Wafer surface treatment liquid

By using a combination of fluorine-containing compounds, silane coupling agents and organic solvents in the wafer surface treatment solution, the gate collapse problem caused by traditional cleaning solutions is solved, the IPA contact angle is increased, and adhesion during the drying process is avoided. , ensuring the stability of high aspect ratio structures.

CN118726010APending Publication Date: 2024-10-01SHANGHAI SINYANG SEMICONDUCTOR MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310349457.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional wafer cleaning solutions cause gate collapse during the drying process, especially in high aspect ratio structures. The cleaning solution is difficult to completely remove contaminants and may cause adhesion and structural collapse during the drying process.

Method used

A wafer surface treatment liquid is provided, which contains a combination of 0.005-1% fluorine-containing compound, 0.1-20% silane coupling agent and organic solvent, specifically selected from the group consisting of isopropyl alcohol, propylene glycol methyl ether acetate, N,N -Dimethylformamide, etc., used to clean high aspect ratio structures and increase the IPA contact angle to avoid adhesion.

Benefits of technology

It effectively avoids adhesion and collapse between gate electrodes during the drying process, ensuring the stability of the high aspect ratio structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004160957080000041
    Figure BDA0004160957080000041
  • Figure BDA0004160957080000051
    Figure BDA0004160957080000051
  • Figure BDA0004160957080000061
    Figure BDA0004160957080000061
Patent Text Reader

Abstract

The invention discloses a wafer surface treatment liquid, and particularly, the wafer surface treatment liquid provided by the invention is prepared from the following raw materials in percentage by mass: 0.005 to 1 percent of fluorine-containing compound, 0.1 to 20 percent of silane coupling agent and organic solvent, the sum of the mass fractions of the components is 100%. The organic solvent is supplemented to the balance; after a wafer is treated by the wafer surface treatment liquid, grid electrodes are not adhered in the drying process, so that grid electrode collapse is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a wafer surface processing liquid. Background Art

[0002] With the continuous development of the semiconductor industry, integrated circuits are gradually developing towards high integration and ultra-fine line widths. Therefore, more and more high aspect ratio structures are involved in the chip manufacturing process (in the semiconductor industry, structures with a depth / height and width ratio greater than or equal to 10 are generally defined as high aspect ratio). High aspect ratio structures not only face huge challenges during etching and deposition, but also have great problems in cleaning after etching. On the one hand, the current mainstream cleaning method is still wet cleaning based on water chemistry. For these micro-nano structures with small openings but large depths, it is difficult for liquids to enter the bottom of the grooves to achieve the purpose of cleaning; on the other hand, once the cleaning liquid enters the deep grooves, it is difficult to remove the liquid under the action of surface tension, resulting in residual contaminants, which become a potential threat to subsequent processes, and even cause device failure in severe cases. At the same time, the capillary force existing during the drying process of these high aspect ratio structures may also cause the collapse of these structures, resulting in device failure.

[0003] In the traditional IPA drying process, when the gate AR (aspect ratio) is greater than or equal to 10, the gate will adhere to the gate during the drying process, causing the gate to collapse during the drying process. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a wafer surface treatment liquid in order to overcome the problem that the gate collapses during the spin-drying process after the wafer is treated with the traditional cleaning liquid. After the wafer is treated with the surface treatment liquid of the present invention, the IPA contact angle is significantly increased, and the gates will not adhere to each other during the drying process, thereby avoiding the occurrence of gate collapse.

[0005] The present invention solves the above technical problems through the following technical solutions.

[0006] The present invention provides a wafer surface treatment liquid, the raw materials of which include the following components in mass fraction: 0.005-1% of a fluorine-containing compound, 0.1-20% of a silane coupling agent and an organic solvent; the sum of the mass fractions of the components is 100%; the organic solvent makes up the balance;

[0007] The organic solvent is selected from one or more of isopropyl alcohol (IPA), propylene glycol methyl ether acetate (PGMEA), N,N-dimethylformamide (DMF), n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene;

[0008] The silane coupling agent is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, 3-glycidylpropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, vinyltrimethoxysilane, dodecyltrimethoxysilane and 3-isocyanatepropyltrimethoxysilane.

[0009] In some embodiments, the fluorine-containing compound is selected from one or more of hydrogen fluoride, ammonium fluoride, ammonium bifluoride, tetramethylammonium fluoride, fluorosulfonic acid and trihydroxyethylammonium fluoride, perfluorooctylethylene, perfluorodecene, perfluorohexylethylene, perfluorooctene, perfluorobutylethylene and 1H,1H,2H-perfluoro-1-hexene;

[0010] Preferably, the fluorine-containing compound is hydrogen fluoride or fluorosulfonic acid.

[0011] In some embodiments, the mass fraction of the fluorine-containing compound is 0.005-0.10%;

[0012] Preferably, the mass fraction of the fluorine-containing compound is 0.01-0.05%.

[0013] In some embodiments, the silane coupling agent is 3-aminopropyltriethoxysilane.

[0014] In some embodiments, the mass fraction of the silane coupling agent is 1-15%;

[0015] Preferably, the mass fraction of the silane coupling agent is 5-10%.

[0016] In some embodiments, the organic solvent is selected from one or more of isopropyl alcohol, propylene glycol methyl ether acetate and N,N-dimethylformamide;

[0017] Preferably, the organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate.

[0018] In some embodiments, when the organic solvent is isopropanol and propylene glycol methyl ether acetate, the mass ratio of the propylene glycol methyl ether acetate to the isopropanol is (1-2):1.

[0019] In some embodiments, the pH value of the wafer surface treatment solution is 7-12.

[0020] In some schemes, the raw materials include the following components in mass fractions: 0.01-0.05% fluorine-containing compound, 5-10% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance;

[0021] The organic solvent is selected from isopropyl alcohol (IPA) and / or propylene glycol methyl ether acetate (PGMEA);

[0022] The silane coupling agent is 3-aminopropyltriethoxysilane;

[0023] The fluorine-containing compound is hydrogen fluoride and / or fluorosulfonic acid.

[0024] In some embodiments, the wafer surface treatment solution comprises raw materials comprising any of the following components in mass fractions:

[0025] Solution 1: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;

[0026] Solution 2: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;

[0027] Solution 3: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;

[0028] Solution 4: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;

[0029] Scheme 5: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0030] Scheme 6: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0031] Scheme 7: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0032] Scheme 8: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0033] Scheme 9: 0.01% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance;

[0034] Scheme 10: 0.01% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance;

[0035] Scheme 11: 0.05% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance;

[0036] Scheme 12: 0.05% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance.

[0037] Preferably, the wafer surface treatment liquid is composed of any of the above schemes.

[0038] In some embodiments, the wafer surface treatment solution is used to clean wafers with a high aspect ratio.

[0039] The term "high aspect ratio" of the present invention: In the semiconductor industry, a structure whose ratio of depth to width is greater than or equal to 10 is generally defined as having a high aspect ratio.

[0040] The "room temperature" of the present invention refers to 25±5°C.

[0041] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0042] The reagents and raw materials used in the present invention are commercially available.

[0043] The positive and progressive effect of the present invention is that after the wafer is treated with the wafer surface treatment liquid of the present invention, no adhesion will occur between the gates during the drying process, thereby avoiding the occurrence of gate collapse. DETAILED DESCRIPTION

[0044] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0045] The surface treatment liquid was prepared according to the ingredients and proportions of each example in Table 1, mixed evenly, and stirred at room temperature for 1 hour (without any order of addition).

[0046] Table 1

[0047]

[0048]

[0049] Note: “ / ” means does not exist.

[0050] This test was conducted using TEOS (tetraethoxysilane) and SiN (silicon nitride) wafers.

[0051] Experimental methods:

[0052] 1. Cut the wafer with aspect ratio of 10 into 30*30mm test pieces;

[0053] 2. Soak the test piece in IPA cleaning solution for 1 minute and take it out;

[0054] 3. Immerse the test pieces in the surface treatment solutions described in Table 1 for 1 min, take them out and blow dry;

[0055] 4. The contact angle of the test piece was tested using a contact angle tester (AttensionThetaLite), the test solution was IPA, the surface roughness was tested at the same time, and the surface of the test piece was observed by electron microscopy; the results are shown in Table 2 below.

[0056] Table 2

[0057]

[0058]

[0059] It can be seen from the test results that after being immersed in the surface treatment liquid, the IPA contact angle increases significantly, and no adhesion occurs between the gates during the drying process, thus avoiding the collapse of the gate.

Claims

1. A wafer surface treatment liquid, characterized in that: The raw materials include the following components in mass fraction: 0.005-1% fluorine-containing compound, 0.1-20% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The organic solvent is selected from one or more of isopropyl alcohol, propylene glycol methyl ether acetate, N,N-dimethylformamide, n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene; The silane coupling agent is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, 3-glycidylpropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, vinyltrimethoxysilane, dodecyltrimethoxysilane and 3-isocyanatepropyltrimethoxysilane.

2. The wafer surface treatment solution according to claim 1, characterized in that: The fluorine-containing compound is selected from one or more of hydrogen fluoride, ammonium fluoride, ammonium bifluoride, tetramethylammonium fluoride, fluorosulfonic acid, trihydroxyethylammonium fluoride, perfluorooctylethylene, perfluorodecene, perfluorohexylethylene, perfluorooctene, perfluorobutylethylene and 1H,1H,2H-perfluoro-1-hexene.

3. The wafer surface treatment solution as claimed in claim 2, characterized in that: The fluorine-containing compound is hydrogen fluoride and / or fluorosulfonic acid.

4. The wafer surface treatment solution according to any one of claims 1 to 3, characterized in that: The surface treatment liquid meets one or more of the following conditions: (1) The silane coupling agent is 3-aminopropyltriethoxysilane; (2) the organic solvent is selected from one or more of isopropyl alcohol, propylene glycol methyl ether acetate and N,N-dimethylformamide; and (3) The pH value of the wafer surface treatment solution is 7-12.

5. The wafer surface treatment liquid as claimed in claim 4, characterized in that: The surface treatment liquid meets one or more of the following conditions: (1) The mass fraction of the fluorine-containing compound is 0.005-0.10%; (2) the mass fraction of the silane coupling agent is 1-15%; and (3) The organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate.

6. The wafer surface treatment solution as claimed in claim 5, characterized in that: The surface treatment liquid meets one or more of the following conditions: (1) The mass fraction of the fluorine-containing compound is 0.01-0.05%; (2) The mass fraction of the silane coupling agent is 5-10%; and (3) When the organic solvent is isopropyl alcohol and propylene glycol methyl ether acetate, the mass ratio of the propylene glycol methyl ether acetate to the isopropyl alcohol is (1-2):

1.

7. The wafer surface treatment solution according to any one of claims 1 to 6, characterized in that: The raw materials include the following components in mass fraction: 0.01-0.05% of fluorine-containing compound, 5-10% of silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The organic solvent is selected from isopropyl alcohol and / or propylene glycol methyl ether acetate; The silane coupling agent is 3-aminopropyltriethoxysilane; The fluorine-containing compound is hydrogen fluoride and / or fluorosulfonic acid.

8. The wafer surface treatment solution as claimed in claim 7, characterized in that: The raw materials include any of the following components in mass fractions: Solution 1: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Solution 2: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Solution 3: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Solution 4: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Scheme 5: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 6: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 7: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 8: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 9: 0.01% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance; Scheme 10: 0.01% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance; Scheme 11: 0.05% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance; Scheme 12: 0.05% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance.

9. The wafer surface treatment liquid as claimed in claim 8, characterized in that: The raw materials of the surface treatment liquid are composed of any one of the schemes in claim 8.

10. The wafer surface treatment liquid according to claim 9, characterized in that: The surface treatment liquid is used for cleaning wafers with a high aspect ratio.