Chip-level underfill adhesive suitable for 2.5 D heterogeneous integrated packaging and preparation method thereof

Through the combination of self-synthetic silicone epoxy resin and epoxy resin and the use of silane coupling agent and spherical silica, the reliability of chip-level underfill in 2.5D heterogeneous integrated packaging under high temperature and high humidity conditions is solved. It solves the problem of deficiencies, achieves high glass transition temperature and excellent bonding strength, and meets the needs of high interconnection density and high energy consumption environment.

CN118725797APending Publication Date: 2024-10-01DEBANG (KUNSHAN) MATERIAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411008098.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The high process temperature and stacking technology of 2.5D heterogeneous integrated packaging lead to internal heat accumulation. Chip-level underfill glue needs to have a higher glass transition temperature and bonding strength to cope with the problem of thermal expansion coefficient mismatch. Traditional filler glue is used in Insufficient reliability under high temperature and high humidity conditions can easily lead to chip warping and filler delamination.

Method used

Self-synthetic silicone epoxy resin A is used with different types of epoxy resin B, combined with silane coupling agent, black paste and spherical silica filler, to prepare chip-level underfill glue through specific synthesis paths and process steps, improving Its glass transition temperature, bonding strength and flow properties.

Benefits of technology

It achieves high reliability and excellent bonding strength under high temperature, high temperature and high humidity conditions, reduces stress caused by thermal expansion coefficient mismatch, meets the high interconnect density and high energy consumption environment requirements of 2.5D heterogeneous integrated packaging, and ensures Overall performance of chip-level underfill.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725797A_ABST
    Figure CN118725797A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of adhesives, and discloses a chip-scale bottom filling adhesive suitable for 2.5 D heterogeneous integrated packaging and a preparation method of the chip-scale bottom filling adhesive, and the filling adhesive comprises the following components in parts by weight: 10-15 parts of self-synthesized organosilicon epoxy resin A, 35-40 parts of epoxy resin, 3-6 parts of a coupling agent, 2-4 parts of black paste, 55-65 parts of filler and 25-35 parts of a curing agent. Compared with the traditional 2D packaged chip-level underfill adhesive, the product provided by the invention has a higher glass transition temperature; the adhesive has rigidity and toughness, and still has excellent bonding strength to silicon wafers at 260 DEG C after being placed in a Uhast environment box for 96 hours; in addition, the product also has the characteristics of excellent flowing property, low CTE and good heat resistance, and can fully meet the operability and reliability requirements of 2.5 D heterogeneous integrated packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of adhesives, and in particular relates to a chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging and a preparation method thereof. Background Art

[0002] In recent years, driven by the demand for new electronic products with smaller size, lower power consumption and better performance, 2.5D heterogeneous integrated packaging has attracted more and more attention from academia and industry. With the development of advanced wafer manufacturing processes, the wafer size has reached 3 nanometers, the characteristic size of transistors has been decreasing, and the density of transistors on chips has been increasing. Innovation in packaging and interconnection technology is no longer just about reducing the size of transistors, but effectively utilizing three-dimensional space to support the continued growth of chip functional density. System-in-package technology can integrate multiple chips into one package by stacking the area, improving product functions while reducing packaging costs, becoming the most effective way to achieve chip miniaturization and high integration.

[0003] As one of the system packaging technologies, 2.5D heterogeneous integrated packaging technology is between two-dimensional and three-dimensional packaging. It connects multiple chips arranged side by side with a single-layer interposer through mature flip-chip technology and advanced silicon through-hole interconnection technology, and interconnects with the substrate through the single-layer interposer, significantly improving the input / output signal density of the package. Importantly, the functional chip of the 2.5D heterogeneous integrated packaging is mainly connected to the single-layer interposer through flip-chip technology, which poses new challenges to the chip-level bottom filler filled between the two.

[0004] Chip-level bottom filler plays an important role in alleviating stress concentration and releasing stress caused by the mismatch of thermal expansion coefficients between the chip and the substrate; it plays a key role in improving the reliability of packaging. Due to the high process temperature of 2.5D heterogeneous integrated packaging and the internal heat accumulation caused by stacking technology, higher requirements are placed on the glass transition temperature of chip-level bottom filler. In addition, the package size of 2.5D heterogeneous integrated packaging is larger, the interconnection density is higher, and a large amount of heat is generated. In a high-temperature environment, the reliability of 2.5D heterogeneous integrated packaging faces more severe challenges; in severe cases, it will cause chip warping and delamination between the chip-level bottom filler and the chip. Therefore, the chip-level bottom filler used in 2.5D heterogeneous integrated packaging is required to have higher bonding strength under high temperature and high temperature and high humidity conditions. In summary, it is of great significance to the technical field to develop a chip-level bottom filler with a high glass transition temperature, excellent bonding strength and high reliability to silicon wafers under high temperature and high temperature and high humidity conditions that can be applied to 2.5D heterogeneous integrated packaging. Summary of the invention

[0005] The present invention aims to solve the above-mentioned deficiencies in the prior art and to provide a chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging and a preparation method thereof.

[0006] To achieve the above objectives, the technical solutions adopted are as follows: One of the purposes of the present invention is to provide a chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging, which comprises the following components in parts by weight: Self-synthesized silicone epoxy resin A 10-15 parts, epoxy resin B 35-40 parts, coupling agent 3-6 parts, black paste 2-4 parts, filler 55-65 parts, curing agent 25-35 parts; The structural formula of the self-synthesized silicone epoxy resin A is: .

[0008] Furthermore, the self-synthesized organosilicon epoxy resin A is synthesized from the following raw materials in parts by weight: 156-164 parts of organosilicon-modified polyphenol monomers, 4-5 parts of benzyltriethylammonium chloride, 80-90 parts of epichlorohydrin, and 35-45 parts of sodium hydroxide aqueous solution.

[0009] Furthermore, the mass fraction of the sodium hydroxide aqueous solution is 50%.

[0010] Furthermore, the organosilicon-modified polyphenol monomer is prepared from the following raw materials in parts by weight: 320 to 350 parts of diallyl bisphenol monomer, 0.8 to 1.0 parts of platinum catalyst, and 110 to 130 parts of 2,4,6,8-tetramethylcyclotetrasiloxane.

[0011] Further, the self-synthesized silicone epoxy resin A is prepared by a two-step method; Further, the synthesis path of the self-synthesized silicone epoxy resin A is: The first step: the diallyl bisphenol monomer and 2,4,6,8-tetramethylcyclotetrasiloxane are subjected to a hydrosilylation reaction catalyzed by platinum to obtain a self-synthesized organosilicon-modified polyphenol monomer. The reaction formula is:

[0012] Step 2: The organosilicon-modified polyphenol monomer obtained in the first step is subjected to epoxidation reaction to obtain a self-synthesized organosilicon epoxy resin A. The reaction formula is:

[0013] Further, the epoxy resin B is at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and naphthalene epoxy resin. Wherein, the bisphenol A epoxy resin is preferably 850CRP of DIC Corporation of Japan, the bisphenol F epoxy resin is preferably YDF8170 of Nippon Steel & Sumitomo Metal Chemical Co., Ltd., and the naphthalene epoxy resin is preferably HP 4032D of DIC Corporation of Japan.

[0014] Furthermore, the epoxy resin B is a combination of bisphenol A epoxy resin, bisphenol F epoxy resin and naphthalene epoxy resin.

[0015] The beneficial effect of adopting the above two-step further scheme is: different types of epoxy resins are selected to make the glass transition temperature (Tg), bonding strength, tensile strength and modulus of the chip-level bottom filling glue reach a balance point, with excellent comprehensive performance.

[0016] Furthermore, the coupling agent is a silane coupling agent, specifically at least one of 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, aminopropyltriethoxysilane, and phenylaminopropyltrimethoxysilane.

[0017] The beneficial effects of adopting the above further scheme are: the silane coupling agent is conducive to improving the wetting performance of the chip-level bottom filling glue on the substrate and improving the fluidity; improving the compatibility between the resin and the filler; improving the wettability of the chip-level bottom filling glue on the substrate and enhancing the bonding strength.

[0018] Furthermore, the black paste is a premix of carbon black and epoxy resin B, specifically a premix of MA100 of Mitsubishi Corporation of Japan and 840 of DIC Corporation of Japan, and the mass ratio of MA100 to 840 is 2:8.

[0019] Furthermore, the curing agent is a liquid aromatic amine curing agent. The liquid aromatic amine curing agent is preferably diethyltoluenediamine, and more preferably ETHACURE 100 from Albemarle Japan Co., Ltd.

[0020] The beneficial effects of adopting the above further scheme are: ensuring that the chip-level bottom filling glue has excellent flow properties and meeting the workability requirements of the chip-level bottom filling glue for 2.5D heterogeneous integrated packaging; meeting the requirements of curing temperature and curing speed required by the 2.5D heterogeneous integrated packaging process.

[0021] Furthermore, the filler is spherical silica, preferably a spherical silica composition of different particle sizes. Spherical silica A is preferably spherical silica with an average particle size of 0.5 μm surface treated with 3-glycidyloxypropyltrimethoxysilane, more preferably SE2200-SEE manufactured by Japan ADMATECHS Co., Ltd. Spherical silica B is preferably spherical silica with an average particle size of 20 nm surface treated with 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, more preferably YA020A-JGP manufactured by Japan ADMATECHS Co., Ltd. The mass of spherical silica A:B is 10-15:1.3-1.7.

[0022] The beneficial effects of adopting the above further scheme are: spherical silica has better fluidity than non-spherical silica when the filler content is the same; a combination of silica micropowders of different particle sizes can maximize the amount of filler added when the viscosity is the same, so that the chip-level bottom filling glue has a lower CTE, thereby ensuring the reliability of 2.5D heterogeneous integrated packaging.

[0023] The second object of the present invention is to provide a method for preparing the above-mentioned chip-level bottom filling glue suitable for 2.5D heterogeneous integrated packaging, comprising the following steps: (1) 320-350 parts of diallyl bisphenol monomer and 0.8-1.0 parts of platinum catalyst are added into a three-necked flask, followed by dropwise addition of 110-130 parts of 2,4,6,8-tetramethylcyclotetrasiloxane, heating to 90° C. and maintaining for 3 hours, filtering and recovering the platinum catalyst, and removing the excess diallyl bisphenol monomer by reduced pressure distillation, thereby preparing an organosilicon-modified polyphenol monomer; Add 156-164 parts of the prepared organosilicon-modified polyphenol monomer, 2-2.5 parts of benzyltriethylammonium chloride and 80-90 parts of epichlorohydrin into a three-necked flask, and stir at 80°C for 5 hours; cool to room temperature, add the remaining benzyltriethylammonium chloride and 35-45 parts of 50% by mass sodium hydroxide aqueous solution to the mixture, and continue stirring and reacting at room temperature for 8 hours; then extract the product three times with ethyl acetate, wash the obtained ethyl acetate phase with deionized water three times, and then dry it with anhydrous magnesium sulfate; concentrate the product by filtering and evaporating; separate and purify the concentrated product by silica gel chromatography to prepare a self-synthesized organosilicon epoxy resin A; (2) 10-15 parts of the self-synthesized silicone epoxy resin A obtained in step (1), 35-40 parts of epoxy resin B, 3-6 parts of coupling agent, 2-4 parts of black paste, and 55-65 parts of filler are put into a stirring kettle, stirred evenly, and vacuumed to degas; then the premix is ​​subjected to a three-roll process and a aging process to ensure that the filler is fully impregnated; the fully impregnated premix is ​​put into a stirring kettle together with 25-35 parts of a curing agent, stirred evenly, and vacuumed to degas, thereby preparing a chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging.

[0024] Compared with the prior art, the present invention has the following beneficial effects: Compared with the chip-level bottom filling glue of traditional 2D packaging, the product of the present invention has a higher glass transition temperature; in addition, the product of the present invention has the characteristics of excellent flow performance, low CTE, and good heat resistance; it has both rigidity and toughness, and after being placed in the Uhast environmental chamber for 96 hours, it still has excellent bonding strength to the silicon wafer at 260°C, reducing the stress generated on the solder joint due to the mismatch of the thermal expansion coefficients of the chip and the substrate, and can fully meet the workability and reliability requirements of 2.5D heterogeneous integrated packaging, avoiding the formation of defects during the flow curing process; The self-synthesized organosilicon epoxy resin A of the present invention has a tetraepoxy functional group structure, and can improve the system crosslinking density and optimize the modulus of the chip-level bottom filling glue by crosslinking reaction with other epoxy resins, so that the chip-level bottom filling glue has a higher glass transition temperature; it has a polyphenyl and alicyclic skeleton structure, which gives the material an outstanding high-temperature modulus and excellent thermal stability, and is suitable for a high-energy-consumption packaging environment with high interconnection density and high heat release caused by high energy consumption; at the same time, multiple ether bonds and silicon-oxygen bond structures are introduced in the molecular structure design, which gives the material excellent flexibility, so that the molecular structure has both rigidity and toughness, thereby improving the material's anti-cracking performance under high and low temperature impact conditions and in the wet heat aging process, so that the chip-level bottom filling glue still has excellent bonding strength to the silicon wafer after aging for 96 hours in a Uhast environmental chamber, thereby ensuring the reliability of the 2.5D heterogeneous integrated packaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the infrared spectrum of the self-synthesized silicone epoxy resin A and 2,4,6,8-tetramethylcyclotetrasiloxane (D4H) in Example 1. DETAILED DESCRIPTION

[0026] The principles and features of the present invention are described below in conjunction with examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0027] Example 1 To prepare chip-level underfill suitable for 2.5D heterogeneous integrated packaging, the steps are as follows: (1) At room temperature, 335 parts by weight of diallyl bisphenol monomer and 0.9 parts by weight of platinum catalyst were added to a three-necked flask. Subsequently, 120 parts of 2,4,6,8-tetramethylcyclotetrasiloxane were added dropwise to the mixture, and the mixture was heated to 90°C and maintained for 3 hours. The platinum catalyst was recovered by filtration, and the excess diallyl bisphenol monomer was removed by reduced pressure distillation, thereby preparing a silicone-modified polyphenol monomer.

[0028] 160 parts of the prepared organosilicon-modified polyphenol monomer, 2.25 parts of benzyltriethylammonium chloride and 85 parts of epichlorohydrin were added to a three-necked flask, and stirred at 80°C for 5 hours; cooled to room temperature, 2.25 parts of benzyltriethylammonium chloride and 40 parts of a 50% by mass sodium hydroxide aqueous solution were added to the mixture, and the reaction was continued to stir at room temperature for 8 hours; the product was then extracted three times with ethyl acetate, the obtained ethyl acetate phase was washed three times with deionized water, and then dried with anhydrous magnesium sulfate; the product was concentrated by filtering and evaporating; the concentrated product was separated and purified by a silica gel column to prepare a self-synthesized organosilicon epoxy resin A. Figure 1 The infrared spectrum of the self-synthesized silicone epoxy resin A and 2,4,6,8-tetramethylcyclotetrasiloxane (D4H). Figure 1 Visible, 2165 cm -1 The -Si-H stretching vibration peak is at 908 cm. Comparison of the two curves of self-synthesized silicone epoxy resin A and 2,4,6,8-tetramethylcyclotetrasiloxane shows that the -Si-H stretching vibration peak on the curve of self-synthesized silicone epoxy resin A completely disappears, indicating that D4H successfully obtains silicone-modified polyphenol monomers through hydrosilylation reaction; -1 The stretching vibration peak of the epoxy group is at 908 cm. By comparing the two curves, it can be seen that the D4H curve has no stretching vibration peak of the epoxy group; while the curve of silicone epoxy resin A has a peak at 908 cm -1 The presence of vibration peaks indicated the successful introduction of epoxy groups, further proving the successful synthesis of self-synthesized silicone epoxy resin A.

[0029] (2) At room temperature, 15 parts of the self-synthesized organosilicon epoxy resin A obtained in step (1), 20 parts of bisphenol A epoxy resin 850CRP, 10 parts of bisphenol F epoxy resin YDF8170, 10 parts of naphthalene epoxy resin HP 4032D, 3 parts of 3-(2,3-epoxypropoxy)propylmethyldiethoxysilane, 2 parts of black paste (the mass ratio of MA100 to 840 is 2:8), 52.2 parts of spherical silica SE2200-SEE with an average particle size of 0.5 μm, and 7.8 parts of spherical silica YA020A-JGP with an average particle size of 20 nm are added into a stirring kettle, stirred evenly, and vacuumed for degassing; then the premix is ​​subjected to a three-roll process and a aging process to ensure sufficient infiltration of the filler; the premix is ​​mixed with 30 parts of ETHACURE 100 are sequentially put into a stirring kettle, stirred evenly, and vacuumed for degassing to obtain the chip-level bottom filling glue suitable for 2.5D heterogeneous integrated packaging of the present invention.

[0030] Example 2 To prepare chip-level underfill suitable for 2.5D heterogeneous integrated packaging, the steps are as follows: (1) Same as Example 1.

[0031] (2) At room temperature, 10 parts by weight of the self-synthesized organosilicon epoxy resin A obtained in step (1), 20 parts by weight of bisphenol A epoxy resin 850CRP, 10 parts by weight of bisphenol F epoxy resin YDF8170, 10 parts by weight of naphthalene epoxy resin HP 4032D, 3 parts by weight of aminopropyl triethoxysilane, 2 parts by weight of black paste (the mass ratio of MA100 to 840 is 2:8), 52.2 parts by weight of spherical silica SE2200-SEE with an average particle size of 0.5 μm, and 7.8 parts by weight of spherical silica YA020A-JGP with an average particle size of 20 nm are added into a stirring kettle, stirred evenly, and vacuumed for degassing; the premix is ​​then subjected to a three-roll process and a aging process to ensure sufficient infiltration of the filler; the premix is ​​mixed with 30 parts by weight of ETHACURE 100 are sequentially put into a stirring kettle, stirred evenly, and vacuumed for degassing to obtain the chip-level bottom filling glue suitable for 2.5D heterogeneous integrated packaging of the present invention.

[0032] Example 3 To prepare chip-level underfill suitable for 2.5D heterogeneous integrated packaging, the steps are as follows: (1) Same as Example 1.

[0033] (2) At room temperature, 15 parts of the self-synthesized silicone epoxy resin A obtained in step (1), 20 parts of bisphenol A epoxy resin 850CRP, 20 parts of bisphenol F epoxy resin YDF8170, 3 parts of 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, 2 parts of black paste (the mass ratio of MA100 to 840 is 2:8), 52.2 parts of spherical silica SE2200-SEE with an average particle size of 0.5 μm, and 7.8 parts of spherical silica YA020A-JGP with an average particle size of 20 nm are added into a stirring kettle, stirred evenly, and vacuumed for degassing; then the premix is ​​subjected to a three-roll process and a aging process to ensure sufficient infiltration of the filler; the premix is ​​mixed with 30 parts of ETHACURE 100 are sequentially put into a stirring kettle, stirred evenly, and vacuumed for degassing to obtain the chip-level bottom filling glue suitable for 2.5D heterogeneous integrated packaging of the present invention.

[0034] Example 4 To prepare chip-level underfill suitable for 2.5D heterogeneous integrated packaging, the steps are as follows: (1) Same as Example 1.

[0035] (2) At room temperature, 15 parts of the self-synthesized organosilicon epoxy resin A obtained in step (1), 20 parts of bisphenol A epoxy resin 850CRP, 20 parts of naphthalene epoxy resin HP 4032D, 3 parts of 3-(2,3-epoxypropoxy)propylmethyldiethoxysilane, 2 parts of black paste (the mass ratio of MA100 to 840 is 2:8), 52.2 parts of spherical silica SE2200-SEE with an average particle size of 0.5 μm, and 7.8 parts of spherical silica YA020A-JGP with an average particle size of 20 nm are added into a stirring kettle, stirred evenly, and vacuumed for degassing; then the premix is ​​subjected to a three-roll process and a aging process to ensure sufficient infiltration of the filler; the premix is ​​mixed with 30 parts of ETHACURE 100 are sequentially put into a stirring kettle, stirred evenly, and vacuumed for degassing to obtain the chip-level bottom filling glue suitable for 2.5D heterogeneous integrated packaging of the present invention.

[0036] Example 5 To prepare chip-level underfill suitable for 2.5D heterogeneous integrated packaging, the steps are as follows: (1) Same as Example 1.

[0037] (2) At room temperature, 15 parts of the self-synthesized organosilicon epoxy resin A obtained in step (1), 20 parts of bisphenol F epoxy resin YDF8170, 20 parts of naphthalene epoxy resin HP 4032D, 3 parts of 3-(2,3-epoxypropoxy)propylmethyldiethoxysilane, 2 parts of black paste (the mass ratio of MA100 to 840 is 2:8), 52.2 parts of spherical silica SE2200-SEE with an average particle size of 0.5 μm, and 7.8 parts of spherical silica YA020A-JGP with an average particle size of 20 nm are added into a stirring kettle, stirred evenly, and vacuumed for degassing; then the premix is ​​subjected to a three-roll process and a aging process to ensure sufficient infiltration of the filler; the premix is ​​mixed with 30 parts of ETHACURE 100 are sequentially put into a stirring kettle, stirred evenly, and vacuumed for degassing to obtain the chip-level bottom filling glue suitable for 2.5D heterogeneous integrated packaging of the present invention.

[0038] Comparative Example 1 Prepare chip-level underfill: At room temperature, 35 parts of bisphenol A epoxy resin 850CRP, 10 parts of bisphenol F epoxy resin YDF8170, 10 parts of naphthalene epoxy resin HP 4032D, 3 parts of 3-(2,3-epoxypropoxy)propylmethyldiethoxysilane, 2 parts of black paste (the mass ratio of MA100 to 840 is 2:8), 52.2 parts of spherical silica SE2200-SEE with an average particle size of 0.5 μm, and 7.8 parts of spherical silica YA020A-JGP with an average particle size of 20 nm are put into a stirring tank, stirred evenly, and vacuumed for degassing; then the premix is ​​subjected to a three-roll process and a aging process to ensure sufficient infiltration of the filler; the premix and 30 parts of ETHACURE 100 are sequentially put into a stirring tank, stirred evenly, and vacuumed for degassing to obtain a chip-level bottom filling adhesive.

[0039] Comparative Example 2 Prepare chip-level underfill: At room temperature, 20 parts of bisphenol A epoxy resin 850CRP, 15 parts of bisphenol F epoxy resin YDF8170, 20 parts of naphthalene epoxy resin HP 4032D, 3 parts of 3-(2,3-epoxypropoxy)propylmethyldiethoxysilane, 2 parts of black paste (the mass ratio of MA100 to 840 is 2:8), 52.2 parts of spherical silica SE2200-SEE with an average particle size of 0.5 μm, and 7.8 parts of spherical silica YA020A-JGP with an average particle size of 20 nm are put into a stirring tank, stirred evenly, and vacuumed for degassing; then the premix is ​​subjected to a three-roll process and a aging process to ensure sufficient infiltration of the filler; the premix and 30 parts of ETHACURE 100 are sequentially put into a stirring tank, stirred evenly, and vacuumed for degassing to obtain a chip-level bottom filling adhesive.

[0040] test The performance of the chip-level underfill adhesives of the above-mentioned embodiments 1 to 5 of the present invention and comparative embodiments 1 to 2 was tested by the following experiments.

[0041] Test 1.260℃ high temperature modulus test The high-temperature modulus at 260 °C was obtained by DMA testing using a dual-cantilever measurement mode, heating from -50 °C to 265 °C at a rate of 3 °C / min, an oscillation frequency of 1 Hz, and an amplitude of 10 μm.

[0042] Test 2. Flow performance test Glass is connected to glass through spacer balls with a gap of 30 um. The size of the glass sheet is 20*20 mm. The flow performance of chip-level bottom filling glue in 2.5D heterogeneous integrated packaging at 110°C is simulated, and the flow time for complete filling is recorded.

[0043] Test 3. Glass transition temperature test The glass transition temperature was obtained by DMA measurement using a dual cantilever measurement mode, heating from −50 °C to 265 °C at a rate of 3 °C / min, an oscillation frequency of 1 Hz, and an amplitude of 10 μm.

[0044] Test 4. Thermal Expansion Coefficient Test (CTE1 <Tg) The thermal expansion coefficient is obtained by TMA test, with a temperature increase from -20°C to 280°C, a heating rate of 5°C / min, and the unit is ppm / °C. Tested according to ASTM D696.

[0045] Test 5. K 1C test K 1CThe test is based on ASTM D5045 test standard, measured by single-edge notch bending technique of a universal testing machine, using a 3-point bending fixture and testing the sample at a crosshead speed of 10 mm / min.

[0046] Test 6. Uhast 96h 260℃ thrust strength test The 260℃ thrust strength of Uhast after 96 hours is obtained by testing with a push-pull tester. The glue and the bare silicon wafer are cured and bonded through a specific mold. After being placed in the Uhast environmental chamber for 96 hours, it is placed on the test platform and heated at 260℃ for 5 minutes for a thrust test. The test rate is 50 mm / min.

[0047] The results of tests 1 to 6 are shown in Table 1.

[0048] Table 1. Comparison of test performance of samples in Examples 1 to 5 and samples in Comparative Examples 1 to 2

[0049] It can be seen from the data in Table 1 that the product of the present invention has a high glass transition temperature and high temperature modulus, meeting the requirements of high process temperature of 2.5D heterogeneous integrated packaging and internal heat accumulation caused by stacking technology; in addition, the product of the present invention has excellent flow performance, meeting the operability requirements of 2.5D heterogeneous integrated packaging; it has both rigidity and toughness, and after being placed in the Uhast environmental chamber for 96 hours, it still has excellent bonding strength to the silicon wafer at 260°C; it has a low CTE, which reduces the stress on the solder joints caused by the mismatch of the thermal expansion coefficients of the chip and the substrate, and effectively ensures the reliability of the 2.5D heterogeneous integrated packaging.

[0050] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A chip-level bottom filler suitable for 2.5D heterogeneous integrated packaging, characterized in that: The composition comprises the following components by weight: 10-15 parts of self-synthesized organosilicon epoxy resin A, 35-40 parts of epoxy resin, 3-6 parts of coupling agent, 2-4 parts of black paste, 55-65 parts of filler, and 25-35 parts of curing agent; The structural formula of the self-synthesized silicone epoxy resin A is: 。 2. The chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging according to claim 1, characterized in that: The self-synthesized organosilicon epoxy resin A is synthesized from the following raw materials in parts by weight: 156-164 parts of organosilicon-modified polyphenol monomers, 4-5 parts of benzyltriethylammonium chloride, 80-90 parts of epichlorohydrin, and 35-45 parts of sodium hydroxide aqueous solution.

3. The chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging according to claim 2, characterized in that: The organosilicon-modified polyphenol monomer is prepared from the following raw materials in parts by weight: 320 to 350 parts of diallyl bisphenol monomer, 0.8 to 1.0 parts of platinum catalyst, and 110 to 130 parts of 2,4,6,8-tetramethylcyclotetrasiloxane.

4. The chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging according to claim 3, characterized in that: The synthesis path of the self-synthesized silicone epoxy resin A is: 。 5. The chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging according to claim 1, characterized in that: The epoxy resin B is at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and naphthalene epoxy resin.

6. The chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging according to claim 5, characterized in that: The epoxy resin B is a combination of bisphenol A epoxy resin, bisphenol F epoxy resin and naphthalene epoxy resin.

7. The chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging according to claim 1, characterized in that: The coupling agent is at least one of 3-(2,3-epoxypropoxy)propylmethyldiethoxysilane, aminopropyltriethoxysilane, and phenylaminopropyltrimethoxysilane; the black paste is a premix of carbon black and epoxy resin B; and the curing agent is a liquid aromatic amine curing agent.

8. The chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging according to claim 1, characterized in that: The filler is a composition of spherical silica with different particle sizes, wherein the mass ratio of spherical silica with an average particle size of 0.5 μm to spherical silica with an average particle size of 20 nm is 10-15:1.3-1.7; and the surface of the spherical silica is epoxidized.

9. A method for preparing a chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging as claimed in any one of claims 1 to 8, characterized in that: The steps include: (1) 320-350 parts of diallyl bisphenol monomer and 0.8-1.0 parts of platinum catalyst are added into a three-necked flask, followed by dropwise addition of 110-130 parts of 2,4,6,8-tetramethylcyclotetrasiloxane, heating to 90° C. and maintaining for 3 hours, filtering and recovering the platinum catalyst, and removing the excess diallyl bisphenol monomer by reduced pressure distillation, thereby preparing an organosilicon-modified polyphenol monomer; Add 156-164 parts of the organosilicon-modified polyphenol monomer prepared above, 2-2.5 parts of benzyltriethylammonium chloride and 80-90 parts of epichlorohydrin into a three-necked flask, and stir at 80°C for 5 hours; cool to room temperature, add the remaining benzyltriethylammonium chloride and 35-45 parts of 50% by mass sodium hydroxide aqueous solution to the above mixture, and continue stirring and reacting at room temperature for 8 hours; then extract the product three times with ethyl acetate, wash the obtained ethyl acetate phase with deionized water three times, and then dry it with anhydrous magnesium sulfate; concentrate the product by filtering and evaporating; The concentrated product is separated and purified by a silica gel column chromatography to prepare a self-synthesized organosilicon epoxy resin A; (2) 10-15 parts of the self-synthesized silicone epoxy resin A obtained in step (1), 35-40 parts of epoxy resin B, 3-6 parts of coupling agent, 2-4 parts of black paste, and 55-65 parts of filler are put into a stirring kettle, stirred evenly, and vacuumed to degas; then the premix is ​​subjected to a three-roll process and a aging process to ensure that the filler is fully impregnated; the fully impregnated premix is ​​put into a stirring kettle together with 25-35 parts of a curing agent, stirred evenly, and vacuumed to degas, thereby preparing a chip-level bottom filling adhesive suitable for 2.5D heterogeneous integrated packaging.

Citation Information

Cited By

  • Chip-level underfill adhesive with low precipitation and excellent bonding performance and preparation method thereof

    CN119570420A

  • Low-temperature-curable low-modulus low-stress adhesive for optical module and preparation method of low-temperature-curable low-modulus low-stress adhesive

    CN120737780A