TiN coating with high film-substrate binding force

Through high-power pulse magnetron sputtering technology, the Ti transition layer is deposited first and then the TiN coating is deposited, which solves the problem of insufficient bonding force between the TiN coating and the substrate, improves the service life and bonding strength of the coating, and is suitable for high-performance decoration coating.

CN118726906APending Publication Date: 2024-10-01LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410765807.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The bonding strength between the TiN coating and the substrate is poor, causing the coating to fall off easily and limiting the service life of the coating.

Method used

High-power pulse magnetron sputtering technology is used to deposit the Ti transition layer first and then the TiN coating. By adjusting process parameters such as argon gas flow, bias, frequency and pulse width, the bonding force between the coating and the substrate is improved.

Benefits of technology

It significantly improves the bonding strength between the TiN coating and the substrate, prolongs the service life of the coating, and the process is simple. The surface color of the coating is golden yellow, making it suitable for colored decoration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726906A_ABST
    Figure CN118726906A_ABST
Patent Text Reader

Abstract

The invention provides a TiN coating with high film-substrate binding force. The TiN coating comprises 40-50 at.% of N and 50-60 at.% of Ti according to the atomic percentage. According to the TiN coating, a high-power pulse magnetron sputtering technology is adopted, a Ti transition layer is deposited firstly, then a TiN coating is deposited, and the TiN coating is formed. The method has the beneficial effects that the bonding strength between the TiN coating and the matrix is improved, and the hardness of the TiN coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a TiN coating with high film-base bonding force, belonging to the technical field of coatings. Background Art

[0002] TiN coating is widely used in the tool industry, medical industry, aerospace, integrated circuits and other fields due to its stable chemical properties and good mechanical properties. For example, as a hard coating with mature industrial applications, TiN coating can effectively protect aircraft engine blades, cutting tools and precision instruments. However, with the continuous improvement of the performance requirements of mechanical parts, the use conditions of the coating have become more and more stringent, which puts higher requirements on the reliability and service life of the protective coating. The bonding strength between the TiN coating and the substrate is poor, which makes the coating easy to fall off, which has always been an important factor limiting the service life of the coating. There are differences in parameters such as lattice constant and thermal expansion coefficient at the heterogeneous interface between the coating and the substrate, which makes the bonding between the coating and the substrate fragile. Summary of the invention

[0003] The present invention provides a TiN coating with high film-base bonding strength, which solves the technical problem in the prior art that the bonding strength between the TiN coating and the base is insufficient, which easily causes the coating to peel off and fail.

[0004] The present invention is implemented as follows: the TiN coating includes N 40-50 at.% and Ti 50-60 at.% according to the atomic mass ratio, and the thickness is 300-500 nm. Through high-power pulse magnetron sputtering, the Ti transition layer is first deposited, and then the TiN coating is deposited.

[0005] As a preferred embodiment, the TiN coating is prepared by the following steps: (1) Substrate pretreatment The substrate is cleaned and dried for later use; (2) Pre-sputtering cleaning The substrate obtained in step (1) is in a vacuum degree of less than 1×10 -3 Pa, temperature 350℃, argon gas flow rate 350 sccm, bias voltage -850 V, frequency 40 kHz, pulse width 4 μs, pre-sputter cleaning 20-30 min; (3) Deposition of Ti transition layer The argon flow rate was adjusted to 60 sccm, the substrate bias voltage was continuously adjusted to -200~-300 V, the frequency was 80 kHz, the pulse width was 6 μs, a high-power pulse power supply was added to the pure Ti target, the peak current was adjusted to 150~300 A, the frequency was 100 Hz, the pulse width was 450 μs, and the deposition time was 15 min; (4) Deposition of TiN coating The Ti target peak current was maintained at 150~300 A, the frequency was 100 Hz, the pulse width was 500 μs, the argon flow rate was maintained at 60 sccm, nitrogen was introduced, the nitrogen flow rate was 10~20 sccm, the bias voltage was -120 V, the frequency was 40 kHz, the pulse width was 12 μs, and the deposition time was 10800 s.

[0006] As a preferred embodiment, the peak current in step (3) is 180 A.

[0007] As a preferred embodiment, the nitrogen flow rate in step (4) is 10 sccm.

[0008] As a preferred embodiment, the pre-sputtering cleaning time in step (2) is 20 minutes.

[0009] The invention has the beneficial effects that the high-power pulsed magnetron sputtering technology has the advantage of high metal ionization rate, and the coating process parameters are regulated to obtain the optimal deposition parameters. By constructing an intermediate transition layer, the interface physical property mutation is reduced, the bonding strength between the coating and the substrate is improved, and the use reliability of the coating is improved. The TiN coating preparation process of the invention is simple, the coating surface color is golden yellow, and can be used for color decoration. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0011] Figure 1 is a cross-sectional SEM image of the TiN coating prepared in Example 1; Figure 2 is a bonding force diagram of the TiN coating prepared in Example 1; Figure 3 is a light microscopy result image of the scratches on the TiN coating prepared in Example 1; Figure 4 1 is a graph of hardness and elastic modulus of the TiN coating prepared in Example 1. DETAILED DESCRIPTION

[0012] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0013] The TiN coating includes N 40-50 at.% and Ti 50-60 at.% according to the atomic mass ratio, and has a thickness of 300-500 nm. The Ti transition layer is first deposited and then the TiN coating is deposited by high-power pulsed magnetron sputtering. Example

[0014] A TiN coating with high film-base bonding strength and a preparation method thereof, wherein the coating is prepared by high-power pulsed magnetron sputtering technology, and the specific steps are as follows: (1) Preprocessing The 9Cr18 alloy steel block substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then placed in a drying chamber for standby use after being blown dry. (2) Pre-sputtering cleaning The 9Cr18 alloy steel block sample treated in step (1) was placed in a vacuum chamber for evacuation. The chamber temperature was heated to 350 °C and the vacuum degree was less than 1×10 -3 Pa, ion etching of the substrate surface was started, Ar was introduced with a flow rate of 350 sccm, a pulse bias voltage of -850 V, a frequency of 40 kHz, and a pulse width of 4 μs was applied to the steel block sample, and the steel block sample was pre-sputtered and cleaned with Ar plasma for 20 min; (3) Deposition of Ti transition layer High-power pulsed magnetron sputtering technology was used, the Ar flow rate was adjusted to 60 sccm, the substrate bias was continuously adjusted to -200 V, the frequency was 80 kHz, and the pulse width was 6 μs. A high-power pulse power supply was added to the pure Ti target, and the peak current was adjusted to 180 A, the frequency was 100 Hz, and the pulse width was 450 μs. The Ti transition layer was deposited for 15 min. (4) Deposition of TiN coating High-power pulsed magnetron sputtering technology was used to deposit TiN coating by keeping the Ti target current unchanged, the frequency 100 Hz, the pulse width 500 μs, the Ar flow rate unchanged, introducing N2 with a flow rate of 10 sccm, applying a pulse bias voltage of -120 V, the frequency 40 kHz, the pulse width 12 μs, and the deposition time 10800 s on the steel block sample.

[0015] See also Figure 1 The thickness of the TiN coating prepared in Example 1 is 500 nm. Figure 2 , the bonding force of the coating is 75N. Figure 3 , the coating was scratched and leaked out of the substrate at a load of 75 N. Figure 4 , the hardness of the coating is about 31 GPa and the elastic modulus is about 280 GPa. Example

[0016] A TiN coating with high film-base bonding strength and a preparation method thereof, wherein the coating is prepared by high-power pulsed magnetron sputtering technology, and the specific steps are as follows: (1) Preprocessing The 9Cr18 alloy steel block substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then placed in a drying chamber for standby use after being blown dry. (2) Pre-sputtering cleaning The 9Cr18 alloy steel block sample treated in step (1) was placed in a vacuum chamber for evacuation. The chamber temperature was heated to 350 °C and the vacuum degree was less than 1×10 -3 Pa, ion etching of the substrate surface was started, Ar was introduced with a flow rate of 350 sccm, a pulse bias voltage of -850 V, a frequency of 40 kHz, and a pulse width of 4 μs was applied to the steel block sample, and the steel block sample was pre-sputtered and cleaned with Ar plasma for 30 min; (3) Deposition of Ti transition layer High-power pulsed magnetron sputtering technology was used, the Ar flow rate was adjusted to 60 sccm, the substrate bias was continuously adjusted to -300 V, the frequency was 80 kHz, and the pulse width was 6 μs. A high-power pulse power supply was added to the pure Ti target, the peak current was adjusted to 150 A, the frequency was 100 Hz, and the pulse width was 450 μs. The Ti transition layer was deposited for 15 min. (4) Deposition of TiN coating High-power pulsed magnetron sputtering technology was used to deposit TiN coating by keeping the Ti target current unchanged, the frequency 100 Hz, the pulse width 500 μs, the Ar flow rate unchanged, introducing N2 with a flow rate of 20 sccm, applying a pulse bias voltage of -120 V, the frequency 40 kHz, the pulse width 12 μs, and the deposition time 10800 s on the steel block sample.

[0017] The thickness of the TiN coating prepared in Example 2 is about 300 nm. The coating has a bonding force of 68 N, a hardness of about 27 GPa, and an elastic modulus of about 261 GPa. Example

[0018] A TiN coating with high film-base bonding strength and a preparation method thereof, wherein the coating is prepared by high-power pulsed magnetron sputtering technology, and the specific steps are as follows: (1) Preprocessing The 9Cr18 alloy steel block substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then placed in a drying chamber for standby use after being blown dry. (2) Pre-sputtering cleaning The 9Cr18 alloy steel block sample treated in step (1) was placed in a vacuum chamber for evacuation. The chamber temperature was heated to 350 °C and the vacuum degree was less than 1×10 -3 Pa, ion etching of the substrate surface was started, Ar was introduced with a flow rate of 350 sccm, a pulse bias voltage of -850 V, a frequency of 40 kHz, and a pulse width of 4 μs was applied to the steel block sample, and the steel block sample was pre-sputtered and cleaned with Ar plasma for 30 min; (3) Deposition of Ti transition layer High-power pulsed magnetron sputtering technology was used, the Ar flow rate was adjusted to 60 sccm, the substrate bias was continuously adjusted to -250 V, the frequency was 80 kHz, and the pulse width was 6 μs. A high-power pulse power supply was added to the pure Ti target, the peak current was adjusted to 300 A, the frequency was 100 Hz, and the pulse width was 450 μs. The Ti transition layer was deposited for 15 min. (4) Deposition of TiN coating High-power pulsed magnetron sputtering technology was used, the Ti target current was kept constant, the frequency was 100 Hz, the pulse width was 500 μs, the Ar flow rate was constant, 15 sccm of N2 was introduced, a pulse bias was applied to the steel block sample, the bias was -120 V, the frequency was 40 kHz, the pulse width was 12 μs, the deposition time was 10800 s, and the TiN coating was deposited.

[0019] The thickness of the TiN coating prepared in Example 3 is about 400 nm. The coating has a bonding force of 55 N, a hardness of about 23 GPa, and an elastic modulus of about 239 GPa.

[0020] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A TiN coating with high film-base bonding strength, characterized in that: The TiN coating includes 40-50 at.% of N and 50-60 at.% of Ti according to the atomic mass ratio, and has a thickness of 300-500 nm. The Ti transition layer is first deposited and then the TiN coating is deposited by high-power pulsed magnetron sputtering.

2. The TiN coating with high film-substrate bonding strength according to claim 1, characterized in that: The TiN coating is prepared by the following steps: (1) Substrate pretreatment The substrate is cleaned and dried for later use; (2) Pre-sputtering cleaning The substrate obtained in step (1) is in a vacuum degree of less than 1×10 -3 Pa, temperature 350℃, argon gas flow rate 350sccm, bias voltage -850 V, frequency 40 kHz, pulse width 4 μs, pre-sputter cleaning 20-30min; (3) Deposition of Ti transition layer The argon flow rate was adjusted to 60 sccm, the substrate bias voltage was continuously adjusted to -200~-300 V, the frequency was 80 kHz, the pulse width was 6 μs, a high-power pulse power supply was added to the pure Ti target, the peak current was adjusted to 150~300 A, the frequency was 100 Hz, the pulse width was 450 μs, and the deposition time was 15 min; (4) Deposition of TiN coating The Ti target peak current was maintained at 150~300 A, the frequency was 100 Hz, the pulse width was 500 μs, the argon flow rate was maintained at 60 sccm, nitrogen was introduced, the nitrogen flow rate was 10~20 sccm, the bias voltage was -120 V, the frequency was 40 kHz, the pulse width was 12 μs, and the deposition time was 10800 s.

3. The TiN coating with high film-substrate bonding strength according to claim 2, characterized in that: The peak current in step (3) is 180 A.

4. The TiN coating with high film-substrate bonding strength according to claim 2, characterized in that: The nitrogen flow rate in step (4) is 10 sccm.

5. The TiN coating with high film-substrate bonding strength according to claim 2, characterized in that: The pre-sputtering cleaning time in step (2) is 20 minutes.

Citation Information

Patent Citations

  • Method for depositing film through high ionization rate high power pulse magnetron sputtering

    CN105154838A

  • TiCN coating based on high-power pulse magnetron sputtering technology and preparation method thereof

    CN116356255A

  • Multi-element refractory high-entropy alloy nitride film and preparation method thereof