properties after the aging resistance test, indicating that the composite polyolefin materials in the present invention can not only improve the mechanical properties, but also ensure the high temperature resistance of the material, thereby expanding the scope of use of the material.

[0058] (3) The composite olefin material particles obtained in Examples 1-2 and Comparative Examples 1-9 were dried and made into test specimens in an injection molding machine. The test specimens were immersed in acetone solvent and trichloroethane solvent for 16 hours, with the volume ratio of acetone to trichloroethane being 1:1, dried, and subjected to mechanical property testing. The solvent resistance was measured by the mechanical property retention rate. The test results are shown in Table 3.

[0059] Table 3 Solvent resistance test results Group Tensile strength retention rate / % Bending strength retention rate / % Impact strength retention rate / % Example 1 92 94 95 Example 2 91 93 90 Comparative Example 1 82 80 79 Comparative Example 2 78 74 75 Comparative Example 3 82 85 81 Comparative Example 4 72 73 76 Comparative Example 5 80 79 85 Comparative Example 6 70 68 73 Comparative Example 7 73 77 75 Comparative Example 8 74 68 72 Comparative Example 9 81 85 79 It can be seen from Table 3 that after being soaked in solvent, the composite polyolefin materials prepared in Examples 1 to 2 can maintain their mechanical properties, indicating that they are solvent-resistant, while the mechanical properties of the composite materials prepared in Comparative Examples 1 to 9 all decrease to varying degrees after being soaked in solvent, indicating that the composite polyolefin materials in the present invention can not only improve the mechanical properties, but also ensure the solvent resistance of the material, thereby expanding the scope of use of the material.

[0060] (4) The composite olefin material particles obtained in Examples 1-2 and Comparative Examples 1-9 were dried and made into test specimens in an injection molding machine. The alkali resistance and acid resistance tensile strength retention rate tests of the test specimens were conducted according to the GB / T20102-2006 method. The alkali resistance test conditions were: 5.0% NaOH, 30±2°C erosion for 96 hours; the acid resistance test conditions were: 10% H2SO4, 30±2°C erosion for 96 hours. After the test was completed, the mechanical properties test was conducted, and the acid and alkali resistance was measured by the tensile strength retention rate. The test results are shown in Table 4.

[0061] Table 4 Acid and alkali resistance test results Group Acid-resistant tensile strength retention rate / % Alkali-resistant tensile strength retention rate / % Example 1 95 93 Example 2 90 92 Comparative Example 1 79 75 Comparative Example 2 70 73 Comparative Example 3 80 82 Comparative Example 4 75 76 Comparative Example 5 83 80 Comparative Example 6 72 70 Comparative Example 7 76 73 Comparative Example 8 80 72 Comparative Example 9 83 81 It can be seen from Table 4 that after the acid and alkali resistance test, the composite polyolefin materials prepared in Examples 1 to 2 can maintain their mechanical properties, indicating that they are resistant to acid and alkali, while the mechanical properties of the composite materials prepared in Comparative Examples 1 to 9 have decreased to varying degrees after the acid and alkali resistance test, indicating that the composite polyolefin material in the present invention can not only improve the mechanical properties, but also ensure the acid and alkali resistance of the material, thereby expanding the scope of use of the material.

[0062] Therefore, the present invention adopts the above-mentioned structure to prepare and apply a corrosion-resistant and highly stable reinforced composite polyolefin material. The composite polyolefin material achieves comprehensive improvement in corrosion resistance, high temperature resistance, solvent resistance and excellent mechanical properties by optimizing the formula and process. It is very suitable for application scenarios such as gas meter core components that have strict requirements on material properties.

[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A corrosion-resistant and highly stable reinforced composite polyolefin material, characterized in that: The following raw materials are included in parts by mass: Modified polyolefin 100~150 parts Modified carbon fiber 10~20 parts Glass fiber 20~30 parts Filler 10~15 parts Antioxidant 1~10 parts Coupling agent 1~10 parts Lubricant 1~10 parts Weathering agent 1~10 parts The modified polyolefin is obtained by reacting polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene, and the mass ratio of polyolefin, surface-treated polytetrafluoroethylene and hexafluoropropylene is (5-8): (2-4): 1; The modified carbon fiber is carbon fiber modified by nano-silicon dioxide.

2. The corrosion-resistant and highly stable reinforced composite polyolefin material according to claim 1, characterized in that: Polyolefins include high-density polyethylene and polypropylene, and the mass ratio of high-density polyethylene to polypropylene is (2~4):1; The preparation method of modified polyolefin is: The polytetrafluoroethylene is placed in a plasma device, evacuated to a vacuum degree of less than 3 Pa, and a mixed gas of argon and oxygen is introduced, wherein the volume ratio of argon and oxygen is 1:1, and then a current and a voltage are applied to plasmaize the mixed gas to treat the polytetrafluoroethylene, wherein the treatment power is 100-150 W and the treatment time is 1-5 minutes, thereby obtaining the polytetrafluoroethylene after surface treatment; The polyolefin, the surface treated polytetrafluoroethylene and hexafluoropropylene are blended, melt-extruded at 250-300°C, cooled and pelletized to obtain the modified polyolefin.

3. The corrosion-resistant and highly stable reinforced composite polyolefin material according to claim 1, characterized in that: The outer diameter of glass fiber is 5μm~8μm, and the aspect ratio is 80~100. The outer diameter of carbon fiber is 0.5μm~2μm, and the aspect ratio is 500~800. The ratio of the aspect ratio of glass fiber to that of carbon fiber is 1:(8~10).

4. The corrosion-resistant and highly stable reinforced composite polyolefin material according to claim 1, characterized in that: The preparation method of modified carbon fiber is: 200-250 g of ethyl orthosilicate, 30-40 g of water and 5-15 g of glycerol were mixed, hydrochloric acid was added to adjust the pH value to 3, and after stirring for 1-3 hours, 30-40 g of a 5-8% polyvinyl alcohol aqueous solution was added, and stirring was continued for 1-3 hours, and then a silica precursor solution was obtained by filtration; The carbon fiber was soaked in acetone for 1 to 5 minutes, washed with deionized water, dried, and then soaked in a silica precursor solution for 5 to 20 minutes. Ultrasonic vibration of 30 to 50 kHz was used during the soaking process. After the soaking was completed, the carbon fiber was taken out and dried at room temperature for 10 to 30 minutes to obtain a pretreated carbon fiber. The pretreated carbon fiber is heated to 180-220°C at a rate of 4°C / min and kept at a constant temperature for 20-40 minutes, then heated to 450-550°C at a rate of 4°C / min and kept at a constant temperature for 60-90 minutes before being naturally cooled. The whole process is carried out under argon protection to obtain silica-modified carbon fiber.

5. The corrosion-resistant and highly stable reinforced composite polyolefin material according to claim 1, characterized in that: The inorganic filler includes one or more of calcium carbonate, talc, kaolin, barium sulfate, and glass microspheres; The antioxidant includes one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tris(2,4-di-tert-butylphenyl) phosphite or di-octadecyl thiodipropionate.

6. The corrosion-resistant and highly stable reinforced composite polyolefin material according to claim 1, characterized in that: The coupling agent includes one or more of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, and a borate coupling agent.

7. The corrosion-resistant and highly stable reinforced composite polyolefin material according to claim 1, characterized in that: The lubricant includes one or both of calcium stearate and N,N'-ethylene bisstearamide.

8. The corrosion-resistant and highly stable reinforced composite polyolefin material according to claim 1, characterized in that: The weathering agent includes one or more of hydroxybenzophenone light stabilizers, hydroxybenzotriazole light stabilizers, and hindered amine light stabilizers.

9. The method for preparing a corrosion-resistant and highly stable reinforced composite polyolefin material according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Put modified polyolefin, modified carbon fiber, glass fiber, filler, antioxidant, coupling agent, lubricant and weathering agent into a mixer according to proportion and mix them evenly to obtain a mixture; (2) The mixed material is fed into a twin-screw extruder through a feeder, sheared and mixed by the twin-screw extruder, extruded from a die, drawn into strips, air-cooled, pelletized, and dried to obtain a composite polyolefin material. The temperature of the twin-screw extruder is 260-300°C.

10. An application of a corrosion-resistant and highly stable reinforced composite polyolefin material according to any one of claims 1 to 8, characterized in that: Application of composite polyolefin materials in gas meter core components.